Liquid metal battery with multiple reaction mechanisms and preparation method thereof
By adopting a combination of positive electrode materials with multiple reaction mechanisms in liquid metal batteries, including high electronegative Te and low electronegative Sb, combined with inactive component M, the low operating voltage of liquid metal batteries and poor stability of Te-based batteries are solved. Problem, achieving higher discharge voltage and stability.
Patent Information
- Application Number
- CN202410966269.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The working voltage of liquid metal batteries is low, resulting in low energy density, and the positive electrode material of Te-based liquid metal batteries has problems such as poor circulation performance and low Coulomb efficiency.
The liquid metal battery with multiple reaction mechanism is adopted, including negative electrode material, positive electrode material and electrolyte. The positive electrode material is composed of high electronegative Te, low electronegative Sb and inactive component M. TexSbyMz is obtained through alloying reaction. x, y, and z represent the mole percentage of components. The electrolyte is a halogen molten salt containing ions of the negative electrode material. The alloying reaction is carried out under an inert atmosphere. The reaction temperature is 650°C to 700°C and the reaction time is 5 to 20 minutes.
The discharge voltage and stability of liquid metal batteries are improved, and the addition of Sb inhibits the dissolution of Te in the electrolyte, realizes a multiple reaction mechanism, and improves the circulation performance and Coulomb efficiency of liquid metal batteries.
Smart Images

Figure CN118919880A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of energy storage liquid metal batteries, and more specifically, to a liquid metal battery with multiple reaction mechanisms and a preparation method thereof. Background Art
[0002] With the continuous growth of global energy demand and the transition to sustainable energy, traditional energy (such as fossil, natural gas, coal, etc.) is difficult to meet the demand, and the use of renewable energy (wind energy, solar energy, etc.) in countries around the world is increasing year by year. However, the intermittent and volatile nature of wind and solar energy makes them unstable in the grid connection of renewable energy. Energy storage technology can effectively eliminate this instability and is a new power system with new energy as the main body.
[0003] Liquid metal battery is a new type of energy storage liquid metal battery system developed in recent years. It uses widely available and low-cost liquid metal or alloy as electrode and inorganic molten salt as electrolyte. This three-layer all-liquid structure breaks through the insertion and extraction mechanism of traditional liquid metal batteries, avoids the structural change of solid electrodes, and thus has an ultra-long cycle life. The long life, high safety and low cost of liquid metal batteries make them have broad application prospects in the field of large-scale energy storage.
[0004] In recent years, researchers at home and abroad have conducted extensive research on liquid metal batteries and proposed a series of liquid metal battery systems such as Sb-based, Bi-based, and Sn-based. However, liquid metal batteries based on metal alloying reactions, such as the liquid metal battery systems Li||Sb-Pb, Li||Sb-Sn, Li||Bi, and Li||Sb reported in recent years, generally have an operating voltage lower than 1.0V. The low operating voltage poses a challenge to the management system of liquid metal battery packs and leads to low energy density of liquid metal batteries. Among all candidate positive electrode metal materials for liquid metal batteries, Te, as a metalloid element, has a strong electronegativity, and the open circuit voltage of the Li||Te system can reach 1.76V. However, the conductivity of the Te electrode is low, and the solubility of Te and its lithium products in molten salt is high, resulting in poor cycle performance and low coulombic efficiency of Te-based liquid metal battery positive electrode materials, which need to be further solved. Summary of the invention
[0005] In view of the above problems, the present invention proposes a liquid metal battery with multiple reaction mechanisms and a preparation method thereof, aiming to improve the operating voltage of the liquid metal battery and the stability of the Te-based liquid metal battery.
[0006] To achieve the above-mentioned object, the first aspect of the present application provides a liquid metal battery with multiple reaction mechanisms, including a negative electrode material, a positive electrode material and an electrolyte; the negative electrode material includes an alkali metal or an alkaline earth metal A; the positive electrode material is composed of a high electronegative metal or metalloid Te, a low electronegative metal or metalloid Sb and an inactive component M; the chemical formula of the positive electrode material is Te x Sb y M z , x, y, z represent the molar percentages of the corresponding components, wherein 32≤x≤42, 58≤y≤68, 0≤z<=5; the sum of the molar percentages of the components in each positive electrode alloy is equal to 100%.
[0007] Furthermore, A is one or more of Li, Na, Mg and Al.
[0008] Furthermore, the inactive component M is one or more of Pb, Zn and Ga.
[0009] Furthermore, the electrolyte is a halogen molten salt containing at least one metal ion corresponding to the negative electrode material.
[0010] The second aspect of the present application provides a method for preparing a liquid metal battery with multiple reaction mechanisms, comprising the following steps: selecting an alkali metal or alkaline earth metal A as a negative electrode material; according to the composition of the positive electrode material, alloying a highly electronegative active component Te, a low electronegative active component Sb, and an inactive component M to obtain a positive electrode material; and assembling the negative electrode material, the positive electrode material, and the electrolyte into a liquid metal battery.
[0011] Furthermore, the alloying reaction is carried out in an inert atmosphere, the reaction temperature is 650°C to 700°C, and the reaction time is 5 to 20 minutes. To prevent the positive electrode material component Te from volatilizing due to excessive heating time, the heating is stopped after alloying, and the desired positive electrode material is obtained after the temperature is lowered and the material is taken out.
[0012] Compared with the prior art, this application has the following technical effects:
[0013] 1. In the initial stage of discharge of a liquid metal battery with multiple reaction mechanisms of the present application, the negative electrode material A reacts simultaneously with the Te and Sb components in the positive electrode material to produce the intermediate product ATeSb. This process has nothing to do with the electronegativity of the positive electrode metal material. In the subsequent discharge process, according to the level of the reaction potential, ATeSb further reacts to produce discharge products ATe and ASb. Among them, ATeSb, ATe and ASb here only represent the elemental composition of the intermediate products and do not involve specific chemical compositions. The synchronous reaction mechanism of the dual-active positive electrode material components of the present application increases the discharge voltage of the liquid metal battery. At the same time, the addition of Sb also inhibits the dissolution of Te in the electrolyte, thereby improving the stability of the liquid metal battery.
[0014] 2. Liquid metal battery Te in this application x Sb y M z The positive electrode can significantly reduce the solubility of Te in the molten salt electrolyte, and improve the discharge voltage and stability of the liquid metal battery. At the same time, the liquid metal battery exhibits multiple reaction mechanisms during the discharge process, which is different from the reaction mechanism in which the negative electrode first reacts with the active component with high electronegativity and then reacts with the active component with low electronegativity during the discharge process. In the early stage of discharge, Te and Sb participate in the reaction at the same time, and then as the discharge continues, Te and Sb react separately. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0016] Figure 1 The liquid metal battery provided in Example 1 of the present application is 50 mA / cm 2 Discharge curve under (550℃);
[0017] Figure 2 X-ray diffraction diagram of the positive electrode of the liquid metal battery provided in Example 1 of the present application under different discharge states;
[0018] Figure 3 The cycle performance (550°C) of the liquid metal battery provided in Application Example 1. DETAILED DESCRIPTION
[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0020] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple, respectively.
[0021] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0022] The weight of the relevant components mentioned in the specification of the examples of this application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the specification of the examples of this application, it is within the scope disclosed in the specification of the examples of this application. Specifically, the mass described in the specification of the examples of this application can be a mass unit known in the biochemical field such as μg, mg, g, kg, etc.
[0023] Embodiment 1, a method for preparing a liquid metal battery with multiple reaction mechanisms, comprising the following steps:
[0024] (1) Li is selected as the negative electrode material;
[0025] (2) The positive electrode material is Te4Sb6. According to the molar ratio of the positive electrode material, the corresponding mass of Te and Sb is weighed on a balance and placed in a heating furnace. The furnace is heated to 650°C in an inert atmosphere (Ar gas) to prevent the positive electrode component Te from volatilizing due to excessive heating time. Therefore, the temperature is kept for 5 to 10 minutes to allow alloying, and then the heating is stopped. After cooling, the desired positive electrode material is obtained by taking it out.
[0026] (3) The electrolyte material is a molten salt composed of LiF, LiCl, and LiBr, and the molar ratio of LiF, LiCl, and LiBr is 22:31:47. The preparation process of the electrolyte is: according to the molar ratio of the electrolyte components, the corresponding masses are weighed and mixed, and after mixing, water is removed at 200°C under vacuum conditions, and then melted and cooled in an inert atmosphere to obtain a usable electrolyte;
[0027] (4) Assembling the negative electrode material, the positive electrode material, and the electrolyte into a liquid metal battery: placing the positive electrode material, the electrolyte, and the negative electrode current collector in the liquid metal battery shell from bottom to top, and the negative electrode material is wrapped in the negative electrode current collector. The test conditions are: 50 mA cm -2 Discharge current density to 0.6 V, 100 mA cm -2 The current density was charged to 2V.
[0028] Figure 1 The liquid metal battery of Example 1 of the present application is at 50 mA / cm 2 The discharge curve below, the operating temperature of the liquid metal battery is 550℃; Figure 2 is the XRD diagram of the positive electrode of the liquid metal battery in Example 1 of the present application under different discharge states;
[0029] Figure 3 This is a cycle performance diagram of the liquid metal battery of Example 1 of the present application at different current densities, and the operating temperature of the liquid metal battery is 550°C.
[0030] Depend on Figure 1 Li||LiF-LiCl-LiBr||Te4Sb6 at 50mA / cm 2 From the discharge curve below, we can see that the entire curve is roughly divided into two voltage platforms: the high voltage range of 1.6V to 1.4V corresponds to the reaction process of Te, and the low voltage range of 1.2V to 0.6V corresponds to the reaction process of Sb. The average discharge voltage of the liquid metal battery is 1.02V. Figure 2 From the phase composition of the positive electrode under different discharge states, it can be seen that the liquid metal battery produces LiSbTe2 in the initial stage of discharge, and then gradually reacts to produce Li2Te and Li3Sb. Figure 3 For the cycle performance of case 1 at different current densities, it can be seen that the liquid metal battery has a high current density at 200 mA / cm 2 It can maintain good cycle stability at low density.
[0031] The steps of Examples 2-15 are the same as those of Example 1, and the only difference is the process parameters, see Table 1 for details.
[0032] Table 1
[0033] Anode Materials Cathode Materials Reaction temperature Reaction time Example 1 Li <![CDATA[Te 40 Sb 60 ]]> 650℃ 10min Example 2 Li <![CDATA[Te 42 Sb 58 ]]> 650℃ 10min Example 3 Li <![CDATA[Te 32 Sb 68 ]]> 680℃ 20min Example 4 Li <![CDATA[Te 38.8 Sb 58.2 Zn3]]> 700℃ 5min Example 5 Li <![CDATA[Te 33 Sb 62 Zn5]]> 700℃ 10min Example 6 Na <![CDATA[Te 32 Sb 68 ]]> 680℃ 20min Example 7 Na <![CDATA[Te 42 Sb 58 ]]> 650℃ 10min Example 8 Mg <![CDATA[Te 32 Sb 68 ]]> 680℃ 5min Example 9 Mg <![CDATA[Te 42 Sb 58 ]]> 650℃ 10min Example 10 Al <![CDATA[Te 32 Sb 68 ]]> 680℃ 20min Embodiment 11 Al <![CDATA[Te 42 Sb 58 ]]> 650℃ 10min Example 12 <![CDATA[Li 25 Al 75 ]]> <![CDATA[Te 40 Sb 60 ]]> 650℃ 10min Example 13 <h2 style=";text-align:left;direction:ltr"><![CDATA[Li <h2 style=";text-align:left;direction:ltr"> 98 <h2 style=";text-align:left;direction:ltr"> Na2]]><h2 style=";text-align:left;direction:ltr"> <![CDATA[Te 40 Sb 60 ]]> 650℃ 5min Embodiment 14 <![CDATA[Na 99.5 Mg 0.5 ]]> <![CDATA[Te 40 Sb 60 ]]> 650℃ 10min Embodiment 15 <![CDATA[Mg 70 Al 30 ]]> <![CDATA[Te 40 Sb 60 ]]> 650℃ 15min
[0034] Table 2 shows the performance parameters of the liquid metal batteries with multiple reaction mechanisms prepared in Examples 1 to 15.
[0035]
[0036]
[0037] It should be noted that the electrolyte molten salt in the embodiment of the present application may also adopt other electrolyte salts known in the prior art, and the operating temperature of the liquid metal battery may be determined according to the melting point of the electrolyte salt used.
[0038] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A liquid metal battery with multiple reaction mechanisms, It is characterized in that Including negative electrode materials, positive electrode materials and electrolytes; The negative electrode material includes an alkali metal or an alkaline earth metal A; The positive electrode material is composed of a high electronegative metal or metalloid Te, a low electronegative metal or metalloid Sb and an inactive component M; the chemical formula of the positive electrode material is Te x Sb y M z , x, y, and z represent the molar percentages of the corresponding components, wherein 32≤x≤42, 58≤y≤68, and 0≤z<=5.
2. A liquid metal battery with multiple reaction mechanisms as claimed in claim 1, It is characterized in that A is one or more of Li, Na, Mg and Al.
3. A liquid metal battery with multiple reaction mechanisms as claimed in claim 1, It is characterized in that The inactive component M is one or more of Pb, Zn and Ga.
4. A liquid metal battery with multiple reaction mechanisms as claimed in claim 1, It is characterized in that The electrolyte is a halogen molten salt containing at least one metal ion corresponding to the negative electrode material.
5. A method for preparing a liquid metal battery with multiple reaction mechanisms as claimed in any one of claims 1 to 4, It is characterized in that The following steps are involved: An alkali metal or alkaline earth metal A is selected as the negative electrode material; according to the composition of the positive electrode material, an active component Te with high electronegativity, an active component Sb with low electronegativity and an inactive component M are subjected to an alloying reaction to obtain the positive electrode material; The negative electrode material, the positive electrode material and the electrolyte are assembled into a liquid metal battery.
6. A method for preparing a liquid metal battery with multiple reaction mechanisms as claimed in claim 5, It is characterized in that The alloying reaction is carried out in an inert atmosphere, the reaction temperature is 650° C. to 700° C., and the reaction time is 5 to 20 minutes.
Citation Information
Patent Citations
Sb2Tey-Si3N4 composite phase change material for phase change memory and preparation method thereof
CN102569644A
High-energy-density liquid metal battery
CN107221677A
Positive electrode material for liquid and semi-liquid metal batteries
CN107482209A
Positive electrode material of liquid-state or semi-liquid-state metal battery and application
CN113809317A
Gel electrolyte, precursor thereof and lithium ion battery