Adhesive film for metal terminal, method for producing same, metal terminal equipped with film, electric storage device, and
By using the adhesive film for metal terminals of the first polyolefin layer and the second polyolefin layer stack, the problems of poor sealing and collapse in a short time in the prior art are solved, and high sealing properties are achieved And excellent following, it improves the overall performance of electrical storage devices.
Patent Information
- Application Number
- CN202410978772.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-04
- Filing Date
- 2021-03-04
- Publication Date
- 2024-11-08
AI Technical Summary
The adhesive film between the existing metal terminal and the hot-welded resin layer is difficult to achieve high sealing in a short time, and the adhesive film collapses due to multiple heat seals, which affects the sealing and productivity of the power storage device. .
The adhesive film for metal terminals consisting of the first polyolefin layer and the second polyolefin layer stack is used to ensure that the melting heat of the first polyolefin layer is greater than the second polyolefin layer, and the melting heat of the base material is set to 70 J. /g or above to achieve high sealing and excellent following in a short time.
It achieves high sealing properties with the hot-welded resin layer in a short time, suppresses the collapse of the adhesive film, improves the following to the outer packaging material, and improves the sealing properties and productivity of the electric storage device.
Smart Images

Figure BDA0004955386980000231 
Figure BDA0004955386980000381 
Figure BDA0004955386980000382
Abstract
Description
[0001] This case is filed on March 4, 2021 、Application No. 202180018969.X(PCT / JP2021 / 008551) , a divisional application of a patent application entitled "Adhesive film for metal terminals, method for manufacturing the same, metal terminals with the film, power storage devices and method for manufacturing the same". Technical Field
[0002] The present invention relates to an adhesive film for metal terminals, a method for producing the adhesive film for metal terminals, a metal terminal with the adhesive film for metal terminals, an electric storage device using the adhesive film for metal terminals, and a method for producing the electric storage device. Background Art
[0003] Various types of energy storage devices have been developed in the past. In all energy storage devices, outer packaging materials for energy storage devices are indispensable components for encapsulating energy storage device components such as electrodes and electrolytes. In the past, as outer packaging materials for energy storage devices, metal outer packaging materials for energy storage devices were mostly used. However, in recent years, with the high performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc., energy storage devices not only require a variety of shapes, but also need to be thinner and lighter. However, the existing commonly used metal outer packaging materials for energy storage devices have the disadvantages of being difficult to keep up with the demand for diversified shapes and also having limitations in terms of lightweighting.
[0004] Therefore, in recent years, as an outer packaging material for storage devices that is easy to process into various shapes and can achieve thinning and lightening, a laminated sheet having a base layer / adhesive layer / barrier layer / thermo-fusible resin layer laminated in sequence has been proposed. When such a film-shaped outer packaging material for storage devices is used, the peripheral edge of the outer packaging material for storage devices is heat-fused in a state where the innermost heat-fusible resin layers of the outer packaging material for storage devices are opposite to each other, thereby encapsulating the storage device element using the outer packaging material for storage devices.
[0005] The metal terminal protrudes from the heat-sealed portion of the outer packaging material for the storage device, and the storage device element encapsulated by the outer packaging material for the storage device is electrically connected to the outside through the metal terminal electrically connected to the electrode of the storage device element. That is, in the heat-sealed portion of the outer packaging material for the storage device, the metal terminal is heat-sealed in a state of being sandwiched between the heat-fusible resin layer. Since the metal terminal and the heat-fusible resin layer are made of different materials, the adhesion is easily reduced at the interface between the metal terminal and the heat-fusible resin layer.
[0006] Therefore, there is a proposal to arrange an adhesive film between the metal terminal and the heat-fusible resin layer for the purpose of improving the above-mentioned adhesion, etc. As such an adhesive film, for example, the adhesive film described in Patent Document 1 can be cited.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2015-79638 Summary of the invention
[0010] Problems to be solved by the invention
[0011] As described above, the adhesive film disposed between the heat-fusible resin layer of the outer packaging material for a power storage device and the metal terminal is required to have adhesion with the heat-fusible resin layer and the metal terminal that can be achieved by heat sealing.
[0012] In the process of bonding the metal terminal to the outer packaging material for the storage device via the adhesive film, the metal terminal and the adhesive film are usually heat-sealed to prepare the metal terminal with the adhesive film in advance. Next, in the peripheral edge portion of the outer packaging material for the storage device, in a state where the heat-fusible resin layers are facing each other, the metal terminal with the adhesive film is arranged between the heat-fusible resin layers facing each other, and the peripheral edge portion is heat-sealed, thereby heat-fusing the heat-fusible resin layers to each other and heat-fusing the heat-fusible resin layers to the adhesive film, and the storage device element is encapsulated by the outer packaging material for the storage device.
[0013] Thus, the adhesive film needs to be heat-sealed at least twice: when it is bonded to the metal terminal and when it is bonded to the heat-fusible resin layer of the outer packaging material for the power storage device.
[0014] Furthermore, when the adhesive film is bonded to the metal terminal, a temporary bonding process of the adhesive film and the metal terminal and a main bonding process are usually performed multiple times of heating and pressurization. The temporary bonding process is a process of temporarily fixing the adhesive film to the metal terminal and removing bubbles, and the main bonding process is a process of bonding the adhesive film to the metal terminal by heating and pressurizing once or multiple times at a higher temperature than the temporary bonding process.
[0015] Therefore, the adhesive film has to be heated and pressurized multiple times for heat sealing until the outer packaging material for the storage device is packaged. Thus, there is a problem that the adhesive film collapses and the thickness decreases due to the multiple heat sealings at high temperature and high pressure until the outer packaging material for the storage device is packaged. When the thickness of the adhesive film decreases, the sealing property of the outer packaging material for the storage device is also easily reduced.
[0016] In addition, in order to improve the productivity of the power storage device, it is necessary to further shorten the heat sealing time (i.e., heating and pressing time) of the outer packaging material for the power storage device. When the heat sealing time of the peripheral edge of the outer packaging material for the power storage device is reduced from, for example, 3 seconds to 1 second, the heat sealing time is 1 / 3 (of the original time), thereby improving productivity. However, when heat sealing is performed in a short time, it is difficult to achieve a high degree of adhesion between the heat-fusible resin layer of the outer packaging material for the power storage device and the adhesive film.
[0017] Moreover, when the heat-fusible resin layer of the outer packaging material for the storage device is heat-sealed with the adhesive film in a short period of time, the adhesive film will not be able to follow the outer packaging material for the storage device sufficiently during heat sealing, and a gap will exist between the adhesive film and the heat-fusible resin layer, thereby causing a problem in which the sealing performance of the storage device is easily reduced.
[0018] Under such circumstances, the main object of the present invention is to provide an adhesive film for metal terminals, which can achieve high sealing performance with a heat-fusible resin layer of an outer packaging material for a storage device in a short time, suppresses collapse caused by heat sealing, and has excellent followability to the outer packaging material for the storage device during heat sealing. In addition, the present invention also aims to provide a method for manufacturing the adhesive film for metal terminals, a metal terminal with the adhesive film for metal terminals using the adhesive film for metal terminals, a storage device using the adhesive film for metal terminals, and a method for manufacturing the storage device.
[0019] Technical solutions to solve problems
[0020] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems. As a result, it was found that in an adhesive film for metal terminals composed of a laminate having a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer packaging material side of a storage device, by making the melting heat ΔH1 of the first polyolefin layer and the melting heat ΔH2 of the second polyolefin layer satisfy the relationship of ΔH1>ΔH2, and setting the melting heat ΔH3 of the substrate to 70 J / g or more, it is possible to obtain an adhesive film for metal terminals that achieves high sealing performance with the heat-fusible resin layer of the outer packaging material for the storage device in a short time, suppresses collapse caused by heat sealing, and has excellent followability to the outer packaging material for the storage device during heat sealing. The present invention is an invention completed by further repeated research based on these cognitions.
[0021] That is, the present disclosure provides inventions in the following aspects.
[0022] An adhesive film for metal terminals, which is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device encapsulating the electric storage device element, wherein the adhesive film for metal terminals is composed of a laminate having a first polyolefin layer arranged on the metal terminal side, a substrate, and a second polyolefin layer arranged on the outer packaging material side of the electric storage device in this order,
[0023] The heat of fusion ΔH1 of the first polyolefin layer and the heat of fusion ΔH2 of the second polyolefin layer measured in accordance with the provisions of JIS K 7122:2012 satisfy the relationship ΔH1>ΔH2.
[0024] The heat of fusion ΔH3 of the substrate measured in accordance with the provisions of JIS K 7122:2012 is 70 J / g or more.
[0025] Effects of the Invention
[0026] According to the present invention, it is possible to provide an adhesive film for metal terminals that can achieve high sealing performance with a heat-fusible resin layer of an outer packaging material for a storage device in a short time, suppress collapse due to heat sealing, and have excellent followability to the outer packaging material for a storage device. In addition, the present invention also aims to provide a method for manufacturing the adhesive film for metal terminals, a metal terminal with an adhesive film for metal terminals using the adhesive film for metal terminals, a storage device using the adhesive film for metal terminals, and a method for manufacturing the storage device. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic top view of the power storage device of the present invention.
[0028] Figure 2 is along Figure 1 Schematic diagram of the cross section along line A-A'.
[0029] Figure 3 is along Figure 1 Schematic diagram of the cross section along line B-B'.
[0030] Figure 4 It is a schematic cross-sectional view of the adhesive film for metal terminals of the present invention.
[0031] Figure 5 It is a schematic cross-sectional view of the adhesive film for metal terminals of the present invention.
[0032] Figure 6 It is a schematic cross-sectional view of the outer packaging material for an electric storage device of the present invention.
[0033] Figure 7 This is a schematic cross-sectional view for explaining a portion where heat-sealed heat-fusible resin layers are formed via a metal terminal with an adhesive film in an example.
[0034] Figure 8 This is a schematic diagram for explaining the sample preparation method for performing adhesion evaluation, followability evaluation, and collapse evaluation in Examples.
[0035] Fig. 9 This is a schematic diagram for explaining the sample preparation method for performing adhesion evaluation, followability evaluation, and collapse evaluation in Examples.
[0036] Fig.10 This is a schematic diagram for explaining the method of preparing samples for evaluating followability in Examples.
[0037] Fig.11 This is the DSC curve obtained in Example 1.
[0038] Explanation of symbols
[0039] 1 Adhesive film for metal terminals
[0040] 2 Metal terminals
[0041] 3 Outer packaging materials for power storage devices
[0042] 3a The peripheral edge of the outer packaging material for power storage devices
[0043] 4. Energy storage device components
[0044] 10 Power storage devices
[0045] 11. Substrate
[0046] 12a 1st polyolefin layer
[0047] 12b Second polyolefin layer
[0048] 13 Adhesion promoter layer
[0049] 31 substrate layer
[0050] 32 Adhesive layer
[0051] 33 Barrier layer
[0052] 34 Adhesive layer
[0053] 35 Thermally fusible resin layer DETAILED DESCRIPTION
[0054] The adhesive film for metal terminals of the present invention is characterized in that it is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element, and the adhesive film for metal terminals is composed of a laminate having a first polyolefin layer arranged on the metal terminal side, a substrate, and a second polyolefin layer arranged on the outer packaging material side of the electric storage device in this order,
[0055] The heat of fusion ΔH1 of the first polyolefin layer and the heat of fusion ΔH2 of the second polyolefin layer measured in accordance with JIS K 7122:2012 satisfy the relationship ΔH1>ΔH2, and the heat of fusion ΔH3 of the substrate measured in accordance with JIS K 7122:2012 is 70 J / g or more.
[0056] Since the adhesive film for metal terminals of the present invention has such characteristics, it can achieve high sealing performance with the heat-fusible resin layer of the outer packaging material in a short time, can suppress collapse caused by heat sealing, and has excellent followability to the outer packaging material for power storage devices.
[0057] In addition, the storage device of the present invention is characterized in that it comprises: a storage device element having at least a positive electrode, a negative electrode and an electrolyte, an outer packaging material for the storage device that encapsulates the storage device element, and metal terminals that are electrically connected to the above-mentioned positive electrode and the above-mentioned negative electrode and protrude to the outside of the outer packaging material for the storage device, and an adhesive film for the metal terminals of the present invention is provided between the metal terminals and the outer packaging material for the storage device.
[0058] The adhesive film for metal terminals and a method for producing the same, and a power storage device using the adhesive film for metal terminals and a method for producing the same of the present invention are described in detail below.
[0059] In addition, in this specification, regarding the numerical range, the numerical range represented by "to" means "above ... and below ...". For example, the notation of 2 to 15 mm means above 2 mm and below 15 mm.
[0060] In addition, as a method for confirming the MD (Machine Direction) of the adhesive film for metal terminals, there is a method for confirming the sea island structure by observing the cross section of the adhesive film for metal terminals (e.g., the cross section of the first polyolefin layer, the substrate, or the second polyolefin layer) with an electron microscope. In this method, the parallel direction of the cross section with the largest average island diameter of the island shape in the direction perpendicular to the thickness direction of the adhesive film for metal terminals can be determined as MD. Specifically, the cross section in the length direction of the adhesive film for metal terminals and each cross section (a total of 10 cross sections) in which the angle is changed by 10 degrees each time from the direction parallel to the cross section in the length direction until the direction perpendicular to the cross section in the length direction are observed in the form of electron microscope photos to confirm the sea island structure. Next, the shape of each island in each cross section is observed separately. The straight-line distance between the leftmost end of the vertical direction perpendicular to the thickness direction of the adhesive film for metal terminals and the rightmost end of the vertical direction in each island shape is set as the island diameter y. In each cross section, the average value of the island diameter y of the top 20 island diameters y of the island shape is calculated in descending order. The direction parallel to the cross section of the island shape where the average value of the island diameter y is the largest is determined as MD.
[0061] 1. Adhesive film for metal terminals
[0062] The adhesive film for metal terminals of the present invention is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element. Specifically, for example Figure 1 to Figure 3 As shown, the adhesive film 1 for metal terminals of the present invention is located between the metal terminal 2 electrically connected to the electrode of the storage device element 4 and the outer packaging material 3 for the storage device that encapsulates the storage device element 4. In addition, the metal terminal 2 protrudes to the outside of the outer packaging material 3 for the storage device, and is clamped by the outer packaging material 3 for the storage device at the peripheral edge portion 3a of the outer packaging material 3 for the storage device that is heat-sealed, with the help of the adhesive film 1 for metal terminals.
[0063] It should be noted that in the present invention, the temporary bonding process of bonding the metal terminal to the metal terminal with the adhesive film is carried out under the conditions of, for example, a temperature of about 140 to 160°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a number of times of about 3 to 6 times, and the main bonding process is carried out under the conditions of, for example, a temperature of about 160 to 240°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a number of times of about 1 to 3 times. In addition, when the metal terminal with the adhesive film is placed between the outer packaging materials for the storage device and heat-sealed, it is carried out under the conditions of a heating temperature of generally about 180 to 210°C, a pressure of generally about 1.0 to 2.0 MPa, a time of about 3 to 5 seconds, and a number of times of about 1 time. In order to achieve high sealing properties with the heat-fusible resin layer of the outer packaging material in a short time, when the metal terminal with the adhesive film is placed between the outer packaging materials for the power storage device and heat-sealed, the heat sealing time can be set to about 0.5 to 3 seconds, about 0.5 to 2 seconds, and further to about 0.5 to 1 second.
[0064] The adhesive film 1 for metal terminals of the present invention is provided to improve the adhesion between the metal terminal 2 and the outer packaging material 3 for the storage device. By improving the adhesion between the metal terminal 2 and the outer packaging material 3 for the storage device, the sealing of the storage device element 4 can be improved. As described above, when the storage device element 4 is heat-sealed, the storage device element is packaged in a state where the metal terminal 2 electrically connected to the electrode of the storage device element 4 protrudes to the outside of the outer packaging material 3 for the storage device. At this time, since the metal terminal 2 formed of metal and the heat-fusible resin layer 35 (a layer formed of a heat-fusible resin such as polyolefin) located in the innermost layer of the outer packaging material 3 for the storage device are formed of different materials, if such an adhesive film is not used, the sealing of the storage device element is likely to be reduced at the interface between the metal terminal 2 and the heat-fusible resin layer 35.
[0065] like Figure 4 and Figure 5 As shown, the adhesive film 1 for metal terminals of the present invention has a structure in which at least a first polyolefin layer 12a, a substrate 11 and a second polyolefin layer 12b are stacked in sequence. The first polyolefin layer 12a is arranged on the side of the metal terminal 2. And the second polyolefin layer 12b is arranged on the side of the outer packaging material 3 for the storage device. In the adhesive film 1 for metal terminals of the present invention, the first polyolefin layer 12a and the second polyolefin layer 12b are respectively located on the two side surfaces (of the adhesive film).
[0066] In the adhesive film 1 for metal terminals of the present invention, the first polyolefin layer 12a and the second polyolefin layer 12b are layers containing polyolefin resins. As polyolefin resins, polyolefins, acid-modified polyolefins, etc. can be cited. The first polyolefin layer 12a preferably contains an acid-modified polyolefin in the polyolefin resin, and more preferably is a layer formed by the acid-modified polyolefin. In addition, the second polyolefin layer 12b preferably contains a polyolefin or an acid-modified polyolefin in the polyolefin resin, more preferably contains a polyolefin, and further preferably is a layer formed by a polyolefin.
[0067] Furthermore, the substrate 11 preferably contains a polyolefin-based resin, preferably contains polyolefin, and more preferably is a layer formed of polyolefin.
[0068] The polyolefin resins in the first polyolefin layer 12a, the second polyolefin layer 12b and the substrate 11 are preferably polypropylene resins, the polyolefin is preferably polypropylene, and the acid-modified polyolefin is preferably acid-modified polypropylene. It should be noted that polyolefin resins such as polyolefin and acid-modified polyolefin may contain known additives and fillers and pigments described later.
[0069] Specific examples of preferred laminated structures of the adhesive film 1 for metal terminals of the present invention include a three-layer structure in which a first polyolefin layer formed of acid-modified polypropylene / a substrate formed of polypropylene / a second polyolefin layer formed of polypropylene are laminated in sequence; a three-layer structure in which a first polyolefin layer formed of acid-modified polypropylene / a substrate formed of polypropylene / a second polyolefin layer formed of acid-modified polypropylene are laminated in sequence, etc. Among them, a three-layer structure in which a first polyolefin layer formed of acid-modified polypropylene / a substrate formed of polypropylene / a second polyolefin layer formed of polypropylene are laminated in sequence is particularly preferred.
[0070] The details of the materials constituting the first polyolefin layer 12 a , the second polyolefin layer 12 b , and the substrate 11 will be described later.
[0071] When the adhesive film 1 for metal terminals of the present invention is arranged between the metal terminal 2 of the power storage device 10 and the outer packaging material 3 for the power storage device, the surface of the metal terminal 2 formed of metal and the heat-fusible resin layer 35 (a layer formed of a heat-fusible resin such as polyolefin) of the outer packaging material 3 for the power storage device are joined via the adhesive film 1 for metal terminals. The first polyolefin layer 12a of the adhesive film for metal terminals 1 is arranged on the metal terminal 2 side, and the second polyolefin layer 12b is arranged on the outer packaging material 3 side for the power storage device, the first polyolefin layer 12a is closely joined to the metal terminal 2, and the second polyolefin layer 12b is closely joined to the heat-fusible resin layer 35 of the outer packaging material 3 for the power storage device.
[0072] In the adhesive film 1 for metal terminals of the present invention, the heat of fusion ΔH1 of the first polyolefin layer 12a and the heat of fusion ΔH2 of the second polyolefin layer 12b measured in accordance with the provisions of JIS K 7122: 2012 satisfy the relationship of ΔH1>ΔH2. Moreover, the heat of fusion ΔH3 of the substrate 11 measured in accordance with the provisions of JIS K 7122: 2012 is 70 J / g or more. In the present invention, the method for measuring the heat of fusion is as follows.
[0073] <Measurement of Heat of Fusion>
[0074] The heat of fusion of each measurement sample is measured according to the provisions of JIS K 7122:2012. The measurement is performed using a differential scanning calorimeter (DSC, such as a differential scanning calorimeter Q200 manufactured by TA Instruments). After the measurement sample is kept at a temperature of -50°C for 15 minutes, the temperature is increased from -50°C to 210°C at a heating rate of 10°C / min, and the first heat of fusion ΔH (J / g) is measured, and then the temperature is maintained at 210°C for 10 minutes. Then, the temperature is decreased from 210°C to -50°C at a cooling rate of 10°C / min and maintained for 15 minutes. The temperature is then increased from -50°C to 210°C at a heating rate of 10°C / min, and the second heat of fusion ΔH (J / g) is measured. It should be noted that the nitrogen flow rate is set to 50 ml / min. According to the above steps, the value of the heat of fusion ΔH (J / g) measured for the first time is adopted. The heat of fusion is the area enclosed by the baseline (the line formed by connecting the starting point and the end point of the ridge line from the base to the base) and the peak in the DSC curve. It should be noted that, for the measurement sample, the first polyolefin layer and the second polyolefin layer obtained from the adhesive film for metal terminals can be used as the measurement sample. In addition, for the heat of fusion of the substrate, the heat of fusion of the first polyolefin layer, the second polyolefin layer and the adhesive film for metal terminals can be measured, and the heat of fusion of the first polyolefin layer and the second polyolefin layer can be removed from the measured heat of fusion of the adhesive film for metal terminals to be used as the heat of fusion of the substrate.
[0075] The heat of fusion of the substrate, the first polyolefin layer, the second polyolefin layer and the adhesive film for metal terminals can be adjusted according to the composition of each resin (for example, the addition ratio of polyethylene components, etc.), molecular skeleton, dispersibility, molecular weight, melting point, MFR, and the T-die, expansion and other conditions in the manufacture of the adhesive film for metal terminals (for example, the extrusion width from the T-die, stretching ratio, stretching speed, heat treatment temperature, and line speed during extrusion, cooling rate, extrusion temperature, etc.).
[0076] From the viewpoint of obtaining the above-mentioned high sealing performance in a short time, suppressing collapse and further improving the tracking performance, in the adhesive film 1 for metal terminals of the present invention, the difference between the melting heat ΔH1 of the first polyolefin layer 12a and the melting heat ΔH2 of the second polyolefin layer 12b is preferably about 3.0 J / g or more, more preferably about 5.0 J / g or more, and further preferably about 10.0 J / g or more. In addition, based on the same viewpoint, the difference is preferably about 18.0 J / g or less, more preferably about 15.0 J / g or less, and further preferably about 12.0 J / g or less. Preferred ranges of the difference include about 3.0 to 18.0 J / g, about 3.0 to 15.0 J / g, about 3.0 to 12.0 J / g, about 5.0 to 18.0 J / g, about 5.0 to 15.0 J / g, about 5.0 to 12.0 J / g, about 10.0 to 18.0 J / g, about 10.0 to 15.0 J / g, and about 10.0 to 12.0 J / g. In particular, from the viewpoint of suppressing the collapse of the adhesive film 1 for metal terminals, the difference is preferably about 3.0 J / g or more.
[0077] Based on the same viewpoint, the difference between the heat of fusion ΔH3 of the substrate 11 and the heat of fusion ΔH1 of the first polyolefin layer 12a is preferably about 15.0 J / g or more, more preferably about 18.0 J / g or more, and further preferably about 21.0 J / g or more. In addition, based on the same viewpoint, the difference is preferably about 35.0 J / g or less, more preferably about 32.0 J / g or less, and further preferably about 29.0 J / g or less. Preferred ranges of the difference include about 15.0 to 35.0 J / g, about 15.0 to 32.0 J / g, about 15.0 to 29.0 J / g, about 18.0 to 35.0 J / g, about 18.0 to 32.0 J / g, about 18.0 to 29.0 J / g, about 21.0 to 35.0 J / g, about 21.0 to 32.0 J / g, and about 21.0 to 29.0 J / g. In particular, from the viewpoint of suppressing the collapse of the adhesive film 1 for metal terminals, the difference is preferably about 15.0 J / g or more.
[0078] Based on the same viewpoint, the heat of fusion ΔH1 of the first polyolefin layer 12a, the heat of fusion ΔH2 of the second polyolefin layer 12b, and the heat of fusion ΔH3 of the substrate 11 preferably satisfy the relationship of ΔH3≥ΔH1>ΔH2, and more preferably satisfy the relationship of ΔH3>ΔH1>ΔH2. By making the heat of fusion ΔH3 of the substrate 11 the largest among the heat of fusion ΔH1 of the first polyolefin layer 12a, the heat of fusion ΔH2 of the second polyolefin layer 12b, and the heat of fusion ΔH3 of the substrate 11, the collapse of the adhesive film 1 can be more effectively suppressed. In addition, by satisfying such a relationship, when the metal terminal with the adhesive film is placed between the outer packaging material 3 for the storage device and heat-sealed, the substrate 11 absorbs the excess heat transferred from the second polyolefin layer 12b side to the first polyolefin layer 12a, and the decrease in the adhesion between the first polyolefin layer 12a and the metal terminal 2 due to excessive heating can be suppressed.
[0079] Based on the same viewpoint, the absolute value of the difference between the heat of fusion ΔH4 of the heat-fusible resin layer 35 of the outer packaging material 3 for the storage device used as the adhesive film for metal terminal 1 and the heat of fusion ΔH2 of the second polyolefin layer 12b of the adhesive film for metal terminal 1 is preferably about 0.0 to 5.0 J / g, or about 0.0 to 3.0 J / g. The smaller the absolute value of the difference between the heat of fusion ΔH4 and the heat of fusion ΔH2 (that is, the closer the absolute value of the difference is to 0.0 J / g), the higher the adhesion between the second polyolefin layer 12b and the heat-fusible resin layer 35 is likely to be. In particular, from the viewpoint of the sealing property and the followability of the adhesive film for metal terminal 1 in a short period of time, the difference is preferably about 0.0 J / g or more.
[0080] From the viewpoint of obtaining the above-mentioned high sealing performance in a short time, suppressing collapse and further improving the tracking performance, in the adhesive film 1 for metal terminals of the present invention, the melting heat ΔH1 of the first polyolefin layer 12a arranged on the side of the metal terminal 2 is preferably about 30.0 J / g or more, and more preferably about 45.0 J / g or more. Based on the same viewpoint, the melting heat ΔH1 is preferably about 80.0 J / g or less, and more preferably about 60.0 J / g or less. As the preferred range of the melting heat ΔH1, about 30.0 to 80.0 J / g, about 30.0 to 60.0 J / g, about 45.0 to 80.0 J / g, and about 45.0 to 60.0 J / g can be cited. In addition, from the viewpoint of improving the film-forming properties of the first polyolefin layer 12a, the heat of fusion ΔH1 is preferably about 60.0 J / g or less, more preferably 58.5 J / g or less, and the preferred range is about 30.0 to 60.0 J / g, about 30.0 to 58.5 J / g, about 45.0 to 60.0 J / g, and about 45.0 to 58.5 J / g.
[0081] Based on the same viewpoint, the heat of fusion ΔH2 of the second polyolefin layer 12b disposed on the side of the outer packaging material 3 for the storage device is preferably about 20.0 J / g or more, and more preferably about 35.0 J / g or more. Based on the same viewpoint, the heat of fusion ΔH2 is preferably about 70.0 J / g or less, and more preferably about 55.0 J / g or less. Preferred ranges of the heat of fusion ΔH2 include about 20.0 to 70.0 J / g, about 20.0 to 55.0 J / g, about 35.0 to 70.0 J / g, and about 35.0 to 55.0 J / g. In particular, from the viewpoint of suppressing the sealing and collapse of the adhesive film 1 for metal terminals in a short period of time, the heat of fusion ΔH2 is preferably about 55.0 J / g or less.
[0082] Based on the same viewpoint, the heat of fusion ΔH3 of the substrate 11 is 70.0 J / g or more, preferably about 75.0 J / g or more, and more preferably about 80.0 J / g or more. Based on the same viewpoint, the heat of fusion ΔH3 is preferably about 100.0 J / g or less, and more preferably about 90.0 J / g or less. Preferred ranges of the heat of fusion ΔH1 include about 70.0 to 100.0 J / g, about 70.0 to 90.0 J / g, about 75.0 to 100.0 J / g, about 75.0 to 90.0 J / g, about 80.0 to 100.0 J / g, and about 80.0 to 90.0 J / g. In particular, from the viewpoint of suppressing the collapse of the adhesive film 1 for metal terminals, the heat of fusion ΔH3 is preferably about 70.0 J / g or more.
[0083] In addition, from the viewpoint of obtaining the above-mentioned high sealing performance in a short time, suppressing collapse and further improving the tracking performance, in the adhesive film 1 for metal terminals of the present invention, the melting peak temperature mp1 of the first polyolefin layer 12a and the melting peak temperature mp2 of the second polyolefin layer 12b preferably satisfy the relationship of mp1>mp2. In the present invention, the method for measuring the melting peak temperature is as follows.
[0084] <Measurement of Melting Peak Temperature>
[0085] According to the provisions of JIS K 7121:2012 (Method for measuring the glass transition temperature of plastics (JIS K7121:1987 Supplementary Standard 1)), the melting peak temperature of each measurement sample is measured. The measurement is performed using a differential scanning calorimeter (DSC, such as the differential scanning calorimeter Q200 manufactured by TA Instruments). After the measurement sample is kept at a temperature of -50°C for 15 minutes, the temperature is increased from -50°C to 210°C at a heating rate of 10°C / min, and the first melting peak temperature P (°C) is measured, and then the temperature is maintained at 210°C for 10 minutes. Then, the temperature is reduced from 210°C to -50°C at a cooling rate of 10°C / min and maintained for 15 minutes. Then, the temperature is increased from -50°C to 210°C at a heating rate of 10°C / min, and the second melting peak temperature Q (°C) is measured. It should be noted that the nitrogen flow rate is set to 50 ml / min. According to the above steps, the melting peak temperature P (°C) measured for the first time and the melting peak temperature Q (°C) measured for the second time are obtained. According to the above steps, the melting peak temperature P (°C) value measured for the first time is used.
[0086] Based on the same viewpoint, the melting peak temperature mp1 of the first polyolefin layer 12a disposed on the metal terminal 2 side is preferably 130°C or higher, and more preferably about 135°C or higher. Based on the same viewpoint, the melting peak temperature mp1 is preferably about 160°C or lower, and more preferably about 150°C or lower. Preferred ranges of the melting peak temperature mp1 include about 130 to 160°C, about 130 to 150°C, about 135 to 160°C, and about 135 to 150°C.
[0087] Based on the same viewpoint, the melting peak temperature mp2 of the second polyolefin layer 12b disposed on the side of the outer packaging material 3 for the storage device is preferably about 130°C or more, and more preferably about 135°C or more. Based on the same viewpoint, the melting peak temperature mp2 is preferably about 160°C or less, and more preferably about 150°C or less. Preferred ranges of the melting peak temperature mp2 include about 130 to 160°C, about 130 to 150°C, about 135 to 160°C, and about 135 to 150°C.
[0088] Based on the same viewpoint, the melting peak temperature mp3 of the substrate 11 is 140°C or higher, preferably about 150°C or higher, and more preferably about 160°C or higher. Based on the same viewpoint, the melting peak temperature mp3 is preferably about 180°C or lower, and more preferably about 170°C or lower. Preferred ranges of the melting peak temperature mp3 include about 140 to 180°C, about 140 to 170°C, about 150 to 180°C, about 150 to 170°C, about 160 to 180°C, and about 160 to 170°C.
[0089] From the same viewpoint, the absolute value of the difference between the melting peak temperature mp1 of the first polyolefin layer 12a and the melting peak temperature mp2 of the second polyolefin layer 12b is preferably about 0 to 10°C, more preferably about 0 to 5°C.
[0090] Based on the same viewpoint, it is preferred that the melting peak temperature mp3 of the substrate 11 is greater than the melting peak temperature mp1 of the first polyolefin layer 12a. As the difference between the melting peak temperature mp3 of the substrate 11 and the melting peak temperature mp1 of the first polyolefin layer 12a (melting peak temperature mp3-melting peak temperature mp1), it is preferably about 10°C or more, more preferably about 15°C or more, and further preferably about 20°C or more. In addition, based on the same viewpoint, as the difference, it is preferably about 30°C or less, more preferably about 27°C or less, and further preferably about 25°C or less. As the preferred range of the difference, it is about 10 to 30°C, about 10 to 27°C, about 10 to 25°C, about 15 to 30°C, about 15 to 27°C, about 15 to 25°C, about 20 to 30°C, about 20 to 27°C, and about 20 to 25°C.
[0091] Based on the same viewpoint, the melting peak temperature mp1 of the first polyolefin layer 12a, the melting peak temperature mp2 of the second polyolefin layer 12b, and the melting peak temperature mp3 of the substrate 11 preferably satisfy the relationship mp3≥mp1>mp2, and more preferably satisfy the relationship mp3>mp1>mp2.
[0092] Based on the same viewpoint, the absolute value of the difference between the melting peak temperature mp4 of the heat-fusible resin layer 35 of the outer packaging material 3 for the storage device used as the adhesive film 1 for metal terminal and the melting peak temperature mp2 of the second polyolefin layer 12b of the adhesive film 1 for metal terminal is preferably about 0 to 5°C or about 0 to 3°C. The smaller the absolute value of the difference between the melting peak temperature mp4 and the melting peak temperature mp2 (that is, the closer the absolute value of the difference is to 0°C), the higher the adhesion between the second polyolefin layer 12b and the heat-fusible resin layer 35 is likely to be. In particular, the smaller the absolute value of the difference between the melting peak temperature mp4 and the melting peak temperature mp2, the higher the high sealing performance and followability in a short time in the adhesive film 1 for metal terminal of the present invention can be.
[0093] From the viewpoint of obtaining the above-mentioned high sealing performance in a short time, suppressing collapse and further improving the tracking performance, in the adhesive film 1 for metal terminals of the present invention, the melt mass flow rate (MFR) T1 of the first polyolefin layer 12a and the melt mass flow rate (MFR) T2 of the second polyolefin layer 12b preferably satisfy the relationship of T2>T1. In the present invention, the method for measuring the melt mass flow rate (MFR) is as follows.
[0094] <Measurement of Melt Mass Flow Rate (MFR)>
[0095] The melt mass flow rate (g / 10min) of each measurement sample is measured using a melt indexer at a measurement temperature of 230°C and an applied weight of 2.16 kg. For example, for polyolefins, the method according to the A method specified in JIS K7210:2014 can be used. In addition, as a measurement sample, the first polyolefin layer, the second polyolefin layer, and the substrate can be obtained from the adhesive film for metal terminals to prepare a measurement sample.
[0096] Based on the same viewpoint, the melt mass flow rate (MFR) T1 of the first polyolefin layer 12a arranged on the side of the metal terminal 2 is preferably about 5.0 g / 10 min or more, and more preferably about 6.0 g / 10 min or more. Based on the same viewpoint, the melt mass flow rate (MFR) T1 is preferably about 10.0 g / 10 min or less, and more preferably about 8.0 g / 10 min or less. As the preferred range of the melt mass flow rate (MFR) T1, about 5.0 to 10.0 g / 10 minutes, about 5.0 to 8.0 g / 10 minutes, about 6.0 to 10.0 g / 10 minutes, and about 6.0 to 8.0 g / 10 minutes can be cited.
[0097] Based on the same viewpoint, the melt mass flow rate (MFR) T2 of the second polyolefin layer 12b disposed on the side of the outer packaging material 3 for the storage device is preferably about 8.0 g / 10 min or more, and more preferably about 10.0 g / 10 min or more. Based on the same viewpoint, the melt mass flow rate (MFR) T2 is preferably about 15.0 g / 10 min or less, and more preferably about 13.0 g / 10 min or less. As the preferred range of the melt mass flow rate (MFR) T2, about 8.0 to 15.0 g / 10 minutes, about 8.0 to 13.0 g / 10 minutes, about 10.0 to 15.0 g / 10 minutes, and about 10.0 to 13.0 g / 10 minutes can be cited.
[0098] Based on the same viewpoint, the melt mass flow rate (MFR) T3 of the substrate 11 is 1.0 g / 10 min or more, preferably about 1.5 g / 10 min or more, and more preferably about 2.0 g / 10 min or more. Based on the same viewpoint, the melt mass flow rate (MFR) T3 is preferably about 5.0 g / 10 min or less, and more preferably about 4.0 g / 10 min or less. The preferred range of the melt mass flow rate (MFR) T3 includes about 1.0 to 5.0 g / 10 minutes, about 1.0 to 4.0 g / 10 minutes, about 1.5 to 5.0 g / 10 minutes, about 1.5 to 4.0 g / 10 minutes, about 2.0 to 5.0 g / 10 minutes, and about 2.0 to 4.0 g / 10 minutes.
[0099] The absolute value of the difference between the melt mass flow rate (MFR) T1 of the first polyolefin layer 12a and the melt mass flow rate (MFR) T2 of the second polyolefin layer 12b is preferably about 2.0 to 6.0 g / 10 minutes, more preferably about 3.0 to 5.0 g / 10 minutes.
[0100] Based on the same viewpoint, it is preferred that the melt mass flow rate (MFR) T1 of the first polyolefin layer 12a is greater than the melt mass flow rate (MFR) T3 of the substrate 11, and the difference between the melt mass flow rate (MFR) T3 of the substrate 11 and the melt mass flow rate (MFR) T1 of the first polyolefin layer 12a (melt mass flow rate (MFR) T3-melt mass flow rate (MFR) T1) is preferably about 2.0 g / 10 min or more, more preferably about 2.5 g / 10 min or more, and further preferably about 3.0 g / 10 min or more. In addition, based on the same viewpoint, the difference is preferably about 6.0 g / 10 min or less, more preferably about 5.5 g / 10 min or less, and further preferably about 5.0 g / 10 min or less. Preferred ranges of the difference include about 2.0 to 6.0 g / 10 minutes, about 2.0 to 5.5 g / 10 minutes, about 2.0 to 5.0 g / 10 minutes, about 2.5 to 6.0 g / 10 minutes, about 2.5 to 5.5 g / 10 minutes, about 2.5 to 5.0 g / 10 minutes, about 3.0 to 6.0 g / 10 minutes, about 3.0 to 5.5 g / 10 minutes, and about 3.0 to 5.0 g / 10 minutes.
[0101] From the same viewpoint, the melt mass flow rate (MFR) T1 of the first polyolefin layer 12a, the melt mass flow rate (MFR) T2 of the second polyolefin layer 12b, and the melt mass flow rate (MFR) T3 of the substrate 11 preferably satisfy the relationship of T2>T1>T3.
[0102] Based on the same viewpoint, the absolute value of the difference between the melt mass flow rate (MFR) T4 of the heat-fusible resin layer 35 as the outer packaging material for the storage device using the adhesive film for metal terminal 1 and the melt mass flow rate (MFR) T2 of the second polyolefin layer 12b of the adhesive film for metal terminal 1 is preferably about 0.0 to 5.0 g / 10 minutes, or about 0.0 to 3.0 g / 10 minutes. The smaller the absolute value of the difference between the melt mass flow rate (MFR) T4 and the melt mass flow rate (MFR) T2 (that is, the closer the absolute value of the difference is to 0.0 g / 10min), the easier it is to improve the adhesion between the second polyolefin layer 12b and the heat-fusible resin layer 35. In particular, the smaller the absolute value of the difference between the melt mass flow rate (MFR) T4 and the melt mass flow rate (MFR) T2, the higher the high sealing performance and followability in a short time in the adhesive film for metal terminal 1 of the present invention can be further improved.
[0103] From the viewpoint of obtaining the above-mentioned high sealing performance in a short time, suppressing collapse and further improving the tracking performance, in the adhesive film 1 for metal terminals of the present invention, the total thickness of the adhesive film 1 for metal terminals is, for example, about 60 μm or more, preferably about 80 μm or more, more preferably about 100 μm or more, more preferably about 120 μm or more, and further preferably about 150 μm or more. In addition, the total thickness of the adhesive film 1 for metal terminals of the present invention is preferably about 300 μm or less, more preferably about 220 μm or less. As the preferred range of the total thickness of the adhesive film 1 for metal terminals of the present invention, about 60 to 300 μm, about 60 to 220 μm, about 80 to 300 μm, about 80 to 220 μm, about 100 to 300 μm, about 100 to 220 μm, about 120 to 300 μm, about 120 to 220 μm, about 150 to 300 μm, about 150 to 220 μm. As a more specific example, when the adhesive film 1 for metal terminals of the present invention is used for a consumer power storage device, the total thickness is preferably about 60 to 100 μm; when used for a vehicle-mounted power storage device, the total thickness is preferably about 100 to 220 μm.
[0104] Next, the materials, thicknesses, etc. constituting the first polyolefin layer 12 a , the second polyolefin layer 12 b , and the substrate 11 will be described in detail.
[0105] [First Polyolefin Layer 12a and Second Polyolefin Layer 12b]
[0106] like Figure 4 and Figure 5As shown, the adhesive film 1 for metal terminals of the present invention is provided with a first polyolefin layer 12a on one side of a substrate 11 and a second polyolefin layer 12b on the other side. The first polyolefin layer 12a is arranged on the side of the metal terminal 2. And the second polyolefin layer 12b is arranged on the side of the outer packaging material 3 for the storage device. In the adhesive film 1 for metal terminals of the present invention, the first polyolefin layer 12a and the second polyolefin layer 12b are respectively located on both side surfaces (of the adhesive film).
[0107] In the adhesive film 1 for metal terminals of the present invention, the first polyolefin layer 12a and the second polyolefin layer 12b are layers containing polyolefin resins, respectively. As polyolefin resins, polyolefins, acid-modified polyolefins, etc. can be cited. The first polyolefin layer 12a preferably contains an acid-modified polyolefin in the polyolefin resin, and more preferably is a layer formed by an acid-modified polyolefin. In addition, the second polyolefin layer 12b preferably contains a polyolefin or an acid-modified polyolefin in the polyolefin resin, more preferably contains a polyolefin, and further preferably is a layer formed by a polyolefin. Acid-modified polyolefins have a high affinity for metals. In addition, polyolefins have a very high affinity for heat-fusible resins such as polyolefins. Therefore, in the adhesive film 1 for metal terminals of the present invention, by configuring the first polyolefin layer 12a formed by acid-modified polyolefins on the metal terminal 2 side, it is possible to show better adhesion at the interface between the adhesive film 1 for metal terminals and the metal terminal 2. Furthermore, by arranging the second polyolefin layer 12 b made of polyolefin on the heat-fusible resin layer 35 side of the power storage device packaging material 3 , better adhesion can be achieved at the interface between the pressure-sensitive adhesive film 1 for metal terminal and the heat-fusible resin layer 35 .
[0108] Specific examples of preferred laminated structures of the adhesive film 1 for metal terminals of the present invention include a three-layer structure in which a first polyolefin layer formed by acid-modified polypropylene / a substrate formed by polypropylene / a second polyolefin layer formed by polypropylene are laminated in sequence; a three-layer structure in which a first polyolefin layer formed by acid-modified polypropylene / a substrate formed by polypropylene / a second polyolefin layer formed by acid-modified polypropylene are laminated in sequence, etc. Among them, a three-layer structure in which a first polyolefin layer formed by acid-modified polypropylene / a substrate formed by polypropylene / a second polyolefin layer formed by polypropylene are laminated in sequence is particularly preferred.
[0109] The acid-modified polyolefin is not particularly limited as long as it is an acid-modified polyolefin, and preferably, a polyolefin graft-modified with an unsaturated carboxylic acid or an anhydride thereof is used.
[0110] Specific examples of the acid-modified polyolefin include polyethylene such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylene such as homopolypropylene, polypropylene block copolymers (such as block copolymers of propylene and ethylene), and polypropylene random copolymers (such as random copolymers of propylene and ethylene); ethylene-butene-propylene terpolymers, etc. Among these polyolefins, polyethylene and polypropylene are preferred, and polypropylene is particularly preferred.
[0111] The acid-modified polyolefin may be a cyclic polyolefin. For example, the carboxylic acid-modified cyclic polyolefin refers to a polymer obtained by copolymerizing a part of the monomers constituting the cyclic polyolefin with an α,β-unsaturated carboxylic acid or its anhydride, or by block-polymerizing or graft-polymerizing an α,β-unsaturated carboxylic acid or its anhydride with a cyclic polyolefin.
[0112] The acid-modified cyclic polyolefin is a copolymer of an olefin and a cyclic monomer. As the olefin of the structural monomer of the cyclic polyolefin, for example, ethylene, propylene, 4-methyl-1-pentene, butadiene, isoprene, etc. can be cited. In addition, as the cyclic monomer of the structural monomer of the cyclic polyolefin, for example, cyclic olefins such as norbornene can be cited, and specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornadiene can be cited. Among these polyolefins, cyclic olefins can be preferably cited, and norbornene is more preferably cited. As the structural monomer, styrene can also be cited.
[0113] Examples of the carboxylic acid or its anhydride used for acid modification include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, etc. When the first polyolefin layer 12a is analyzed by infrared spectroscopy, it is preferred that a peak derived from maleic anhydride can be detected. For example, when maleic anhydride-modified polyolefin is measured by infrared spectroscopy, a peak at a wave number of 1760 cm ﹣1 Nearby and wave number 1780cm ﹣1 In the vicinity, the peak from maleic anhydride can be detected. When the first polyolefin layer 12a or the second polyolefin layer 12b is a layer formed by maleic anhydride-modified polyolefin, using infrared spectroscopy to measure, the peak from maleic anhydride can be detected. However, when the acid modification degree is low, the peak value becomes smaller and may not be detected. In this case, analysis can be performed by nuclear magnetic resonance spectroscopy.
[0114] The first polyolefin layer 12a and the second polyolefin layer 12b may be formed of a single resin component, or may be formed of a blended polymer composed of two or more resin components. Furthermore, the first polyolefin layer 12a and the second polyolefin layer 12b may each be formed of only one layer, or may be formed of two or more layers composed of the same or different resin components. From the viewpoint of the film-forming properties of the first polyolefin layer 12a and the second polyolefin layer 12b, these layers are preferably formed of a blended polymer composed of two or more resin components. When forming a blended polymer, the first polyolefin layer 12a preferably has acid-modified polypropylene as the main component (a component of 50% by mass or more), and 50% by mass or less is other resin (preferably polyethylene from the viewpoint of improving flexibility). In addition, for the second polyolefin layer 12b, it is preferred that polypropylene is the main component (a component of 50% by mass or more), and 50% by mass or less is other resin (preferably polyethylene from the viewpoint of improving flexibility). On the other hand, from the viewpoint of the electrolyte corrosion resistance of the first polyolefin layer 12a and the second polyolefin layer 12b, the first polyolefin layer 12a preferably contains acid-modified polypropylene alone as a resin, and the second polyolefin layer 12b preferably contains polypropylene alone as a resin.
[0115] Moreover, the first polyolefin layer 12a and the second polyolefin layer 12b may contain fillers as needed. By adding fillers, the first polyolefin layer 12a and the second polyolefin layer 12b can effectively suppress the short circuit between the metal terminal 2 and the barrier layer 33 of the outer packaging material 3 for the storage device because the fillers function as spacers. As the particle size of the filler, a range of about 0.1 to 35 μm, preferably about 5.0 to 30 μm, and more preferably about 10 to 25 μm can be cited. In addition, as the content of the filler, about 5 to 30 parts by mass can be cited relative to 100 parts by mass of the resin component forming the first polyolefin layer 12a and the second polyolefin layer 12b, respectively, and more preferably about 10 to 20 parts by mass.
[0116] As filler, any one of inorganic filler and organic filler can be used. As inorganic filler, for example, carbon (carbon, graphite), silica, aluminum oxide, barium titanate, iron oxide, silicon carbide, zirconium oxide, zirconium silicate, magnesium oxide, titanium oxide, calcium aluminate, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, calcium carbonate, etc. can be cited. In addition, as organic filler, for example, fluororesin, phenolic resin, urea resin, epoxy resin, acrylic resin, benzoguanamine-formaldehyde condensate, melamine-formaldehyde condensate, polymethyl methacrylate crosslinked body, polyethylene crosslinked body, etc. can be cited. From the viewpoint of shape stability, rigidity, and resistance to corrosion of contents, aluminum oxide, silica, fluororesin, acrylic resin, benzoguanamine-formaldehyde condensate are preferred, and spherical aluminum oxide and silica are particularly preferred. As a mixing method for mixing fillers into the resin components that form the first polyolefin layer 12a and the second polyolefin layer 12b, a method of preliminarily melt-mixing the two using a Banbury mixer to form a masterbatch and setting the masterbatch to a predetermined mixing ratio, or a method of directly mixing with the resin components can be adopted.
[0117] In addition, the first polyolefin layer 12a and the second polyolefin layer 12b may contain pigments as needed. As the pigment, various inorganic pigments can be used. As a specific example of the pigment, preferably carbon (carbon, graphite) exemplified in the above-mentioned filler can be cited. Carbon (carbon, graphite) is a material commonly used inside the storage device, and there is no risk of dissolving into the electrolyte. Moreover, not only can a sufficient coloring effect be obtained with an amount added that does not hinder the adhesion due to the good coloring effect, but also it will not melt due to heat, and the apparent melt viscosity of the added resin can be increased. Moreover, it can prevent the pressurized portion from becoming thinner during thermal bonding (heat sealing), and can impart excellent sealing properties between the outer packaging material for the storage device and the metal terminal.
[0118] When a pigment is added to the first polyolefin layer 12a and the second polyolefin layer 12b, the amount of the pigment added can be, for example, about 0.05 to 0.3 parts by mass, preferably about 0.1 to 0.2 parts by mass, relative to 100 parts by mass of the resin component forming the first polyolefin layer 12a and the second polyolefin layer 12b, when carbon black having a particle size of about 0.03 μm is used. By adding a pigment to the first polyolefin layer 12a and the second polyolefin layer 12b, it is possible to detect the presence of the adhesive film 1 for metal terminals by using a sensor or by visual inspection. It is particularly preferred that the first polyolefin layer 12a contains a pigment. It should be noted that, when fillers and pigments are added to the first polyolefin layer 12a and the second polyolefin layer 12b, the fillers and pigments can be added to the same first polyolefin layer 12a and the second polyolefin layer 12b. From the viewpoint of not hindering the thermal fusion bonding of the adhesive film 1 for metal terminals, the fillers and pigments are preferably added separately to the first polyolefin layer 12a and the second polyolefin layer 12b.
[0119] From the viewpoint of obtaining the above-mentioned high sealing performance in a short period of time, suppressing collapse and further improving the tracking performance, in the adhesive film 1 for metal terminals of the present invention, the thickness of the first polyolefin layer 12a and the second polyolefin layer 12b are preferably about 10 μm or more, more preferably about 15 μm or more, further preferably about 20 μm or more, and further preferably about 30 μm or more; and are preferably about 60 μm or less, more preferably about 55 μm or less, further preferably about 50 μm or less, and further preferably 40 μm or less. Preferred ranges for the thickness of the first polyolefin layer 12a and the second polyolefin layer 12b include about 10 to 60 μm, about 10 to 55 μm, about 10 to 50 μm, about 10 to 40 μm, about 15 to 60 μm, about 15 to 55 μm, about 15 to 50 μm, about 15 to 40 μm, about 20 to 60 μm, about 20 to 55 μm, about 20 to 50 μm, about 20 to 40 μm, about 30 to 60 μm, about 30 to 55 μm, about 30 to 50 μm, and about 30 to 40 μm, respectively.
[0120] Based on the same viewpoint, the ratio of the thickness of the substrate 11 to the total thickness of the first polyolefin layer 12a and the second polyolefin layer 12b is preferably about 0.3 or more, more preferably about 0.4 or more, and further preferably about 0.5 or more. In addition, it is preferably about 1.0 or less, and more preferably about 0.8 or less. Preferred ranges include 0.3 to 1.0, 0.3 to 0.8, 0.4 to 1.0, 0.4 to 0.8, 0.5 to 1.0, and 0.5 to 0.8.
[0121] Furthermore, when the total thickness of the adhesive film for metal terminal 1 is 100%, the ratio of the total thickness of the first polyolefin layer 12a and the second polyolefin layer 12b is preferably about 30 to 80%, more preferably about 50 to 70%.
[0122] [Substrate 11]
[0123] In the adhesive film for metal terminal 1 , the base material 11 is a layer provided as necessary and functions as a support body of the adhesive film for metal terminal 1 .
[0124] There is no particular limitation on the material forming the substrate 11. Examples of the material forming the substrate 11 include polyolefin resins, polyamide resins, polyester resins, epoxy resins, acrylic resins, fluororesins, silicone resins, phenolic resins, polyetherimides, polyimides, polycarbonates, and mixtures or copolymers thereof, among which polyolefin resins are particularly preferred. That is, the material forming the substrate 11 is preferably a resin having a polyolefin skeleton, such as polyolefin or acid-modified polyolefin. The fact that the resin constituting the substrate 11 has a polyolefin skeleton can be analyzed by, for example, infrared spectroscopy, gas chromatography-mass spectrometry, and the like.
[0125] As described above, the substrate 11 preferably contains a polyolefin resin, preferably contains polyolefin, and more preferably is a layer formed by polyolefin. The layer formed by polyolefin can be a stretched polyolefin film or an unstretched polyolefin film, preferably an unstretched polyolefin film. As polyolefins, specific examples include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, polypropylene block copolymers (such as block copolymers of propylene and ethylene), and polypropylene random copolymers (such as random copolymers of propylene and ethylene); ethylene-butene-propylene terpolymers, etc. Among these polyolefins, polyethylene and polypropylene can be preferably mentioned, and polypropylene is more preferably. In addition, due to its excellent resistance to electrolyte corrosion, the substrate 11 preferably contains homopolypropylene, more preferably is formed by homopolypropylene, and further preferably is an unstretched homopolypropylene film.
[0126] Specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (I represents isophthalic acid and T represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid, and polyamides containing aromatic compounds such as poly(meta-xylylene adipamide) (MXD6); alicyclic polyamides such as polyaminomethylcyclohexyl adipamide (PACM6); and polyamides copolymerized with lactam components and isocyanate components such as 4,4'-diphenylmethane-diisocyanate, polyester amide copolymers and polyether ester amide copolymers which are copolymers of copolymerized polyamides and polyesters and / or polyalkylene ether glycols; copolymers of the above compounds, etc. These polyamides may be used alone or in combination of two or more.
[0127] Specific examples of the polyester include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, copolyesters containing ethylene terephthalate as a main repeating unit, and copolyesters containing butylene terephthalate as a main repeating unit. In addition, specific examples of copolymer polyesters with ethylene terephthalate as the main repeating unit include copolymer polyesters with ethylene terephthalate as the main repeating unit and ethylene isophthalate (hereinafter referred to as poly(ethylene terephthalate / isophthalate)), poly(ethylene terephthalate / isophthalate), poly(ethylene terephthalate / adipate), poly(ethylene terephthalate / sodium sulfonate), poly(ethylene terephthalate / sodium isophthalate), poly(ethylene terephthalate / phenyl dicarboxylic acid), poly(ethylene terephthalate / sebacyl carboxylic acid), and the like. In addition, as the copolyester with butylene terephthalate as the main repeating unit, specifically, there can be mentioned copolymer polyester with butylene terephthalate as the main repeating unit and butylene isophthalate (hereinafter referred to as poly(butylene terephthalate / isophthalate)), poly(butylene terephthalate / adipate), poly(butylene terephthalate / sebacate), poly(butylene terephthalate / sebacate), polybutylene naphthalate, etc. These polyesters can be used alone or in combination of two or more.
[0128] In addition, the substrate 11 may also be formed of a nonwoven fabric made of the above-mentioned resin. When the substrate 11 is a nonwoven fabric, the substrate 11 is preferably made of the above-mentioned polyolefin resin, polyamide resin, or the like.
[0129] The substrate 11 may be a single layer or a multilayer. When the substrate 11 is a multilayer, it may include at least one layer having the above-mentioned heat of fusion ΔH3 of 70 J / g or more. As a specific example of a multilayer, a three-layer structure of block polypropylene / homopolypropylene / block polypropylene stacked in sequence may be cited.
[0130] In addition, the base material 11 may be a layer containing a colorant by adding a colorant to the base material 11. In addition, the light transmittance may be adjusted by selecting a resin with low transparency. When the base material 11 is a film, a colored film or a film with low transparency may be used. In addition, when the base material 11 is a non-woven fabric, a non-woven fabric using fibers containing a colorant, an adhesive, etc., or a non-woven fabric with low transparency may be used.
[0131] When the substrate 11 is composed of a resin film, the surface of the substrate 11 may be subjected to a known adhesion facilitating treatment such as a corona discharge treatment, an ozone treatment, or a plasma treatment as required.
[0132] From the viewpoint of obtaining the above-mentioned high sealing performance in a short time, suppressing collapse and further improving the tracking performance, in the adhesive film 1 for metal terminals of the present invention, the thickness of the substrate 11 is preferably 120 μm or less, more preferably 100 μm or less, more preferably about 80 μm or less, and further preferably about 70 μm or less. In addition, the thickness of the substrate 11 is preferably about 20 μm or more, more preferably about 30 μm or more, and further preferably about 40 μm or more. As the preferred range of the thickness of the substrate 11, about 20 to 120 μm, about 20 to 100 μm, about 20 to 80 μm, about 20 to 70 μm, about 30 to 120 μm, about 30 to 100 μm, about 30 to 80 μm, about 30 to 70 μm, about 40 to 120 μm, about 40 to 100 μm, about 40 to 80 μm, about 40 to 70 μm, about 40 to 100 μm, about 40 to 80 μm, about 40 to 70 μm.
[0133] [Adhesion promoter layer 13]
[0134] The adhesion promoter layer 13 is a layer provided for the purpose of firmly bonding the substrate 11 to the first polyolefin layer 12a and the second polyolefin layer 12b as required (see Figure 5 The adhesion promoter layer 13 may be provided on one side between the substrate 11 and the first polyolefin layer 12a and the second polyolefin layer 12b, or may be provided on both sides.
[0135] The adhesion promoter layer 13 can be formed by using known adhesion promoters such as isocyanate, polyethyleneimine, polyester, polyurethane and polybutadiene. From the viewpoint of further improving the corrosion resistance of the electrolyte, it is preferably formed by an isocyanate adhesion promoter. As an isocyanate adhesion promoter, the lamination strength of the adhesion promoter made of isocyanate components selected from triisocyanate monomers and poly MDI is high, and the lamination strength decreases less after immersion in the electrolyte. It is particularly preferred to be formed by an adhesion promoter containing triphenylmethane-4,4',4"-triisocyanate as a triisocyanate monomer and polymethylene polyphenyl polyisocyanate (NCO content is about 30%, viscosity is 200 to 700 mPa·s) as poly MDI. In addition, it is also preferably formed by a two-component curing type adhesion promoter with tri(p-isocyanatephenyl)thiophosphate or polyethyleneimine as a triisocyanate monomer as the main component and polycarbodiimide as a cross-linking agent.
[0136] The adhesion promoter layer 13 can be formed by coating and drying by a known coating method such as a bar coating method, a roll coating method, a gravure coating method, etc. The coating amount of the adhesion promoter is 20 to 100 mg / m2 in the case of an adhesion promoter made of triisocyanate. 2 About 40 to 60 mg / m 2 In the case of an adhesion promoter made of polymer MDI, it is 40 to 150 mg / m 2 About 60 to 100 mg / m 2 In the case of a two-component curing adhesion promoter with polyethylene imine as the main component and polycarbodiimide as the crosslinking agent, 5 to 50 mg / m 2 About 10 to 30 mg / m 2 It should be noted that the triisocyanate monomer is a monomer having three isocyanate groups in one molecule, and the polymerized MDI is a mixture of MDI and MDI oligomers obtained by polymerization of MDI, which is a compound shown in the following formula.
[0137] [Chemical formula 1]
[0138]
[0139] The adhesive film 1 for metal terminals of the present invention can be manufactured by laminating the first polyolefin layer 12a and the second polyolefin layer 12b on both side surfaces of the substrate 11, for example. The lamination of the substrate 11 with the first polyolefin layer 12a and the second polyolefin layer 12b can be performed by a known method such as an extrusion lamination method, a T-die method, an expansion method or a heat lamination method. In addition, when the substrate 11 and the first polyolefin layer 12a and the second polyolefin layer 12b are laminated with the aid of the adhesion promoter layer 13, the adhesion promoter constituting the adhesion promoter layer 13 can be applied on the substrate 11 by the above method, dried, and the first polyolefin layer 12a and the second polyolefin layer 12b are laminated respectively from above the adhesion promoter layer 13.
[0140] There is no particular limitation on the method of placing the adhesive film for metal terminal 1 between the metal terminal 2 and the outer packaging material 3 for the power storage device. Figures 1 to 3 As shown, the adhesive film 1 for metal terminals is wrapped around the metal terminal 2 at the portion of the metal terminal 2 held by the outer packaging material 3 for the storage device. In addition, the portion of the metal terminal 2 held by the outer packaging material 3 for the storage device, which is not shown in the figure, may be omitted, and the adhesive film 1 for metal terminals may be provided on both sides of the metal terminal 2 in such a manner that the adhesive film 1 for metal terminals crosses the two metal terminals 2.
[0141] [Metal terminal 2]
[0142] The adhesive film 1 for metal terminals of the present invention is used in a manner of being arranged between a metal terminal 2 and an outer packaging material 3 for an electrical storage device. The metal terminal 2 (Tab) is a conductive member electrically connected to an electrode (positive electrode or negative electrode) of an electrical storage device element 4 and is made of a metal material. There are no particular restrictions on the metal material constituting the metal terminal 2, and examples thereof include aluminum, nickel, copper, and the like. For example, the metal terminal 2 connected to the positive electrode of a lithium-ion electrical storage device is usually made of aluminum or the like. In addition, the metal terminal 2 connected to the negative electrode of a lithium-ion electrical storage device is usually made of copper, nickel, or the like.
[0143] From the viewpoint of improving the corrosion resistance of the electrolyte, the surface of the metal terminal 2 is preferably subjected to a chemical conversion treatment. For example, when the metal terminal 2 is made of aluminum, as a specific example of the chemical conversion treatment, a known method of forming a corrosion-resistant film such as a phosphate, a chromate, a fluoride, a triazine thiol compound, etc. can be cited. Among the methods for forming the corrosion-resistant film, a phosphochromate treatment using a three-component composition of a phenolic resin, a chromium (III) fluoride compound, and phosphoric acid is suitable.
[0144] The size of the metal terminal 2 can be appropriately set according to the size of the power storage device used. As the thickness of the metal terminal 2, it is preferably about 50 to 1000 μm, and more preferably about 70 to 800 μm. In addition, as the length of the metal terminal 2, it is preferably about 1 to 200 mm, and more preferably about 3 to 150 mm. In addition, as the width of the metal terminal 2, it is preferably about 1 to 200 mm, and more preferably about 3 to 150 mm.
[0145] [Outer packaging materials for power storage devices 3]
[0146] As the outer packaging material 3 for the power storage device, there can be mentioned a member having a laminated structure in which at least a base material layer 31, a barrier layer 33 and a heat-fusible resin layer 35 are laminated in this order. Figure 6 In the figure, as an example of the cross-sectional structure of the outer packaging material 3 for a storage device, a substrate layer 31, an adhesive layer 32 provided as required, a barrier layer 33, an adhesive layer 34 provided as required, and a heat-fusible resin layer 35 are stacked in sequence. In the outer packaging material 3 for a storage device, the substrate layer 31 becomes the outer layer side, and the heat-fusible resin layer 35 becomes the innermost layer. When the storage device is assembled, the surfaces of the heat-fusible resin layer 35 located on the periphery of the storage device element 4 contact each other and are heat-fused, so that the storage device element 4 is sealed and the packaging of the storage device element 4 is achieved. It should be noted that Figure 1 to Figure 3 The figure shows the storage device 10 in the case of an embossed storage device outer packaging material 3 formed by embossing molding, but the storage device outer packaging material 3 can also be a soft package type (pouch type) without molding. It should be noted that the soft package type can be any type, such as three-way sealing, four-way sealing, pillow type, etc.
[0147] There is no particular limitation on the thickness of the laminate constituting the outer packaging material 3 for the storage device. As for the upper limit, from the perspective of cost reduction and energy density improvement, it is preferably about 190 μm or less, about 180 μm or less, about 160 μm or less, about 155 μm or less, about 140 μm or less, about 130 μm or less, or about 120 μm or less. As for the lower limit, from the perspective of maintaining the function of the outer packaging material 3 for the storage device such as protecting the storage device element 4, it is preferably about 35 μm or more, about 45 μm or more, about 60 μm or more, or about 80 μm or more. As a preferred range, for example, about 35 to 190 μm, about 35 to 180 μm, about 35 to 160 μm, about 35 to 155 μm, about 35 to About 140μm, about 35-130μm, about 35-120μm, about 45-190μm, about 45-180μm, about 45-160μm, about 45-155μm, about 45-140μm, about 45-130μm, about 45-120μm, about 60-190μm, about 60-180μm, about 60-160μm, about 60-155μm, about 60-140μm, about 60-130μm, about 60-120μm, about 80-190μm, about 80-180μm, about 80-160μm, about 80-155μm, about 80-140μm, about 80-130μm, about 80-120μm.
[0148] (Base material layer 31)
[0149] In the electricity storage device packaging material 3 , the base material layer 31 is a layer that functions as a base material of the electricity storage device packaging material and is a layer forming the outermost layer side.
[0150] There are no particular restrictions on the material forming the substrate layer 31 as long as it has insulating properties. Examples of the material forming the substrate layer 31 include polyester, polyamide, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, phenolic resin, polyetherimide, polyimide, and mixtures and copolymers thereof. Polyesters such as polyethylene terephthalate and polybutylene terephthalate are suitable as the material forming the substrate layer 31 because of their good resistance to corrosion by electrolytes and their difficulty in whitening due to the adhesion of electrolytes. In addition, polyamide films are suitable as the material forming the substrate layer 31 because of their excellent ductility and the ability to prevent whitening caused by resin cracking of the substrate layer 31 during molding.
[0151] The substrate layer 31 may be formed of a uniaxially or biaxially stretched resin film, or may be formed of an unstretched resin film. Among them, a uniaxially or biaxially stretched resin film, particularly a biaxially stretched resin film, may be suitably used as the substrate layer 31 because it has improved heat resistance through oriented crystallization.
[0152] Among them, the resin film forming the base material layer 31 is preferably nylon or polyester, and more preferably biaxially stretched nylon or biaxially stretched polyester.
[0153] In order to improve the anti-pinhole property and the insulation property when forming the package of the storage device, the substrate layer 31 can also be a laminate of resin films of different materials. Specifically, a multilayer structure of a laminate of polyester film and nylon film, a multilayer structure of a laminate of biaxially stretched polyester and biaxially stretched nylon, etc. can be cited. When the substrate layer 31 forms a multilayer structure, each resin film can be bonded by an adhesive, or can be directly laminated without an adhesive. In the case of bonding without an adhesive, for example, a method of bonding in a hot melt state such as a coextrusion method, a frosted lamination method, a hot lamination method, etc. can be cited.
[0154] In addition, the substrate layer 31 may be subjected to a low friction treatment to improve formability. When the substrate layer 31 is subjected to a low friction treatment, there is no particular limitation on the coefficient of friction of the surface thereof, and for example, it may be 1.0 or less. In order to perform a low friction treatment on the substrate layer 31, for example, a matte treatment, the formation of a lubricant film layer, or a combination thereof may be cited.
[0155] The thickness of the base material layer 31 is, for example, about 10 to 50 μm, preferably about 15 to 30 μm.
[0156] (Adhesive layer 32)
[0157] In the power storage device packaging material 3 , the adhesive layer 32 is a layer disposed on the base layer 31 as necessary in order to impart adhesion to the base layer 31 . That is, the adhesive layer 32 is provided between the base layer 31 and the barrier layer 33 .
[0158] The adhesive layer 32 is formed of an adhesive that can bond the substrate layer 31 to the barrier layer 33. The adhesive used to form the adhesive layer 32 may be a two-component curing adhesive or a one-component curing adhesive. In addition, the bonding mechanism of the adhesive used to form the adhesive layer 32 is not particularly limited, and may be any of a chemical reaction type, a solvent volatilization type, a hot melt type, a hot pressing type, and the like.
[0159] As the resin component of the adhesive that can be used to form the adhesive layer 32, preferably, there can be mentioned polyurethane-based two-component curing adhesives; polyamides, polyesters or blended resins of these with modified polyolefins, from the viewpoint of having excellent ductility, durability under high humidity conditions, yellowing inhibition, thermal degradation inhibition during heat sealing, etc., being able to inhibit the reduction in the lamination strength between the substrate layer 31 and the barrier layer 33, and effectively inhibiting the occurrence of peeling.
[0160] In addition, the adhesive layer 32 may be formed into multiple layers using different adhesive components. When the adhesive layer 32 is formed into multiple layers using different adhesive components, from the viewpoint of improving the lamination strength between the substrate layer 31 and the barrier layer 33, it is preferred to select a resin having excellent adhesion to the substrate layer 31 as the adhesive component disposed on the substrate layer 31 side, and to select an adhesive component having excellent adhesion to the barrier layer 33 as the adhesive component disposed on the barrier layer 33 side. When the adhesive layer 32 is formed into multiple layers using different adhesive components, specifically, as the adhesive component disposed on the barrier layer 33 side, preferably, acid-modified polyolefins, metal-modified polyolefins, mixed resins of polyesters and acid-modified polyolefins, resins containing copolyesters, and the like can be cited.
[0161] The thickness of the adhesive layer 32 is, for example, about 2 to 50 μm, preferably about 3 to 25 μm.
[0162] (Barrier layer 33)
[0163] In the outer packaging material for the storage device, the barrier layer 33 is a layer that has the function of preventing water vapor, oxygen, light, etc. from invading the interior of the storage device in addition to the function of improving the strength of the outer packaging material for the storage device. The barrier layer 33 is preferably a metal layer, that is, a layer formed of metal. As the metal constituting the barrier layer 33, aluminum, stainless steel, titanium, etc. can be specifically mentioned, and aluminum can be preferably mentioned. The barrier layer 33 can be formed of, for example, metal foil or metal vapor-deposited film, inorganic oxide vapor-deposited film, carbon-containing inorganic oxide vapor-deposited film, a thin film provided with these vapor-deposited films, etc., preferably formed of metal foil, and more preferably formed of aluminum foil. When manufacturing an outer packaging material for a storage device, from the viewpoint of preventing wrinkles and pinholes from forming in the barrier layer 33, it is more preferable that the barrier layer is formed of a soft aluminum foil such as annealed aluminum (JIS H4160: 1994A8021H-O, JIS H4160: 1994A8079H-O, JIS H4000: 2014A8021P-O, JIS H4000: 2014A8079P-O).
[0164] The thickness of the barrier layer 33 is preferably about 10 to 200 μm, more preferably about 20 to 100 μm, from the viewpoint of making the outer packaging material for a power storage device thin and less likely to generate pinholes due to molding.
[0165] In addition, for the purpose of stabilizing adhesion, preventing dissolution and corrosion, etc., it is preferred that at least one surface, preferably both surfaces, of the barrier layer 33 be chemically treated. In the present invention, chemical treatment refers to a treatment for forming a corrosion-resistant film on the surface of the barrier layer.
[0166] (Adhesive layer 34)
[0167] In the power storage device packaging material 3 , the adhesive layer 34 is a layer provided between the barrier layer 33 and the thermally-adhesive resin layer 35 as necessary in order to firmly adhere the thermally-adhesive resin layer 35 .
[0168] The adhesive layer 34 is formed of an adhesive that can bond the barrier layer 33 to the heat-fusible resin layer 35. The composition of the adhesive used to form the adhesive layer is not particularly limited, and an example thereof may be a resin composition containing an acid-modified polyolefin. Examples of the acid-modified polyolefin include the same compounds as those exemplified in the first polyolefin layer 12a and the second polyolefin layer 12b.
[0169] The thickness of the adhesive layer 34 is, for example, about 1 to 40 μm, preferably about 2 to 30 μm.
[0170] (Thermal Fusible Resin Layer 35)
[0171] In the electricity storage device packaging material 3, the heat-fusible resin layer 35 corresponds to the innermost layer, and is a layer in which the heat-fusible resin layers are heat-fused to each other to seal the electricity storage device element when the electricity storage device is assembled.
[0172] As described above, the absolute value of the difference between the heat of fusion ΔH4 of the heat-fusible resin layer 35 of the storage device outer packaging material 3 using the adhesive film for metal terminal 1 of the present invention and the heat of fusion ΔH2 of the second polyolefin layer 12b of the adhesive film for metal terminal 1 is preferably about 0.0 to 5.0 J / g or about 0.0 to 3.0 J / g. The smaller the absolute value of the difference between the heat of fusion ΔH4 and the heat of fusion ΔH2 (that is, the closer the absolute value of the difference is to 0.0 J / g), the easier it is to improve the adhesion between the second polyolefin layer 12b and the heat-fusible resin layer 35.
[0173] The resin component used for the heat-fusible resin layer 35 is not particularly limited as long as it can be heat-fusible. Examples thereof include polyolefins and cyclopolyolefins.
[0174] In addition, as described above, the absolute value of the difference between the melting peak temperature mp4 of the heat-fusible resin layer 35 of the outer packaging material for the storage device using the adhesive film 1 for metal terminals of the present invention and the melting peak temperature mp2 of the second polyolefin layer 12b of the adhesive film 1 for metal terminals is preferably about 0 to 5° C. or about 0 to 3° C. The smaller the absolute value of the difference between the melting peak temperature mp4 and the melting peak temperature mp2 (that is, the closer the absolute value of the difference is to 0° C.), the easier it is to improve the adhesion between the second polyolefin layer 12b and the heat-fusible resin layer 35.
[0175] In addition, as described above, the absolute value of the difference between the melt mass flow rate (MFR) T4 of the heat-fusible resin layer 35 of the outer packaging material for the storage device using the adhesive film for metal terminal 1 of the present invention and the melt mass flow rate (MFR) T2 of the second polyolefin layer 12b of the adhesive film for metal terminal 1 is preferably about 0 to 5 g / 10 minutes or about 0 to 3 g / 10 minutes. The smaller the absolute value of the difference between the melt mass flow rate (MFR) T4 and the melt mass flow rate (MFR) T2 (that is, the closer the absolute value of the difference is to 0 g / 10 minutes), the easier it is to improve the adhesion between the second polyolefin layer 12b and the heat-fusible resin layer 35.
[0176] As the above-mentioned polyolefin, specifically, polyethylene such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene can be cited; crystalline or amorphous polypropylene such as homopolypropylene, polypropylene block copolymers (such as block copolymers of propylene and ethylene), and polypropylene random copolymers (such as random copolymers of propylene and ethylene); ethylene-butene-propylene terpolymers, etc. Among these polyolefins, polyethylene and polypropylene can be preferably cited.
[0177] The above-mentioned cyclopolyolefin is a copolymer of an olefin and a cyclic monomer. As the olefin of the structural monomer of the above-mentioned cyclopolyolefin, for example, ethylene, propylene, 4-methyl-1-pentene, butadiene, isoprene, etc. can be cited. In addition, as the cyclic monomer of the structural monomer of the above-mentioned cyclopolyolefin, for example, cycloolefins such as norbornene can be cited, and specifically, cyclopentadiene, dicyclopentadiene, cyclohexadiene, cyclodiene, and the like cyclic dienes can be cited. Among these polyolefins, cycloolefins can be preferably cited, and norbornene is more preferably cited. As a structural monomer, styrene can also be cited.
[0178] Among these resin components, preferred are crystalline or amorphous polyolefins, cyclic polyolefins, and polymer blends of these olefins; more preferred are polyethylene, polypropylene, copolymers of ethylene and norbornene, and polymer blends of two or more of the above compounds.
[0179] The heat-fusible resin layer 35 may be formed of a single resin component or a blended polymer of two or more resin components. Furthermore, the heat-fusible resin layer 35 may be formed of only one layer or two or more layers of the same or different resin components. When the second polyolefin layer 12b and the heat-fusible resin layer 35 use the same resin, it is particularly preferred because the adhesion between them can be improved.
[0180] The thickness of the thermally fusible resin layer 35 is not particularly limited, and is, for example, about 2 to 2000 μm, preferably about 5 to 1000 μm, and more preferably about 10 to 500 μm.
[0181] 2. Power storage devices
[0182] The electric storage device 10 of the present invention comprises an electric storage device element 4 having at least a positive electrode, a negative electrode and an electrolyte, an outer packaging material 3 for an electric storage device for packaging the electric storage device element 4, and metal terminals 2 electrically connected to the positive electrode and the negative electrode, respectively, and protruding to the outside of the outer packaging material 3 for the electric storage device. In the electric storage device 10 of the present invention, it is characterized in that the adhesive film 1 for metal terminals of the present invention is provided between the metal terminal 2 and the outer packaging material 3 for the electric storage device. That is, the electric storage device 10 of the present invention can be produced by a method having a step of providing the adhesive film 1 for metal terminals of the present invention between the metal terminal 2 and the outer packaging material 3 for the electric storage device.
[0183] Specifically, an electric storage device element 4 having at least a positive electrode, a negative electrode and an electrolyte is covered with an outer packaging material 3 for an electric storage device, and the metal terminals 2 connected to the positive electrode and the negative electrode are allowed to protrude to the outside thereof, and the adhesive film 1 for metal terminals of the present invention is sandwiched between the metal terminals 2 and the heat-fusible resin layer 35, and a flange portion (a region where the heat-fusible resin layers 35 are in contact with each other, the outer packaging material 3a of the electric storage device) is formed at the periphery of the electric storage device element 4, and the heat-fusible resin layers 35 of the flange portion are sealed by heat sealing, thereby providing an electric storage device 10 using the outer packaging material 3 for an electric storage device. It should be noted that when the outer packaging material 3 for an electric storage device is used to accommodate the electric storage device element 4, the member is used in such a manner that the heat-fusible resin layer 35 of the outer packaging material 3 for an electric storage device is on the inner side (the surface in contact with the electric storage device element 4).
[0184] The outer packaging material for the storage device of the present invention can be applied to storage devices such as batteries (including capacitors (condenser), capacitors (capacitor) etc.). In addition, the outer packaging material for the storage device of the present invention can be used for any of primary batteries and secondary batteries, preferably secondary batteries. There is no particular restriction on the type of secondary battery to which the outer packaging material for the storage device of the present invention is applicable, and examples thereof include lithium ion batteries, lithium ion polymer batteries, all-solid-state batteries, lead-acid batteries, nickel-hydrogen batteries, nickel-cadmium batteries, nickel-iron batteries, nickel-zinc batteries, silver-zinc oxide batteries, metal-air batteries, multivalent cation batteries, capacitors, capacitors etc. Among these secondary batteries, lithium ion batteries and lithium ion polymer batteries can be cited as preferred applicable objects of the outer packaging material for the storage device of the present invention.
[0185] Example
[0186] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.
[0187] <Manufacturing of Adhesive Film for Metal Terminal>
[0188] Examples 1 to 8, 10, 11, and 13
[0189] Maleic anhydride modified polypropylene (PPa) was prepared as the polyolefin forming the first polyolefin layer disposed on the metal terminal side, polypropylene (PP) was prepared as the polyolefin forming the second polyolefin layer disposed on the outer packaging material side for the storage device, and an unstretched polypropylene film (CPP, homopolypropylene) was prepared as the substrate. Then, in Examples 1 to 8, 10, 11, and 13, maleic anhydride modified polypropylene (PPa) was extruded on one side of the substrate (CPP) by a T-die extruder to form the first polyolefin layer; and polypropylene (PP) was extruded on the other side of the substrate (CPP) by a T-die extruder to form the second polyolefin layer, thereby obtaining an adhesive film for metal terminals in which the first polyolefin layer (PPa layer) / substrate (CPP layer) / second polyolefin layer (PP layer) were sequentially laminated. Regarding the laminated structure including the thickness of each layer, Examples 1, 2, and 10 are the first polyolefin layer (PPa layer, thickness 50 μm) / substrate (CPP layer, thickness 50 μm) / second polyolefin layer (PP layer, thickness 50 μm); Examples 3 to 8 and 11 are the first polyolefin layer (PPa layer, thickness 50 μm) / substrate (CPP layer, thickness 60 μm) / second polyolefin layer (PP layer, thickness 40 μm); Example 13 is the first polyolefin layer (PPa layer, thickness 20 μm) / substrate (CPP layer, thickness 40 μm) / second polyolefin layer (PP layer, thickness 20 μm). The heat of fusion, melting peak temperature, and melt mass flow rate (MFR) of the first polyolefin layer, the second polyolefin layer, and the substrate are shown in Tables 1 to 3, respectively. These physical property values are values adjusted according to the composition of each resin (ratio of polyethylene components, etc.), molecular weight, etc.
[0190] Example 9
[0191] In the same manner as in Example 1, an adhesive film for metal terminals in which the first polyolefin layer (PPa layer, 50 μm thick) / substrate (the above-mentioned 3-layer film, with a total thickness of 50 μm) / second polyolefin layer (PP layer, 50 μm thick) are laminated in sequence is obtained, except that the unstretched polypropylene film (CPP, homopolypropylene) is replaced with a 3-layer film in which block polypropylene (thickness 5 μm) / homopolypropylene (thickness 40 μm) / block polypropylene (thickness 5 μm) are laminated in sequence as the substrate. The heat of fusion, melting peak temperature and melt mass flow rate (MFR) of the first polyolefin layer, the second polyolefin layer and the substrate are shown in Tables 1 to 3. These physical property values are values adjusted according to the composition of each resin (ratio of polyethylene components, etc.), molecular weight, etc.
[0192] Example 12
[0193] In addition to extruding maleic anhydride modified polypropylene (PPa) on one side of the substrate (thickness 50μm, CPP, homopolypropylene) by a T-die extruder to form a first polypropylene layer (thickness 100μm); and extruding polypropylene (PP) on the other side of the substrate by a T-die extruder to form a second polypropylene layer (thickness 50μm), to obtain an adhesive film for metal terminals in which the first polyolefin layer (PPa layer) / substrate (CPP layer) / second polyolefin layer (PP layer) are sequentially laminated, the same method as in Example 1 is used to obtain an adhesive film for metal terminals in which the first polyolefin layer (PPa layer, thickness 100μm) / substrate (CPP layer, thickness 50μm) / second polyolefin layer (PP layer, thickness 50μm) are sequentially laminated. The heat of fusion, melting peak temperature and melt mass flow rate (MFR) of the first polyolefin layer, the second polyolefin layer and the substrate are shown in Tables 1 to 3. These physical property values are values adjusted according to the composition of each resin (ratio of polyethylene components, etc.), molecular weight, etc.
[0194] Comparative Example 1
[0195] As the polyolefin forming the first polyolefin layer, maleic anhydride modified polypropylene (PPa) was prepared; as the polyolefin forming the second polyolefin layer, polypropylene (PP) was prepared; as the polyolefin layer forming the substrate, a polypropylene film (PP) colored black with carbon black was prepared. Without using a substrate, maleic anhydride modified polypropylene (PPa) and polypropylene (PP) were co-extruded to obtain an adhesive film for metal terminals in which the first polyolefin layer (PPa layer, thickness 70μm) / substrate (PP layer, thickness 50μm) / second polyolefin layer (PP layer, thickness 30μm) were stacked in sequence. The heat of fusion, melting peak temperature and melt mass flow rate (MFR) of the first polyolefin layer, the second polyolefin layer and the substrate are shown in Tables 1 to 3, respectively. These physical property values are values adjusted according to the composition of each resin (ratio of polyethylene components, etc.), molecular weight, etc.
[0196] Comparative Example 2
[0197] As the polyolefin forming the first polyolefin layer, maleic anhydride-modified polypropylene (PPa) was prepared; as the polyolefin forming the second polyolefin layer, maleic anhydride-modified polypropylene (PPa) was prepared; as the substrate, a polypropylene film (PP, homopolypropylene) was prepared. Using each layer of resin, multi-layer air-cooling expansion molding was carried out to obtain an adhesive film for metal terminals in which the first polyolefin layer (PPa layer, thickness 35μm) / substrate (PP layer, thickness 80μm) / second polyolefin layer (PPa layer, thickness 35μm) were stacked in sequence. The heat of fusion, melting peak temperature and melt mass flow rate (MFR) of the first polyolefin layer, the second polyolefin layer and the substrate are shown in Tables 1 to 3, respectively. These physical property values are values adjusted according to the composition of each resin (ratio of polyethylene components, etc.), molecular weight, etc.
[0198] <Measurement of Heat of Fusion>
[0199] The first polyolefin layer, the second polyolefin layer and the heat-fusible resin layer of the outer packaging material are obtained from the adhesive film for metal terminals to prepare a measurement sample. The heat of fusion of the substrate is obtained by measuring the heat of fusion of the first polyolefin layer, the second polyolefin layer and the adhesive film for metal terminals, and subtracting the heat of fusion of the first polyolefin layer and the second polyolefin layer from the measured heat of fusion of the adhesive film for metal terminals to obtain the heat of fusion of the substrate. According to the provisions of JIS K 7122: 2012, the heat of fusion ΔH1, ΔH2, ΔH3 and ΔH4 of each measurement sample are measured. The measurement is performed using a differential scanning calorimeter (DSC, such as a differential scanning calorimeter Q200 manufactured by TA Instruments). After the measurement sample is kept at a temperature of -50°C for 15 minutes, the temperature is increased from -50°C to 210°C at a heating rate of 10°C / min, and the first heat of fusion ΔH (J / g) is measured, and then the temperature is kept at 210°C for 10 minutes. Then, cool down from 210°C to -50°C at a cooling rate of 10°C / min and maintain for 15 minutes. Then, increase the temperature from -50°C to 210°C at a heating rate of 10°C / min, and measure the heat of fusion ΔH (J / g) for the second time. It should be noted that the nitrogen flow rate is set to 50ml / min. According to the above steps, the value of the heat of fusion ΔH (J / g) measured for the first time is adopted. The heat of fusion is the area enclosed by the baseline (the line formed by connecting the starting point and end point of the ridge line from the base to the base) and the peak in the DSC curve. For reference, the DSC curve obtained in Example 1 is shown in Fig.11 .exist Fig.11 The baseline is indicated by a dotted line.
[0200] <Measurement of Melting Peak Temperature>
[0201] The first polyolefin layer, the second polyolefin layer and the substrate are obtained from the adhesive film for the metal terminal to prepare a measurement sample. For each measurement sample, the melting peak temperatures mp1, mp2 and mp3 are measured according to the provisions of JIS K 7121:2012 (Method for measuring the glass transition temperature of plastics (JIS K7121:1987 Supplementary Standard 1)). The measurement is performed using a differential scanning calorimeter (DSC, such as the differential scanning calorimeter Q200 manufactured by TA Instruments). After the measurement sample is kept at a temperature of -50°C for 15 minutes, the temperature is increased from -50°C to 210°C at a heating rate of 10°C / min, and after the first melting peak temperature P (°C) is measured, it is kept at a temperature of 210°C for 10 minutes. Then, the temperature is reduced from 210°C to -50°C at a cooling rate of 10°C / min and kept for 15 minutes. Then, the temperature is raised from -50°C to 210°C at a heating rate of 10°C / min, and the second melting peak temperature Q(°C) is measured. It should be noted that the nitrogen flow rate is set to 50 ml / min. According to the above steps, the first measured melting peak temperature P(°C) and the second measured melting peak temperature Q(°C) are obtained, and the first measured melting peak temperature P is used as the melting peak temperature.
[0202] <Measurement of Melt Mass Flow Rate (MFR)>
[0203] Resins constituting the first polyolefin layer, the second polyolefin layer, and the substrate used in the manufacture of the adhesive film for metal terminals were prepared into measurement samples. The melt mass flow rate (g / 10 min) of each measurement sample was measured using a melt indexer at a measurement temperature of 230°C and an applied weight of 2.16 kg according to the method A specified in JIS K7210:2014.
[0204] <Measurement of Adhesion Strength between Adhesive Film for Metal Terminal and Thermally Fusible Resin Layer>
[0205] (Production of outer packaging materials)
[0206] First, an outer packaging material for a storage device (hereinafter referred to as "outer packaging material") was prepared according to the following steps. A substrate layer (30 μm thick) composed of a polyethylene terephthalate film (12 μm thick) / adhesive layer (3 μm thick) / nylon film (15 μm thick) was laminated on an aluminum alloy foil (40 μm thick) by dry lamination, and a heat-melting resin layer was laminated on the other side surface by coextrusion. Specifically, a two-component polyurethane adhesive (polyol compound and aromatic isocyanate compound) was applied to the nylon film to form an adhesive layer (3 μm thick) on the nylon film. Then, the adhesive layer and the polyethylene terephthalate film were laminated on the nylon film to form a substrate layer. Next, a two-component polyurethane adhesive (polyol compound and aromatic isocyanate compound) was applied to one side surface of the barrier layer made of aluminum alloy foil to form an adhesive layer (3 μm thick) on the aluminum alloy foil. Then, after laminating an adhesive layer and a substrate layer with the nylon film side as the adhesive surface on the aluminum alloy foil, an aging treatment was performed to prepare a laminate of substrate layer / adhesive layer / barrier layer. Next, on the barrier layer of the laminate, an adhesive layer (thickness 40 μm, arranged on the metal layer side) formed by maleic anhydride modified polypropylene resin and a heat-melting resin layer (thickness 40 μm, innermost layer) formed by random polypropylene resin were co-extruded, and an adhesive layer / heat-melting resin layer was laminated on the barrier layer. Then, the obtained laminate was heated at a temperature of 190°C for 2 minutes to obtain an outer packaging material for a storage device in which a substrate layer, an adhesive layer, a barrier layer, an adhesive layer, and a heat-melting resin layer were laminated in sequence. The heat of fusion ΔH4, the melting peak temperature mp4, and the melt mass flow rate (MFR) T4 of the heat-melting resin layer are shown in Tables 1 to 3, respectively. The measurement methods of these parameters are the same as those for the adhesive film for metal terminals, except that the heat-fusible resin layer is used as the measurement sample.
[0207] (Evaluation of heat sealing for 3 seconds)
[0208] As a metal terminal, an aluminum foil (JIS H4160: 1994A8079H-O) with a MD of 40 mm, a TD of 22.5 mm, and a thickness of 400 μm was prepared. In addition, each adhesive film obtained in the examples and comparative examples was cut into a length (MD) of 45 mm and a width (TD) of 20 mm. Figure 8As shown, a metal terminal is clamped between two adhesive films to obtain a laminate of adhesive film / metal terminal / adhesive film. In this case, the lamination is achieved in such a way that the MD and TD of the metal terminal are respectively consistent with the length direction (MD) and width direction (TD) of the adhesive film, and the center of the metal terminal and the adhesive film are consistent. Then, in a state where the laminate is clamped by two tetrafluoroethylene-ethylene copolymer films (ETFE films, thickness 100μm), it is placed on a heating plate heated to 190°C, and a 500g weight with a sponge is placed on it. After standing for 12 seconds, the adhesive film is heat-fused to the metal terminal to make a metal terminal with an adhesive film. At this time, as Figure 8 As shown in FIG. 1 , the metal terminal is sandwiched between the adhesive films so that the periphery of the metal terminal is covered by the adhesive film and a portion where the two adhesive films are heat-fused to each other is formed. Next, the outer packaging material is cut into a size of TD60mm and MD 200mm, as shown in FIG. Fig. 9 As shown in the figure, the outer packaging material is folded in half so that the length of MD becomes half of 100 mm, and the heat-fusible resin layers are on the inside and facing each other, and the resulting laminate is sandwiched between the facing heat-fusible resin layers. At this time, the laminate is laminated so that the MD and TD of the outer packaging material are respectively consistent with the width direction (TD) and the length direction (MD) of the laminate. In this state, a heat seal tester is used to measure the width of the laminate at 7 mm ( Fig. 9 Heat seal was performed under the conditions of (7 mm in the y-axis direction of (b)), 190°C, surface pressure 1.0 MPa, and time 3 seconds (reference Fig. 9 The outer packaging material and the adhesive film were heat-fused to obtain a laminate (see FIG. Fig. 9 (b) Schematic diagram of the process).
[0209] Then, the TD center portion of the obtained laminated outer packaging material was cut into a width of 15 mm (see the cutting position for reference). Fig. 9 (b) Double dashed line). Next, the outer packaging material and the metal terminal were clamped together at 25°C using a TENSILON universal material testing machine (RTG-1210 manufactured by A&D Co., Ltd.) and Fig. 9 (b) The adhesive film and the heat-fusible resin layer of the outer packaging material are peeled off in the y direction. The maximum strength during peeling is taken as the peel strength of the outer packaging material (N / 15mm). The peeling speed is 300mm / min, the peeling angle is 180°, the chuck spacing is 30mm, and the average value of 3 measurements is taken.
[0210] A: Peel strength is above 120N / 15mm.
[0211] B: The peel strength is 100 N / 15 mm or more and less than 120 N / 15 mm.
[0212] C: The ratio of the peel strength to the reference peel strength is less than 100 N / 15 mm.
[0213] (Evaluation of the adhesion of short-time (1 second) heat seal)
[0214] The adhesive film and the heat-fusible resin layer of the outer packaging material were peeled off in the same manner as above, and the peel strength was measured, except that the heat sealing conditions using the heat seal tester in the above (adhesion after heat sealing for 3 seconds) were changed to shorter conditions of 190°C, surface pressure of 1.0 MPa, and time of 1 second.
[0215] A: Peel strength is above 100N / 15mm.
[0216] B: The peel strength is greater than or equal to 80 N / 15 mm and less than or equal to 100 N / 15 mm.
[0217] C: The ratio of the peel strength to the reference peel strength is less than 80 N / 15 mm.
[0218] <Follow-up evaluation>
[0219] Ten laminates of the outer packaging material and the adhesive film obtained in the above (Evaluation of Adhesion after Short-time (1 Second) Heat Sealing) were prepared (refer to Fig.10 ), as a sample. Fig.10 In the state where the y1 side of the schematic diagram is the upper side and the y2 side is the lower side, the heat-fusible resin layers of each sample facing each other are opened, and the heat-fusible resin layers are opened from the upper side (y1 side) toward the heat-fusible position of the adhesive film, that is, the two ends of the metal terminals exposed ( Fig.10 A highly permeable dyeing liquid (Microcheck, manufactured by Taiho Kozai Co., Ltd.) was sprayed on the adhesive film and the outer packaging material (indicated by the arrows at both ends of the x-axis direction) to confirm the penetration of the dyeing liquid into the gap between the adhesive film and the outer packaging material, and the followability of the adhesive film of the outer packaging material caused by heat sealing was evaluated. The evaluation was performed based on the number of samples in which the dyeing solution penetrated into the gap between the adhesive film and the outer packaging material. Fig.10 The dye solution permeated from the upper side (y1 side) to the lower side (y2 side) of the adhesive film. The sample in which the permeated solution exceeded the heat-sealed portion S and reached the lower side (y2 side) was evaluated as a sample in which the dye solution permeated into the gap. The dye solution permeation state was confirmed at a position 1 mm outside the adhesive film of each sample (refer to Fig.10 The sample was cut at the position of the double dotted line in the figure and the cross section was observed. The evaluation criteria are as follows. The results are shown in Table 4.
[0220] A: Among the 10 samples, the penetration of the dye solution into the gap was 0.
[0221] B: Among the 10 samples, the dye solution penetrated into the gaps in 1 or more and 2 or less samples.
[0222] C: The dye solution penetrated into the gaps in 3 or more of the 10 samples.
[0223] <Collapse Evaluation>
[0224] The laminate of the outer packaging material and the adhesive film obtained in the above (Evaluation of Adhesion after Short-time (1 Second) Heat Sealing) was used as a sample, and the laminate was cut along the thickness direction at the center of the heat-sealed part of the adhesive film ( Fig. 9 (b) The thickness of the adhesive film was measured by cutting along the y-axis and thickness direction at the center of the laminate in the x-axis direction. The thickness of the adhesive film before heat sealing was 100%, and the collapse evaluation was performed according to the following standards based on the thickness ratio after heat sealing. The thickness was taken as the average thickness of the two adhesive films located above and below the metal terminal. The results are shown in Table 4.
[0225] A: The thickness of the adhesive film after heat sealing is at least 95% of the thickness before heat sealing.
[0226] B: The thickness of the adhesive film after heat sealing is at least 80% and less than 95% of the thickness before heat sealing.
[0227] C: The thickness of the adhesive film after heat sealing is less than 80% of the thickness before heat sealing.
[0228] <Film-forming property evaluation>
[0229] The film-forming property of the first polyolefin layer in the above-mentioned <Manufacture of an adhesive film for metal terminals> was evaluated. Specifically, the unevenness in the width direction (TD) during the film-forming process of the first polyolefin layer was evaluated. The unevenness in the width direction was the thickness of the first polyolefin layer measured at intervals of 5 mm along the width direction, and was evaluated according to the following standard based on 2σ. The results are shown in Table 4.
[0230] A: 2σ of unevenness in width direction is less than 2.5
[0231] B: 2σ of unevenness in the width direction is 2.5 to 3.0
[0232] C: 2σ of unevenness in the width direction exceeds 3.0 [Table 1]
[0233]
[0234] [Table 2]
[0235]
[0236] [Table 3]
[0237]
[0238] [Table 4]
[0239]
[0240] As described above, the present invention provides the following aspects of the invention.
[0241] Item 1: An adhesive film for a metal terminal, wherein the adhesive film for a metal terminal is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device encapsulating the electric storage device element,
[0242] The adhesive film for metal terminals is composed of a laminate having in this order a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer packaging material side of the power storage device.
[0243] The heat of fusion ΔH1 of the first polyolefin layer and the heat of fusion ΔH2 of the second polyolefin layer measured in accordance with the provisions of JIS K 7122:2012 satisfy the relationship ΔH1>ΔH2.
[0244] The heat of fusion ΔH3 of the substrate measured in accordance with the provisions of JIS K 7122:2012 is 70 J / g or more.
[0245] Item 2: The adhesive film for metal terminal according to Item 1, wherein the heat of fusion ΔH1 of the first polyolefin layer, the heat of fusion ΔH2 of the second polyolefin layer, and the heat of fusion ΔH3 of the substrate satisfy the relationship ΔH3 ≥ ΔH1 > ΔH2.
[0246] Item 3: The adhesive film for metal terminal according to Item 1 or 2, wherein the heat of fusion ΔH2 of the second polyolefin layer is 20 J / g or more and 70 J / g or less.
[0247] Item 4: The adhesive film for a metal terminal according to any one of Items 1 to 3, wherein the heat of fusion ΔH1 of the first polyolefin layer is 30 J / g or more and 80 J / g or less.
[0248] Item 5: An adhesive film for metal terminals according to any one of Items 1 to 4 above, wherein the melting peak temperature mp1 of the first polyolefin layer, the melting peak temperature mp2 of the second polyolefin layer and the melting peak temperature mp3 of the substrate measured in accordance with the provisions of JIS K7121:2012 satisfy the relationship mp3≥mp1>mp2.
[0249] Item 6: An adhesive film for metal terminals according to any one of Items 1 to 5 above, wherein the melt mass flow rate T1 of the first polyolefin layer, the melt mass flow rate T2 of the second polyolefin layer and the melt mass flow rate T3 of the substrate at 230°C satisfy the relationship T2>T1>T3.
[0250] Item 7: The adhesive film for metal terminal according to any one of Items 1 to 6, wherein the substrate contains a polyolefin skeleton.
[0251] Item 8: The adhesive film for a metal terminal according to any one of Items 1 to 7, wherein the thickness of each of the first polyolefin layer and the second polyolefin layer is 60 μm or less.
[0252] Item 9: The adhesive film for a metal terminal according to any one of Items 1 to 8, wherein the thickness of the substrate is 120 μm or less.
[0253] Item 10: The adhesive film for metal terminal according to any one of Items 1 to 9, wherein the thickness of the adhesive film for metal terminal is 220 μm or less.
[0254] Item 11: A method for producing an adhesive film for a metal terminal, wherein the adhesive film for a metal terminal is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device encapsulating the electric storage device element,
[0255] The adhesive film for metal terminals is composed of a laminate having in this order a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer packaging material side of the power storage device.
[0256] The method comprises the steps of obtaining a laminate having the first polyolefin layer, the substrate and the second polyolefin layer in this order,
[0257] The heat of fusion ΔH1 of the first polyolefin layer and the heat of fusion ΔH2 of the second polyolefin layer measured in accordance with the provisions of JIS K 7122:2012 satisfy the relationship ΔH1>ΔH2.
[0258] The heat of fusion ΔH3 of the substrate measured in accordance with the provisions of JIS K 7122:2012 is 70 J / g or more.
[0259] Item 12: A metal terminal with an adhesive film for a metal terminal, wherein the adhesive film for a metal terminal according to any one of Items 1 to 10 is attached to the metal terminal.
[0260] Item 13: An electric storage device, comprising: the electric storage device element having at least a positive electrode, a negative electrode and an electrolyte; the electric storage device outer packaging material for packaging the electric storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and protruding to the outside of the electric storage device outer packaging material,
[0261] The adhesive film for metal terminal according to any one of items 1 to 10 is interposed between the metal terminal and the outer packaging material for the electric storage device.
[0262] Item 14: A method for manufacturing an electric storage device, wherein the electric storage device comprises: the electric storage device element having at least a positive electrode, a negative electrode and an electrolyte; the electric storage device outer packaging material for packaging the electric storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and protruding to the outside of the electric storage device outer packaging material,
[0263] The method includes the steps of sandwiching the adhesive film for metal terminal described in any one of items 1 to 10 between the metal terminal and the outer packaging material for the electric storage device, and sealing the electric storage device element with the outer packaging material for the electric storage device.
Claims
1. An adhesive film for a metal terminal, wherein: The adhesive film for metal terminals is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element. The adhesive film for metal terminals is composed of a laminate having a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer packaging material side of the power storage device in this order. The ratio of the thickness of the substrate to the total thickness of the first polyolefin layer and the second polyolefin layer is 0.3 or more, The heat of fusion ΔH1 of the first polyolefin layer and the heat of fusion ΔH2 of the second polyolefin layer measured according to the provisions of JIS K 7122:2012 satisfy the relationship of ΔH1>ΔH2. The heat of fusion ΔH3 of the substrate measured in accordance with the provisions of JIS K 7122:2012 is 70 J / g or more.
2. An adhesive film for a metal terminal, wherein: The adhesive film for metal terminals is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element. The adhesive film for metal terminals is composed of a laminate having a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer packaging material side of the power storage device in this order. The heat of fusion ΔH1 of the first polyolefin layer and the heat of fusion ΔH2 of the second polyolefin layer measured according to the provisions of JIS K 7122:2012 satisfy the relationship of ΔH1>ΔH2. The heat of fusion ΔH3 of the substrate measured according to JIS K 7122:2012 is 70 J / g or more, The outer packaging material for an electric storage device is composed of a laminate having at least a base layer, a barrier layer and a heat-fusible resin layer in this order. An absolute value of a difference between a heat of fusion ΔH4 of the heat-adhesive resin layer of the electricity storage device packaging material and a heat of fusion ΔH2 of the second polyolefin layer of the adhesive film for metal terminal is 0.0 to 5.0 J / g.
3. The adhesive film for metal terminals according to claim 1 or 2, wherein The heat of fusion ΔH1 of the first polyolefin layer, the heat of fusion ΔH2 of the second polyolefin layer, and the heat of fusion ΔH3 of the substrate satisfy the relationship ΔH3 ≥ ΔH1 > ΔH2.
4. The adhesive film for metal terminal according to any one of claims 1 to 3, wherein The heat of fusion ΔH2 of the second polyolefin layer is greater than or equal to 20 J / g and less than or equal to 70 J / g.
5. The adhesive film for a metal terminal according to any one of claims 1 to 4, wherein The first polyolefin layer has a heat of fusion ΔH1 of not less than 30 J / g and not more than 80 J / g.
6. The adhesive film for metal terminal according to any one of claims 1 to 5, wherein The melting peak temperature mp1 of the first polyolefin layer, the melting peak temperature mp2 of the second polyolefin layer, and the melting peak temperature mp3 of the substrate measured in accordance with JIS K 7121:2012 satisfy the relationship mp3≥mp1>mp2.
7. The adhesive film for a metal terminal according to any one of claims 1 to 6, wherein The melt mass flow rate T1 of the first polyolefin layer, the melt mass flow rate T2 of the second polyolefin layer, and the melt mass flow rate T3 of the substrate at 230° C. satisfy the relationship of T2>T1>T3.
8. The adhesive film for a metal terminal according to any one of claims 1 to 7, wherein The substrate comprises a polyolefin backbone.
9. The adhesive film for a metal terminal according to any one of claims 1 to 8, wherein The thickness of the first polyolefin layer and the second polyolefin layer is respectively 60 μm or less.
10. The adhesive film for a metal terminal according to any one of claims 1 to 9, wherein The thickness of the substrate is less than 120 μm.
11. The adhesive film for a metal terminal according to any one of claims 1 to 10, wherein The adhesive film for metal terminals has a thickness of 220 μm or less.
12. The adhesive film for a metal terminal according to any one of claims 1 to 11, wherein The thickness of the substrate is above 60 μm.
13. The adhesive film for a metal terminal according to any one of claims 1 to 12, wherein The adhesive film for metal terminals has a thickness of 160 μm or more.
14. A method for producing an adhesive film for a metal terminal, wherein: The adhesive film for metal terminals is located between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element. The adhesive film for metal terminals is composed of a laminate having a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer packaging material side of the power storage device in this order. The ratio of the thickness of the substrate to the total thickness of the first polyolefin layer and the second polyolefin layer is 0.3 or more, The method comprises the steps of obtaining a laminate having the first polyolefin layer, the substrate and the second polyolefin layer in this order, The heat of fusion ΔH1 of the first polyolefin layer and the heat of fusion ΔH2 of the second polyolefin layer measured according to the provisions of JIS K 7122:2012 satisfy the relationship of ΔH1>ΔH2. The heat of fusion ΔH3 of the substrate measured in accordance with the provisions of JIS K 7122:2012 is 70 J / g or more.
15. A metal terminal with an adhesive film for a metal terminal, wherein: The adhesive film for a metal terminal according to any one of claims 1 to 13 is mounted on a metal terminal.
16. An electric storage device, comprising: The power storage device element has at least a positive electrode, a negative electrode and an electrolyte; The outer packaging material for the power storage device for packaging the power storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode respectively and protruding to the outside of the outer packaging material for the power storage device, The adhesive film for metal terminal according to any one of claims 1 to 13 is interposed between the metal terminal and the outer packaging material for the electric storage device.
17. A method for manufacturing an electric storage device, wherein: The electric storage device comprises: the electric storage device element having at least a positive electrode, a negative electrode and an electrolyte; the outer packaging material for the electric storage device that packages the electric storage device element; and the metal terminals that are electrically connected to the positive electrode and the negative electrode, respectively, and protrude to the outside of the outer packaging material for the electric storage device. The method comprises the steps of sandwiching the adhesive film for metal terminal according to any one of claims 1 to 13 between the metal terminal and the outer packaging material for the electric storage device, and sealing the electric storage device element with the outer packaging material for the electric storage device.
Citation Information
Patent Citations
Terminal with adhesive tape, method of manufacturing terminal with adhesive tape, and thin battery
JP2015079638A
Polyamic acid composition and polyimide, and metal-clad laminate and its manufacturing method
JP2021008551A