Tin-doped high-power-density silver-antimony-tellurium thermoelectric material, preparation method and application thereof

By doping tin into the silver antimony tellurium material, impurity bands are formed and the formation of n-type Ag2Te is suppressed, the problems of material instability and low power factor are solved, and the thermoelectric performance with high power density and high efficiency energy conversion efficiency is achieved.

CN118922048APending Publication Date: 2024-11-08INST OF WENZHOU ZHEJIANG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410992695.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing silver antimony tellurium thermoelectric materials have low power factor (PF) in the medium temperature range, which limits the power density of thermoelectric devices, and the instability of the material leads to high thermal conductivity, affecting thermoelectric performance.

Method used

By doping trace tin (Sn) into the silver antimony tellurium material, an impurity band is introduced at the top of the valence band to inhibit the formation of n-type Ag2Te, improve electron transport performance, and prepare high-power density AgSb1-xSnxTe2 material through SPS sintering technology.

Benefits of technology

It significantly improves the power factor of thermoelectric materials to reach 27μWcm-1K-2 and the thermoelectric superiority (zT) to 2.5, achieving energy conversion efficiency up to 12.1% and power density of 1.13W/cm2, enhancing the stability and thermoelectricity of the material. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922048A_ABST
    Figure CN118922048A_ABST
Patent Text Reader

Abstract

The invention discloses a tin-doped high-power-density silver-antimony-tellurium thermoelectric material, which is characterized in that AgSbTe2 is used as a matrix, an AgSbTe2 material is modified through hole doping of Sn, an impurity band is introduced to the top of a valence band of the AgSbTe2 material, and the chemical structural formula of the obtained product is AgSb1-xSnxTe2, 0 < x < = 0.1. The AgSbTe2 material is modified through hole doping of Sn, an impurity band is introduced to the top of a valence band of the AgSbTe2 material, the electrical transport performance is remarkably improved, a thermoelectric power factor as high as 27 mu Wcm <-1 > K <-2 > is successfully realized, which is the highest record of the material at present, the thermoelectric figure of merit (zT) reaches 2.5 at 673K, the excellent performance is attributed to the formation of a new impurity band, and the performance of the AgSbTe2 material is greatly improved. And a reduction in the formation energy of the defective complex # imgabs0 #. According to the invention, bipolar diffusion of minority carriers is inhibited and formation of an n-type Ag2Te impurity phase is prevented, so that the stability and Seebeck coefficient of the doped material are significantly improved. According to the invention, the Sn-doped AgSbTe2 material is utilized to manufacture a thermoelectric device, the energy conversion efficiency up to 12.1% and the power density of 1.13 W / cm < 2 > are realized, and important theoretical basis and practical application value are provided for realizing the application of p-type AgSbTe2 in the field of medium-temperature thermoelectricity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermoelectric materials, and in particular to a tin-doped high-power-density silver-antimony-tellurium thermoelectric material, a preparation method and application thereof. Background Art

[0002] Thermoelectric (TE) devices not only provide a simple solution for waste heat power generation, but also can achieve precise temperature control and refrigeration functions. Thermoelectric products have been widely used in consumer electronics, communications, medical and automotive fields. The performance of thermoelectric materials is usually characterized by the dimensionless figure of merit zT = (S2σ / κ)T; where T is the absolute temperature, S is the Seebeck coefficient, σ is the electrical conductivity, and κ is the thermal conductivity.

[0003] There are two main ways to optimize the performance of thermoelectric materials: reducing the lattice thermal conductivity (κL) and improving the thermoelectric power factor (PF). These properties are interconnected through the charge carriers within the material, and optimizing one parameter will inevitably affect the other.

[0004] Silver antimony telluride (AgSbTe2) is a promising p-type thermoelectric material, especially for applications in the medium temperature range (200-400°C). Due to its spontaneously formed micro / nanostructure and asymmetry, this material has low thermal conductivity. In addition, AgSbTe2 also exhibits a high Seebeck coefficient, which is caused by its flat band structure with high degeneracy.

[0005] Doping has been widely used to tune the band structure of AgSbTe2 and optimize its carrier concentration, thereby improving thermoelectric performance. For example, it has been reported that heavy doping with Se / S effectively increases the hole concentration and significantly improves the thermoelectric power factor by promoting multiple valence bands to participate in charge transport. Other studies have reported that zT can be significantly increased to 2.6 by doping with elements such as Cd, Hg, Yb or Ag vacancies to enhance the cation order to form a nanoscale superstructure. This enhancement is mainly due to the significant reduction in thermal conductivity to 0.2 W m -1 K -1 Nevertheless, the PF achieved by these works is still below 20 μW cm -1 K -2 , which is significantly lower than that of commercial thermoelectric materials. Although the thermoelectric figure of merit is crucial to improving device conversion efficiency, the relatively low PF continues to limit the overall power density of AgSbTe2 thermoelectric devices. Therefore, it is quite necessary to simultaneously improve zT and PF for its practical application.

[0006] AgSbTe2 is a p-type thermoelectric (TE) material suitable for medium temperature range. Past research has focused on improving its thermoelectric performance by reducing the lattice thermal conductivity (κL) by forming ordered nanostructured domains. However, the low power factor (PF) limits the improvement of the power density of AgSbTe2 thermoelectric devices. Summary of the invention

[0007] The purpose of the present invention is to provide a tin-doped high-power density silver antimony telluride thermoelectric material, a preparation method and its application, using Sn as a dopant to enhance the electron transport performance of p-type AgSbTe2, significantly enhancing the stability of AgSbTe2 through Sn doping, effectively inhibiting the formation of n-type Ag2Te, and introducing an impurity band at the top of the valence band (VBM), significantly improving the PF and zT values ​​of the thermoelectric material.

[0008] The present invention provides a tin-doped high power density silver antimony tellurium thermoelectric material, which takes AgSbTe2 as a matrix, modifies the AgSbTe2 material by hole doping Sn, introduces an impurity band at the top of its valence band, and the chemical structure of the obtained product is AgSb 1- x Sn x Te2; 0<x≤0.1.

[0009] In a preferred embodiment, the AgSbTe2 material has a face-centered cubic (fcc) crystal structure, in which the Ag and Sb ions are randomly distributed at the cation sites in the lattice, while Te occupies the anion sites.

[0010] The present invention also provides a method for preparing a tin-doped high power density silver antimony tellurium thermoelectric material, comprising the following steps:

[0011] S1. Weigh the raw materials according to the stoichiometric ratio, place the mixed powder of silver, antimony, tellurium and tin in a reactor, slowly heat it to a set temperature under vacuum conditions, keep it warm for a predetermined time, and then slowly cool it to room temperature to obtain a bulk ingot;

[0012] S2. The obtained block ingot is crushed into powder and sintered by SPS to obtain a cylinder, namely AgSb 1-x Sn x Te2 material.

[0013] In step S1, the quartz tube is heated from room temperature to 1173-1373K under vacuum conditions, kept at 1173-1373K for 3-10 hours, and finally slowly cooled to room temperature. The cooling process lasts for 6-24 hours to obtain a bulk ingot.

[0014] In step S2, spark sintering (SPS) is performed by applying a pressure of 20 to 60 MPa at 623 to 773 K for 1 to 5 minutes and resolidifying to obtain AgSb1-x Sn x Te2 material.

[0015] Furthermore, the relative density of the obtained cylinder is higher than 95% of the theoretical value.

[0016] The present invention also provides a thermoelectric device module, wherein the P-type leg of the module adopts the AgSb 0.94 Sn 0.06 Te2 material, N-type legs use Yb 0.25 Co 3.75 Fe 0.25 Sb 12 Skutterudite material.

[0017] Pure AgSbTe2 is thermodynamically unstable at temperatures below 633K and decomposes into Ag2Te and Sb2Te3 phases; since Ag2Te is an n-type semiconductor that undergoes a structural phase transition at about 425K, even a small amount of Ag2Te can adversely affect the electrical transport properties of p-type AgSbTe2. Therefore, suppressing the formation of Ag2Te impurities is crucial to optimizing the thermoelectric properties of AgSbTe2. Crystal orbital analysis shows that the instability of AgSbTe2 comes from the antibonding states present within the Fermi level. Due to the strong hybridization of Sb-5s and Te-5p states, this causes the Te-5p antibonding state to migrate to the valence band boundary. From the perspective of electronic structure, the contribution of this antibonding state occupies the main component at the top of the valence band, resulting in intrinsic instability. Therefore, AgSbTe2 spontaneously decomposes into Ag2Te and Sb2Te3 phases. To address this issue, p-type doping is used as an effective strategy to mitigate the impact of these antibonding states and enhance the stability of the AgSbTe2 system. To this end, the present invention stabilizes the AgSbTe2 matrix by doping a trace amount of Sn into the lattice. 2+ Preferentially replace Sb 3+ , because it has one less valence electron, which helps to generate additional holes and bring the system to the optimal carrier concentration.

[0018] Compared with the prior art, the present invention has at least the following advantages:

[0019] (1) The present invention is a tin-doped high-power density silver antimony telluride thermoelectric material. The AgSbTe2 material is modified by hole doping with Sn, and an impurity band is introduced at the top of its valence band, which significantly improves the electrical transport performance and successfully achieves 27μWcm -1 K -2 The power factor is the highest record for this material, and the thermoelectric figure of merit (zT) reaches 2.5 at 673K. This excellent performance is attributed to the formation of new impurity bands and defect complexes. Reduction of formation energy.

[0020] (2) The present invention discloses a tin-doped high-power density silver antimony telluride thermoelectric material. By doping Sn into AgSbTe2, the bipolar diffusion of minority carriers is suppressed and the formation of n-type Ag2Te impurity phase is prevented. The lattice thermal conductivity of the thermoelectric material is minimized to 0.41 W / mK, and the Seebeck coefficient of the thermoelectric material is significantly improved.

[0021] (3) The present invention uses Sn-doped AgSbTe2 materials to manufacture thermoelectric devices, achieving an energy conversion efficiency of up to 12.1% and a 2 The power density provides an important theoretical basis and practical application value for the application of p-type AgSbTe2 in the field of medium-temperature thermoelectricity. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the phase diagram of pure AgSbTe2 material in Example 1.

[0023] Figure 2 Schematic diagram of the improvement of TE performance of Sn-doped AgSbTe2.

[0024] Figure 3 AgSbTe2 material, AgSb 1-x Sn x XRD pattern of Te2 material.

[0025] Figure 4 AgSbTe2 material, AgSb 1-x Sn x DSC curve of Te2 material.

[0026] Figure 5 The AgSb synthesized in Example 2 0.94 Sn 0.06 XPS spectrum of Te2 material.

[0027] Figure 6 (a) Ag calculated by DFT 16 Sb 16 Te 32 and (b) Ag 16 Sb 15 SNT 32 The band structure of .

[0028] Figure 7 Defect formation energy of single defect and complex defect relative to Fermi level: (c) Ag 16 Sb 16 Te 32 and (d) Ag 16 Sb 15 SNT 32 .

[0029] Figure 8 is the partial density of states (DOS) of Ag, Sb and Te atoms: (e) Ag 16 Sb 16 Te 32 and (f)Ag 16 Sb 15 SNT 32 Zero energy corresponds to the Fermi level.

[0030] Fig. 9 Undoped AgSbTe2 and doped AgSb 0.94 Sn 0.06 The carrier concentration and mobility of Te2 material vary with temperature.

[0031] Fig.10 For (a) from AgSb 0.94 Sn 0.06 Atomic resolution HAADF-STEM image of Te2 sample and its corresponding FFT image, double diffraction spots circled in red and green; (b) Inverse composite and individual FFT images of the diffraction spots circled in red and green in panel a; (c) Schematic illustration of the short-range order of Ag / Sb induced by Sn doping; (d) Visualization of the AgSb in the direction of its

[211] crystal axis. 0.94 Sn 0.06 HRTEM micrograph of Te2 grains; (e) the corresponding selected area diffraction pattern; the HRTEM images of the red and green box areas in Figure d and the corresponding FFT images are (f) and (g), respectively.

[0032] Fig.11 Atomic-resolution HAADF-STEM micrograph and FFT pattern of an AgSbTe2 sample visualized along its

[111] /

[211] crystallographic axis.

[0033] Fig.12 AgSb 1-x Sn x Temperature dependence of thermoelectric properties of Te2: (a) conductivity, σ; (b) carrier concentration, n H ; (c) Mobility, μ H ; (d) Seebeck coefficient, S; (e) power factor, PF; (f) maximum PF compared with the state-of-the-art AgSbTe2 material; (g) thermal conductivity, κ; (h) ambipolar diffusion and lattice contribution to thermal conductivity; (i) thermoelectric figure of merit, zT.

[0034] Fig.13 AgSb 1-x Sn xTemperature dependence of thermoelectric properties of Te2: (a) Lorentz number, L; (b) electronic thermal conductivity, κ e (c) Subtract the electronic thermal conductivity from the total thermal conductivity, κ tot -κ e ; (d) Polycrystalline AgSb 1-x Sn x Bipolar thermal conductivity κ of Te2 samples bi Temperature variation graph.

[0035] Fig.14 For different batches of AgSb synthesized separately 0.94 Sn 0.06 Reproducibility of thermoelectric properties of Te2 samples; temperature-dependent TE properties include: (a) electrical conductivity, σ; (b) Seebeck coefficient, S; (c) total thermal conductivity, κ; (d) TE performance index, zT; the uncertainty of zT measurement is about ~20%.

[0036] Fig.15 AgSb 0.94 Sn 0.06 Reversibility of TE performance of Te2 during three heating-cooling cycles; temperature-dependent TE properties include: (a) electrical conductivity, σ; (b) Seebeck coefficient, S; (c) total thermal conductivity, κ; (d) TE performance index, zT; the uncertainty of zT measurement is about ∼20%.

[0037] Fig.16 Yb as the n-leg 0.25 Co 3.75 Fe 0.25 Sb 12 TE properties of skutterudite materials; temperature-dependent TE properties include: (a) electrical conductivity, σ; (b) Seebeck coefficient, S; (c) total thermal conductivity, κ; and (d) TE performance index, zT.

[0038] Fig.17 (a) Schematic diagram of thermoelectric device measurement; (b) Photograph of the fabricated device and power generation measurement setup.

[0039] Fig.18 The performance of the thermoelectric device: (a) internal resistance; (b) open circuit voltage, V oc ; (c) heat flow, Q out ; (d) Maximum output power P max as a function of ΔT.

[0040] Fig.19 (a) shows the p-type AgSb 0.94 Sn 0.06 Te2 and n-type skutterudite Yb 0.25 Co3.75 Fe 0.25 Sb 12 (a) shows the current dependence of the output power of the thermoelectric device; (b) shows the relationship between the maximum power density and ΔT; (c) shows the conversion efficiency (η) of the thermoelectric device; (d) compares the AgSb 0.94 Sn 0.06 The maximum conversion efficiency (η) of Te2 thermoelectric devices under different ΔT conditions max )Comparison of efficiency with other AgSbTe2 thermoelectric devices.

[0041] Fig. 20 AgSb made for (a) 0.94 Sn 0.06 Output power density of Te2 thermoelectric modules; (b) comparison with the power density of state-of-the-art AgSbTe2-based devices.

[0042] Fig.21 Comparison of zT with the latest TE materials in low, medium and high temperature regions. DETAILED DESCRIPTION

[0043] The specific implementation modes of the present invention will be described clearly and completely below with reference to the accompanying drawings.

[0044] The raw materials used in the implementation of the present invention are as follows:

[0045] Silver particles (Ag, 99.9%, Thermo Scientific), antimony particles (Sb, Alfa Aesar 99.9999%), tin powder (Sn, Sigma Aldrich 99.99%) and tellurium bulk (Te, Alfa Aesar 99.9%).

[0046] The test characterization method used in the implementation of the present invention is as follows:

[0047] Electrical conductivity σ and Seebeck coefficient S: (ULVAC-RIKO ZEM-3 system, Japan), using a rod-shaped sample of 2 mm×2 mm×12 mm.

[0048] Temperature Dependence of Thermal Diffusivity: Laser Flash System (LFA-467HT Germany).

[0049] Specific heat capacity: Differential scanning calorimeter (Netzsch DSC 214, Germany, heating / cooling rate of 15 K / min).

[0050] X-ray diffraction analysis was performed using a PANalytical Empyrean instrument under Cu-Kα radiation with a 2θ angle range of 10-60°.

[0051] Charge carrier concentration and mobility were characterized using a LakeShore Hall Effect System (8400 Series HMS, LakeShore) at 0.9 T magnetic field.

[0052] High resolution transmission electron microscopy (HRTEM) analysis was performed using a FEI Titan G2. TEM samples were prepared by focused ion beam (FIB). Microstructural morphology was determined using a field emission scanning electron microscope (FESEM, FEI Verios G4) operating at 5.0 kV. Energy dispersive X-ray analysis (EDX) was performed using an OxfordAztec spectrometer connected to a FEI Verios G4 SEM, operating at 20.0 kV, for measuring material composition.

[0053] X-ray Photoelectron Spectroscopy (XPS): A Physical Electronics VersaProbe III instrument was used, equipped with a monochromatic Al Kα x-ray source (hν=1,486.6 eV) and a concentric hemispherical analyzer.

[0054] Charge neutralization was performed using low energy electrons (<5 eV) and argon ions. The peak was calibrated to the CHx band at 284.8 eV in the carbon 1s spectrum. The measurement was performed at a sampling angle of 50° to the plane of the sample surface. Quantification was performed using the instrument relative sensitivity factor, taking into account the x-ray cross section and the inelastic mean free path of the electrons. The analysis area diameter was approximately ~200 μm.

[0055] Low-temperature Hall resistivity ρxy measurements were performed using a standard four-probe technique in a physical properties measurement system (PPMS, Quantum Design) over the temperature range from 5 K to 300 K and a magnetic field range of 9 T.

[0056] Total thermal conductivity κ total : By κ total =D×ρ×Cp, where D, ρ and Cp are thermal diffusivity, density and specific heat capacity, respectively; the density is measured using the Archimedean principle, and the thermal conductivity measurement error is estimated to be about ±4%.

[0057] Sb 1-x Sn x The electronic thermal conductivity (κe) of Te2 was calculated according to the Widmann-Franz law, κe=LσT, where L and σ are the Lorentz number and conductivity, respectively.

[0058] The Lorentz number is calculated based on the measured Seebeck coefficient: L = [1.5 + exp(-|S| / (116μVK -1 ))]10 -8 WΩK -2, proposed by GJ Snyder et al.; the results presented here are the average results of 3 pellets measured under the same conditions; the standard deviation of the measurements between different samples is less than 10%.

[0059] By xy =[ρ xy (+μ o H)-ρ xy (-μ o H)] / 2 to obtain the field dependence of ρxy. Both the original and doped AgSbTe2 samples show nonlinear field dependence. xy (H>6T) shows a linear field dependence, and the carrier concentration n is estimated using a single-band model, where e is the charge and R H From ρ xy (H) Slope-extracted Hall coefficient. Specific heat capacity of pristine and doped AgSbTe2 measured from 3K to 100K by adiabatic relaxation technique using a commercial PPMS Quantum Design under zero field conditions.

[0060] Density functional theory (DFT): First-principles calculations were performed using the projector augmented wave (PAW) method implemented in the Vienna Ab-initio Simulation Package (VASP). The exchange-correlation energies were calculated using the modified generalized gradient approximation (GGA) Perdew-Burke-Ernzerhof (PBEsol). For all calculations, the plane wave cutoff was set to 500 eV and a Monkhorst-Pack Γ-centered 11 × 11 × 11 k grid was used for Brillouin zone sampling. The well-known AgSbTe2 regular cell (64 atoms) was chosen as the initial structure. The internal atomic positions were fully relaxed until the residual forces between atoms were less than And the total energy reaches a convergence value of 10-8eV, and the electronic band structure and state density are calculated based on the fully relaxed structure.

[0061] The present invention is further described below in conjunction with specific embodiments and accompanying drawings:

[0062] Example 1

[0063] Step 1: Weigh the raw materials according to the stoichiometric ratio, place the mixed powder of silver, antimony and tellurium in a quartz tube, and seal it under vacuum (about 10 -4 Pa), slowly heating from room temperature to 900°C, the heating process lasts for 6 hours, then keeping at 900°C for 6 hours, and finally slowly cooling to room temperature, the cooling process lasts for 10 hours, to obtain a bulk ingot;

[0064] Step 2: crush the obtained bulk ingot into powder, sinter it by SPS (SPS, Dr. Sinter-625V, Fuji Corporation, Japan), apply 40 MPa pressure at 430°C, sinter for 2 minutes, and re-solidify to obtain AgSbTe2 material.

[0065] Example 2

[0066] A method for preparing a tin-doped high power density silver antimony telluride thermoelectric material comprises the following steps:

[0067] S1. Weigh the raw materials according to the stoichiometric ratio, place the mixed powder of silver, antimony, tellurium and tin in a quartz tube, seal it under vacuum (about 10 -4 Pa), slowly heating from room temperature to 900°C, the heating process lasts for 6 hours, then keeping at 900°C for 6 hours, and finally slowly cooling to room temperature, the cooling process lasts for 10 hours, to obtain a bulk ingot;

[0068] S2. The obtained bulk ingot was crushed into powder, and sintered by SPS (SPS, Dr. Sinter-625V, Fuji Corporation, Japan) at 430°C, applying 40 MPa pressure, sintering for 2 minutes, and resolidifying to obtain AgSb 0.94 Sn 0.06 Te2 material.

[0069] Example 3

[0070] The doping amount of Sn was changed to prepare Sn-doped AgSbTe2 thermoelectric material with x=0.03. The remaining preparation steps were the same as those in Example 2 to obtain AgSbTe2. 0.97 Sn 0.03 Te2 material.

[0071] Example 4

[0072] The doping amount of Sn was further changed to prepare Sn-doped AgSbTe2 thermoelectric material with x=0.1. The remaining preparation steps were the same as those in Example 2 to obtain AgSbTe2. 0.9 Sn 0.1 Te2 material.

[0073] Example 5

[0074] The thermoelectric device unit module in this embodiment is manufactured based on the technology in our previous report (Li W, Poudel B, NozariasbmarzA, et al. Bismuth telluride / half-Heusler segmented thermoelectric unicouple modules provide 12% conversion efficiency[J]. Advanced Energy Materials, 2020, 10(38): 2001924; ZhangY, Li Z, Singh S, et al. Defect-engineering-stabilizedAgSbTe2 with high thermoelectric performance[J]. Advanced Materials, 2023, 35(11): 2208994.).

[0075] The P-type leg adopts AgSb prepared in Example 2 0.94 Sn0 .06 Te2 material, and a Ni layer about 20 microns thick is deposited on the surface by chemical nickel plating. The N-type leg is made of Yb 0.25 Co 3.75 Fe 0.25 Sb 12 Skutterudite material. The fabricated bulk sample was cut into legs of specific sizes (P leg: 2.7 mm (length) × 2.9 mm (width) × 4.8 mm (height), N leg: 1.9 mm (length) × 1.4 mm (width) × 4.8 mm (height)) along the pressing direction using a wire saw. These legs were connected together by direct bonding of the copper substrate with gallium-indium eutectic metal. The output characteristics of the fabricated module were measured using a homemade power generation device. The measurement method and test principle have been explained in our previous work. The maximum power output P obtained from the thermoelectric module max (P out ) is calculated by the following expression:

[0076]

[0077] Among them, V oc is the measured open circuit voltage, R i is the internal resistance of the module. The heat flow of the unit device is calculated by:

[0078]

[0079] Where κ, A, l and ΔT are the thermal conductivity, cross-sectional area, length and temperature difference of the thermoelectric leg, respectively;

[0080] The conversion efficiency of the two-leg module is quantified by the following formula:

[0081]

[0082] Among them, Q in represents the heat flow from the heat source. The uncertainties of output power and conversion efficiency are ±1% and ±3%, respectively.

[0083] The undoped Sn material in Example 1 was compared, and the results showed that the thermoelectric power factor PF of the undoped Sn AgSbTe2 material was lower, and the thermoelectric figure of merit zT was also significantly lower than that of the Sn-doped material. The overall thermoelectric properties were inferior to those of the doped AgSbTe2 material.

[0084] Figure 1 is the phase diagram of pure AgSbTe2 material. Figure 1 It can be seen that the undoped pure phase AgSbTe2 is thermodynamically unstable at temperatures below 633K and will automatically decompose into Ag2Te and Sb2Te3 phases.

[0085] Figure 3 AgSbTe2 material, AgSb 1-x Sn x XRD spectrum of Te2 material, from Figure 3 It can be seen that the synthesized AgSbTe2 has a face-centered cubic (fcc) crystal structure. In addition, XRD also detected a small amount of monoclinic Ag2Te diffraction peaks, which confirmed the presence of these two phases in the synthesized material. XRD analysis confirmed that the Sn-doped material also exhibited a cubic AgSbTe2 phase, and no Ag2Te impurity phase was detected.

[0086] Figure 4 AgSbTe2 material, AgSb 1-x Sn x DSC curve of Te2 material; Differential scanning calorimetry analysis further confirmed that the endothermic peak of Ag2Te phase transition from β-Ag2Te to α-Ag2Te at 423K was suppressed.

[0087] Figure 5 The AgSb synthesized in Example 2 0.94 Sn 0.06 XPS spectrum of Te2 material; Figure 5 As shown in Figure 2, only one Sn 3d doublet peak at 486.1 eV (3d5 / 2) was observed. This is related to the divalent Sn state, further confirming that Sn 2+ Sn was successfully doped into the AgSbTe2 system. Overall, we observed that the incorporation of Sn effectively suppressed the formation of the Ag2Te heterophase and enhanced the thermodynamic stability of AgSbTe2.

[0088] In order to fully understand the effect of Sn doping on the AgSbTe2 structure, we used density functional theory (DFT) calculations to analyze the electronic band structure (e.g. Figure 6 a, 6b), and calculated the formation energy of various defects (such as Figure 7 c, 7d), the calculation analysis of the electronic band structure of undoped AgSbTe2 (as shown in Figure 6 a), near the Fermi level, we observed a light electron band and a heavy hole band (mainly formed by Te-5p orbitals), which indicates that the conductivity of AgSbTe2 mainly comes from high-mobility electrons and low-mobility holes. In addition, the flat valence band top and degenerate valence band structure indicate that the Seebeck coefficient of undoped AgSbTe2 is larger than that of other thermoelectric chalcogenides such as PbTe and SnTe. After the incorporation of Sn, the band structure of AgSbTe2 changed significantly. The valence band top becomes flatter at the Γ point, accompanied by significant band splitting, indicating that the Seebeck coefficient is enhanced. Specifically, due to the Sn 2+ Replace Sb 3+ , a new impurity band appears above the valence band top ( Figure 6 b). This impurity band is partially occupied and the Fermi level falls within its energy range. Therefore, carrier generation will jump from the impurity band edge to the conduction band. This mechanism leads to an increase in the hole concentration in the valence band, which is confirmed from the Hall measurement experimental data (Table S1).

[0089] Table S1. AgSbTe2 and AgSb at room temperature 1-x Sn x Comparison of carrier concentration and mobility of Te2 samples

[0090]

[0091] Atomic disorder usually causes additional scattering of charge carriers, which reduces carrier mobility. This results in a lower mobility for disordered systems than for pure compounds. Remarkably, even the introduction of a trace amount of disorder results in a significant decrease in mobility. This is further confirmed by our experimental results. Specifically, the hole mobility of undoped AgSbTe2 is 288 cm 2 / Vs, while in the Sn-doped disordered sample, the mobility drops to as low as 31 cm 2 / Vs (Table S1).

[0092] Ag vacancy (V Ag ) shows that it will spontaneously form in undoped AgSbTe2 ( Figure 7 c) V AgAs an acceptor to provide holes, however, the self-compensation effect leads to fewer Ag vacancies in the system to maintain the charge neutrality of the system, so the number of carriers is limited, resulting in a low net hole concentration in AgSbTe2. In the case of doping ( Figure 7 d), Sn doping generates composite defects (V Ag +Sn Sb ) further reduces V Ag The formation energy of the defects is much lower than that of other defects. By introducing the amount of Sn to control the preferential generation of composite defects, not only more holes are introduced, but also their concentration can be more finely adjusted and optimized. The partial state density (DOS) is as follows Figure 8 As shown, it is further verified that Sn doping reduces the contribution of Te-5p state in AgSbTe2 system, thereby improving its inherent instability. Overall, Sn doping plays a key role in stabilizing the AgSbTe2 structure by adjusting the band structure and changing the defect formation energy, thereby synergistically enhancing the hole concentration.

[0093] Low temperature (5-200K, Fig. 9 ) and high temperature (300-670K, Fig.12 The experimental data of carrier density in region b) verified this theory. With the introduction of Sn doping, the room temperature carrier density increased to 2.0×10 19 cm -3 , significantly higher than that of undoped AgSbTe2.

[0094] We then investigated the effect of Sn doping on the resulting atomic disorder due to the random occupancy of Ag and Sb ions in the cation sublattice of AgSbTe2. Our results show that doping with tin (Sn) causes the lattice structure of AgSbTe2 to become ordered in the short range and more disordered in the long range. High-resolution high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) observations reconfirmed that the Sn-doped AgSbTe2 sample exhibited a face-centered cubic phase (space group: Fm-3m) structure with a lattice parameter of a = 0.608nm ( Fig.10 a). In AgSb 0.94 Sn 0.06 The multiple double diffraction spots observed in the power spectrum of Te2 (circled in red and green) originate from structural perturbations within the AgSbTe2 structure. The composite image ( Fig.10b) confirmed that these double diffraction spots are not caused by impure phases, but are produced by the disordered lattice of the system. Individual FFT images obtained from the diffraction spots circled in green and red clearly show structural perturbations especially in the red circled area. This disordered lattice structure originates from the microstructure composed of multiple short-range ordered Ag / Sb cations in the Sn-doped AgSbTe2 matrix. Fig.10 e, the weaker diffraction spots (marked by red arrows) observed are located between the basic spots, indicating that the cation ordered domains in Sn-doped AgSbTe2 lead to the doubling of the unit cell. Some of the reflection spots show double diffraction ( Fig.10 e), indicating that the short-range cation order in the sample may be irregular. Fig.10 The micrographs in f and 10g show the Fig.10 d Detailed high-resolution transmission electron microscopy (HRTEM) images of the red and green boxed areas and their corresponding FFTs further demonstrate the similarity with undoped AgSbTe2 ( Fig.11 ) is more chaotic in structure.

[0095] For undoped AgSbTe2, the conductivity (σ) first decreases and then increases ( Fig.12 a). This increase is attributed to the contribution of bipolar conductivity in the high temperature region, which is consistent with the reported findings. In undoped AgSbTe2, the bipolar effect begins to appear at 460K, slightly higher than the Bi2Te3 system (350-400K), which is related to the smaller band gap of 0.15eV of Bi2Te3. The bipolar transport phenomenon reduces the Seebeck coefficient of undoped AgSbTe2 in the high temperature range because the minority carriers (electrons) thermally excited at high temperature offset the contribution of holes to the Seebeck coefficient. The Seebeck coefficient of undoped AgSbTe2 increases from 270μV / K at 300K to 389μV / K at 465K. The high Seebeck coefficient observed in undoped AgSbTe2 originates from the degenerate flat valence band, which induces a distortion of the electronic density of states and leads to an increase in the effective mass (m*). The measured high Seebeck coefficient and the significant bipolar phenomenon at high temperatures demonstrate the semiconductor characteristics of AgSbTe2. When Sn 2+ Substitute for Sb 3+ The conductivity of the sample increases significantly in the entire temperature range, from 89S / cm of undoped AgSbTe2 to 100S / cm of doped AgSbTe2 at 300K. 0.94 Sn 0.06 231S / cm for Te2. This increase in conductivity is related to the increase in hole concentration caused by newly generated impurity bands and defect complexes. The optimal doping concentration is 6mol% Sn doping. It is worth noting that AgSb 0.94 Sn 0.06The hole concentration of Te2 at 2K is 4.8×10 20 cm -3 , compared with undoped AgSbTe2 (6.9×10 19 cm -3 ) is six times higher. After the introduction of Sn, the Seebeck coefficient decreases due to the increase in charge carrier concentration. However, the doped samples still show excellent Seebeck coefficients over the entire temperature range, exceeding 170 μV / K ( Fig.12 d) This phenomenon is mainly due to the change of band structure after Sn doping, which is manifested as band flattening and splitting, resulting in m * The increase helps to maintain a relatively high Seebeck coefficient. Compared with undoped AgSbTe2, the Seebeck coefficient of the Sn-doped sample continues to increase after 450K, which is mainly attributed to the significant suppression of the bipolar effect. 0.94 Sn 0.06 The greatly improved conductivity and relatively high Seebeck coefficient of Te2 lead to a significant increase in its power factor over the entire temperature range ( Fig.12 e). At 673K, AgSb 0.94 Sn 0.06 The peak power factor PF of Te2 reaches 27μWcm -1 K -2 , exceeding Cu 2-x Se, PbTe, SnTe, etc., and to the best of our knowledge, this is the highest recorded value reported for AgSbTe2 ( Fig.12 f). This is comparable to the power factor of commercial thermoelectric material Bi2Te3, indicating that it has great potential in practical power generation device applications. The total thermal conductivity (κ) of undoped AgSbTe2 first decreases with temperature, from 0.55 W / mK at 300 K to 0.48 W / mK at about 450 K ( Fig.12 g), and then increases. This rise in thermal conductivity is attributed to the contribution of the bipolar thermal conductivity (κbi) ( Fig.12 h and Fig.13 ). The low thermal conductivity of undoped AgSbTe2 is consistent with previous studies that have shown that undoped AgSbTe2 exhibits ultra-low intrinsic thermal conductivity, which has been attributed to defects, stacking faults, and spontaneously formed mixed phases. Sn-doped AgSbTe2 exhibits higher thermal conductivity than undoped AgSbTe2 due to increased electronic thermal conductivity (κe) and slightly higher lattice thermal conductivity κL. In addition, partial substitution of Sn in AgSbTe2 significantly reduces the contribution of κbi, although the suppression of the bipolar effect is not complete. This reduction is attributed to the substantial reduction in the number of n-type carriers after doping. As temperature increases, AgSb 0.94 Sn 0.06The lowest lattice thermal conductivity κL of Te2 sample reaches 0.41W / mK. From the combination of increasing carrier concentration and high Seebeck coefficient, AgSb 0.94 Sn 0.06 Te2 material shows a high zT value, up to 2.5, and an average zT of 1.32 in the temperature range of 300 to 673K ​​(see Fig.12 i).

[0096] By analyzing multiple batches of synthetic samples (see Fig.14 ) and performance in multiple heating and cooling cycles (see Fig.15 ), demonstrating the reproducibility of these high zT values.

[0097] After obtaining a higher zT value and power factor (PF), we further fabricated a thermoelectric power generation device (Example 5), which includes p-type AgSb 0.94 Sn 0.06 Te2 legs and n-type skutterudite Yb 0.25 Co 3.75 Fe 0.25 Sb 12 Legs (see Fig.16 and Fig.17 ).

[0098] When the cold side temperature is set to 300K, the open circuit voltage (Voc) increases linearly with ΔT (see Fig.18 ), verifying the smaller contact resistance within the device. It is worth noting that the maximum output power (Pout) increases from 4.5 mW at ΔT = 80K to 103 mW at ΔT = 370K, as shown in Fig.19 and Fig. 20 As shown, a power density of 1.13 watts per square centimeter was achieved, which is the highest value reported in all studies on AgSbTe2. Fig.19 ). In addition, an excellent energy conversion efficiency (η) of 12.1% was achieved under the temperature difference condition of ΔT = 370K. These values ​​prove that p-type AgSb 0.94 Sn 0.06 Te2 material is a promising key material for thermoelectric energy conversion in the medium temperature range.

[0099] AgSbTe2 and AgSb at room temperature 1-x Sn x The density of the Te2 sample is shown in Table S2, and the relative density of the obtained cylinder is more than 95% higher than the theoretical value.

[0100] Table S2. Density of AgSbTe2 and AgSb1-xSnxTe2 samples

[0101] Sample name Density(g / cm3) Relative density <![CDATA[AgSbTe2]]> 6.85 96.1% <![CDATA[AgSb 0.97 Sn 0.03 Te2]]> 6.81 95.5% <![CDATA[AgSb 0.94 Sn 0.06 Te2]]> 6.87 96.3% <![CDATA[AgSb 0.9 Sn 0.1 Te2]]> 6.89 96.7%

[0102] In summary, the carrier density of polycrystalline AgSbTe2 is optimized by Sn doping. The substitution of Sn for Sb helps to form a new impurity band above the highest point of the valence band. In addition, the introduction of Sn suppresses the ambipolar diffusion effect and prevents the formation of n-type Ag2Te, resulting in a relatively high Seebeck coefficient. Therefore, AgSb 0.94 Sn 0.06 Te2 alloy showed a high performance of 27 μW cm -1 K -2 In addition, Sn doping also leads to a more disordered lattice structure, which is manifested by the minimum lattice thermal conductivity reaching 0.41W / mK. Although this enhanced structural disorder fails to effectively reduce the lattice thermal conductivity of AgSbTe2, the excellent power factor makes up for this limitation. Overall, AgSb 0.94 Sn 0.06 Te2 achieves a maximum zT value of 2.5 at 673K, and an average zT of 1.32 in the temperature range of 300 to 673K, which is better than the current state-of-the-art mid-temperature range p-type materials. We further designed thermoelectric devices and achieved energy conversion efficiencies of up to 12.1% and 1.13W / cm at ΔT = 370K. 2 Overall, this work provides key technologies for the engineering design of high-performance intermediate-temperature thermoelectric materials and devices that can be effectively used in power generation applications, such as Fig.21 shown.

[0103] The above are only preferred embodiments of the present invention, and only describe the implementation methods of the present invention. They do not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A tin-doped high power density silver antimony telluride thermoelectric material, characterized in that: Taking AgSbTe2 as the matrix, the AgSbTe2 material is modified by hole doping Sn, and an impurity band is introduced at the top of its valence band. The chemical structure of the obtained product is AgSb 1- x Sn x Te2; 0<x≤0.

1.

2. The tin-doped high power density silver antimony telluride thermoelectric material according to claim 1, characterized in that: AgSbTe2 material has a face-centered cubic (fcc) crystal structure, with Ag and Sb ions randomly distributed in the cation sites of the lattice, while Te occupies the anion sites.

3. A method for preparing a tin-doped high power density silver antimony telluride thermoelectric material, comprising the following steps: S1. Weigh the raw materials according to the stoichiometric ratio, place the mixed powder of silver, antimony, tellurium and tin in a reactor, slowly heat it to a set temperature under vacuum conditions, keep it warm for a predetermined time, and then slowly cool it to room temperature to obtain a bulk ingot; S2. The obtained block ingot is crushed into powder and sintered by SPS to obtain a cylinder, namely AgSb 1-x Sn x Te2 material.

4. The method for preparing the tin-doped high power density silver antimony telluride thermoelectric material according to claim 3, characterized in that: In step S1, the quartz tube is heated from room temperature to 1173-1373K under vacuum conditions, kept at 1173-1373K for 3-10 hours, and finally slowly cooled to room temperature. The cooling process lasts for 6-24 hours to obtain a bulk ingot.

5. The method for preparing the tin-doped high power density silver antimony telluride thermoelectric material according to claim 3, characterized in that: The AgSb was re-densified by spark sintering (SPS), specifically: applying 20-60 MPa pressure at 623-773 K for 1-5 minutes to obtain AgSb 1-x Sn x Te2 material.

6. A thermoelectric device unit module, characterized in that: The P-leg of the module adopts the AgSb 0.94 Sn 0.06 Te2 material, N-type legs use Yb 0.25 Co 3.75 Fe 0.25 Sb 12 Skutterudite material.

Citation Information

Cited By

  • Large-size SnSb2Te4 single crystal and growth method thereof

    CN119800514A