Non-siloxane sensory modifiers

The polyolefins are crosslinked by polyether crosslinking agent to form a crosslinked elastomer with carbon-silicon-carbon bonds, solving the problem of low molecular weight volatility in silicone elastomers, achieving a skin feeling similar to silicone and a variety of skin sensations and Organic solvent compatibility provides safer skin care product ingredients.

CN118922166APending Publication Date: 2024-11-08DOW SILICONES CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029663.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-02-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, silicone elastomers have the possibility of low molecular weight volatile silicones and cyclic compounds as sensory modifiers in skin care products, and it is difficult to find materials similar to silicones but without silicones. Moreover, traditional silicone modified polyolefins still rely on silicone polymers, affecting the compatibility of various organic solvents of the material.

Method used

Cross-linking of polyolefins through polyether crosslinking agents forms a cross-linked elastomer with carbon-silicon-carbon bonds, avoiding Si-O-Si bonds, achieving a skin feeling similar to silicone elastomers and a phase of multiple organic solvents. Capacity.

Benefits of technology

Achieving a skin feel similar to a silicone elastomer and a wide range of organic solvent compatibility in the absence of silicone, providing safer and more flexible skin care product ingredients.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005055388810000041
    Figure BDA0005055388810000041
  • Figure BDA0005055388810000121
    Figure BDA0005055388810000121
  • Figure BDA0005055388810000122
    Figure BDA0005055388810000122
Patent Text Reader

Abstract

A composition comprising a cross-linked elastomer comprising a polyolefin backbone cross-linked by a polyether chain, where the cross-linked elastomer has a carbon-silicon-carbon bond between the polyolefin backbone and the polyether chain, and where the cross-linked elastomer is free of Si-O-Si bonds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention is a cross-linked elastomer free of siloxane bonds, a composition comprising the cross-linked elastomer, and a method for producing the cross-linked elastomer. Background Art

[0002] US9999586 ('586) teaches that silicone elastomers are considered to be one of the best sensory modifiers for use in skin care formulations. '586 identifies the unique structure of silicone elastomers because silicone elastomers have a skin feel different from any silicone fluid or cationic quaternary ammonium compound previously used as a sensory modifier. The feel of silicone elastomers has been described as "velvety, powdery, smooth and cushioned feel". Silicone elastomers are used as sensory modifiers in solvent-swollen pastes, wherein the elastomer is solvent-swollen and blended to break the elastomer into pieces to form a paste. Ideally, the solvent-swollen elastomer pieces have an average particle size in the range of 1 micron to 1,000 microns, preferably 1 micron to 100 microns, more preferably 1 micron to 50 microns and even more preferably 1 micron to 25 microns. Smaller particles are more ideal for a smoother feel.

[0003] However, it would be desirable to identify sensory modifiers that provide a similar feel to silicone elastomers but with materials other than silicone because of the possibility that silicones may undesirably contain low molecular weight volatile silicones and cyclic compounds.

[0004] US9999586 describes silicone modified polyolefins as possible alternatives to silicone elastomers for use as sensory modifiers in skin care formulations. Silicone modified polyolefins are sought to have a similar sensory feel to silicone elastomers, but contain polyolefin and silicone polymer components to reduce the amount of silicone polymer in the material. Silicone modified polyolefins still rely on silicone polymers to achieve a unique structure associated with the desired skin feel of the sensory modifier.

[0005] It is also desirable that the elastomers and elastomeric pastes be compatible with a variety of organic solvents used in cosmetic formulations so that the elastomers can be formulated in a variety of cosmetic formulations. Typical organic solvents include octyl methoxycinnamate, ethylhexyl salicylate, sunflower oil, squalane, and mineral oil. Compatible elastomers and pastes form clear or turbid mixtures with the solvents, rather than being turbid, opaque, or phase separated from the solvent.

[0006] It would be desirable to identify an elastomer that could be a sensory modifier that has a similar skin feel to the silicone elastomers commonly used as sensory modifiers in the cosmetic industry, but without the need for silicone. It would also be desirable for the elastomer to have solvent compatibility with a variety of organic solvents used in cosmetic formulations. Summary of the invention

[0007] The present invention provides an elastomer that can be a sensory modifier, having a similar skin feel to silicone elastomers, but without the need for silicone. The present invention can also provide an elastomer that can form a paste that is at least as compatible with a variety of organic solvents as similar pastes of silicone elastomers commonly used in the cosmetic field.

[0008] The present invention is the result of the discovery that crosslinking polyolefins with polyether crosslinkers and linking polyolefins and polyethers with carbon-silicon-carbon (C-Si-C) bonds produces an elastomer that can be solvent swollen and mixed into a paste that has a skin feel similar to that of a paste made with silicone elastomers. The combination of C-Si-C bonds and polyether crosslinks is believed to cause a particular skin feel. The unique bond angles created by the C-Si-C bonds are believed to help form an ideal morphology that promotes a desired skin feel. The polyether provides an ideal compatibility for the elastomer to allow the elastomer to be formulated in a variety of formulations and to provide the desired mobility between the polyolefin backbones. The C-Si-C bonds and polyether crosslinks together are believed to produce an elastomer that has a skin feel similar to that of a paste made with silicone elastomers in a solvent swollen paste.

[0009] In a first aspect, the present invention is a composition comprising a crosslinked elastomer comprising a polyolefin backbone crosslinked by polyether chains, wherein the crosslinked elastomer has carbon-silicon-carbon bonds between the polyolefin backbone and the polyether chains, and wherein the crosslinked elastomer is free of Si-O-Si bonds, which are essential in silicones.

[0010] In a second aspect, the present invention is a method for producing the composition of the first aspect, the method comprising providing a crosslinked elastomer by performing a hydrosilylation reaction with a reaction composition, the reaction composition comprising: (a) a hydrosilane-functional polyolefin that does not contain Si-O-Si bonds; (b) a polyether crosslinker that contains at least two terminal alkenyl groups and does not contain Si-O-Si bonds; (c) a hydrosilylation catalyst; and (d) an organic solvent.

[0011] The compositions of the present invention are useful as sensory modifiers in skin care products. DETAILED DESCRIPTION

[0012] When a test method number is not used to indicate a date, the test method refers to the most current test method as of the priority date of this document. Reference to a test method includes reference to both the testing association and the test method number. The following test method abbreviations and designations apply herein: ASTM refers to ASTM International methods; EN refers to European Standards; DIN refers to the German Institute for Standardization; ISO refers to the International Organization for Standardization; and UL refers to Underwriters Laboratories.

[0013] Products identified by their trade names refer to compositions available under those trade names on the priority date of this document.

[0014] "Plurality" means two or more. "And / or" means "and, or as an alternative." Unless otherwise indicated, all ranges are inclusive.

[0015] The term "interpolymer" refers to polymers prepared by polymerizing at least two different types of monomers. The term interpolymer encompasses the term copolymer (which refers to polymers prepared from two different types of monomers) and polymers prepared from more than two different types of monomers.

[0016] For the polymers herein, the number average molecular weight ("Mn") was determined using the following gel permeation chromatography method: (GPC) ”):

[0017] Gel Permeation Chromatography Method for Molecular Weight

[0018] The chromatographic system consists of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5). The autosampler oven compartment is set at 160°C and the column compartment is set at 150°C. These columns are an Agilent PLgel MIXED 7.5×50mm, 20μm linear mixed bed guard column and four Agilent PLgel MIXED-A 7.5×300mm, 20μm linear mixed bed columns. The chromatographic solvent is 1,2,4-trichlorobenzene, which contains 200ppm of butylated hydroxytoluene (BHT). The injection volume used is 200 microliters, and the flow rate is 1.0 ml / min.

[0019] Calibration of the GPC column set was performed using Agilent EasiCal polystyrene standards (EasiCal PS-1 and EasiCal PS-2). Each EasiCal system consists of two different spatulas supporting a mixture of 5 polymer standards (approximately 5 mg) to obtain 20 molecular weight points ranging from approximately 580 g / mole to 6,570,000 g / mole. A single spatula was added to a vial covered with a septum, sealed and loaded into the PolymerChar autosampler. 8 mL of solvent was added to each vial using the PolymerChar instrument control software, and the standards were dissolved at 160 ° C for 15 minutes under high-speed shaking before being injected into the chromatography system. The nominal polystyrene standard peak molecular weight was fitted using a third-order polynomial to obtain the molecular weight equivalent calibration point at each chromatographic slice.

[0020] Total plate counts for the GPC column set were performed using decane (3% v / v TCB introduced via a micro pump). For four Agilent "Mixed A" 30 cm 20-micron linear mixed bed columns, the plate count for the chromatography system should be greater than 18,000.

[0021] The samples were prepared semi-automatically using the PolymerChar instrument control software, with the target sample weight set at 2 mg / ml and the solvent added to a sealed vial capped with a septum by the PolymerChar high temperature autosampler. The samples were dissolved at 160°C for two hours with high speed shaking.

[0022] Mn (GPC) 、Mw (GPC) and Mz (GPC) The calculation of is based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR spectrometer according to equations 1-3. TM Software that converts the baseline-subtracted IR chromatogram at each equally spaced data collection point (i) into a polystyrene equivalent molecular weight obtained from a narrow standard calibration curve of equivalent chromatographic data points (i). Equations 1-3 are as follows:

[0023]

[0024] To monitor deviations over time, a flow rate marker (solvent containing 3% v / v decane) was introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow rate marker (FM) was used to linearly correct the pump flow rate for each sample (Flow Rate (Nominal)) by comparing the RV of the corresponding decane peak in the sample (RV (FM Sample)) with the RV of the decane peak in the narrow standard calibration (RV (FM Calibrated)). Any changes in the timing of the decane marker peak were then assumed to be related to a linear change in the flow rate (Flow Rate (Effective)) over the entire run. After calibrating the system based on the flow marker peak, the effective flow rate (relative to the narrow standard calibration) was calculated as Equation 4. TM The software completes the processing of the flow marker peaks. An acceptable flow rate correction is such that the effective flow rate should be within + / - 0.7% of the nominal flow rate.

[0025] Flow rate (effective) = flow rate (nominal) * (RV (FM calibration) / RV (FM sample)) (Equation 4)

[0026] The composition of the present invention comprises a crosslinked elastomer comprising a polyolefin backbone crosslinked by polyether chains and further characterized by having carbon-silicon-carbon (C-Si-C) bonds connecting the polyolefin backbone and the polyether chains and being free of siloxane (Si-O-Si) bonds.

[0027] The polyolefin backbone is a homopolymer or interpolymer comprising interpolymerized monomers polymerized through carbon-carbon double bonds (C=C). Ideally, the polyolefin backbone comprises a polymerized olefin selected from the group consisting of olefins having 2 or more, preferably 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, even 8 or more, and typically 10 or less, 9 or less, 8 or less, 7 or less, 6 or less carbon atoms. Most ideally, the polyolefin backbone comprises an interpolymer containing polymerized ethylene and octene.

[0028] The polyolefin backbone also includes an interpolymerization monomer that produces a side chain carbon chain comprising a carbon-silicon bond (C-Si) connecting a silicon atom to the polyolefin backbone, preferably the side chain carbon chain is terminated with C-Si. Crosslinking occurs through the Si of the C-Si bond, particularly through a C-Si-C bond comprising a C-Si bond. The polyolefin may, for example, include interpolymerized alkenyl silanes, such as 7-octenyl dimethyl silane and / or 5-hexenyl dimethyl silane. Crosslinking may then occur through the silicone hydride bond (Si-H) of the silane to produce a C-Si-C bond between the backbone and the polyether crosslinking agent.

[0029] Desirably, the polyolefin backbone is an interpolymer comprising or consisting of the following polymerized monomer segments: (a) 20 to 35 mole percent octene; (b) 65 to 80 mole percent ethylene; and (c) 1 to 10 mole percent of one or any combination of more than one of 7-octenyldimethylsilane and 5-hexenyldimethylsilane.

[0030] The polyether chain of the crosslinked polyolefin backbone generally comprises polyether units selected from -RO- groups, wherein R is an alkylene group having 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, or even 7 or more carbon atoms and at the same time generally having 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, or even 3 or less carbon atoms. For example, the polyether chain may comprise any one of polyethylene oxide, polypropylene oxide, and polybutylene oxide, or any combination of more than one.

[0031] The polyether chains crosslinking the polyolefin backbone typically contain 3 or more, 5 or more, 10 or more, 15 or more, or even 20 or more -RO- groups, while typically containing 100 or less, 75 or less, 60 or less, 50 or less, 45 or less, 40 or less, 30 or less, 25 or less, or even 20 or less -RO- groups.

[0032] The crosslinked elastomer desirably comprises or consists of the following interpolymeric polymer segments:

[0033] (a) 20 mol % to 35 mol % of an average chemical structure of

[0034] One or more than one of the CH2CHR'- chain segments;

[0035] (b) 65 mol% to 80 mol% -CH2CH2-; and

[0036] (c) 1 to 10 mole percent of -CH2CHA-;

[0037] Wherein mol% is the number of moles of interpolymer segments relative to the crosslinked elastomer; each R'

[0038] is independently selected at each occurrence from the group consisting of: having one or more, 2 or more, 3 or more, 4 or more, 5 or more, even 6 or more carbon atoms, while typically having 8 or less, 7 or less, even 6 or more

[0039] An alkyl group having less than 1 carbon atom; and A has the following average chemical structure (I):

[0040] -(CH2) n Si(CH3)2-BD(I)

[0041] And among them:

[0042] n, independently at each occurrence, is a value in the range of 4 to 6, and may be 4, 5, or 6;

[0043] B is -(CH2)3O(RO) p’ (CH2)3-;

[0044] in:

[0045] Each R at each occurrence is independently as defined above, and is preferably a combination of one or two alkylene groups selected from -CH2CH2- and -CH2CH(CH3)- groups; and

[0046] The subscript p' has 15 或更大 , or a value of 20 or more and 25 or less; and

[0047] D is another A group -Si(CH3)2(CH2) n -groups, so that component B is a cross-linking group connecting two main chain groups consisting of other interpolymer segments.

[0048] The composition of the present invention may also include a solvent with a crosslinked elastomer. The crosslinked elastomer may be swollen with the elastomer to form a solvent-swollen elastomer. A solvent-swollen elastomer is an elastomer that has absorbed a solvent. Typically, a solvent-swollen elastomer has a greater volume than the elastomer alone in the absence of the solvent.

[0049] Typical solvents include hydrocarbons, esters and ethers. Examples of suitable solvents include any one or a combination of more than one selected from isohexadecane, isododecane, undecane, tridecane, dioctyl carbonate, isodecyl neopentanoate and di-n-octyl ether.

[0050] Desirably, the composition comprises solvent in a concentration of 90 wt % or more, or even 95 wt % or more, and typically 97 wt % or less, based on the weight of the composition.

[0051] The composition may comprise microparticles of a solvent swollen elastomer. Desirably, the composition comprises a solvent swollen elastomer having an average particle size of 1 micron or more, 5 microns or more, 10 microns or more, 20 microns or more, 30 microns or more, 40 microns or more, 50 microns or more, 75 microns or more, 100 microns or more, 125 microns or more, 150 microns or more, 175 microns or more, 200 microns or more, 225 microns or more, 250 microns or more, 275 microns or more, 300 microns or more, 325 microns or more, 350 microns or more, 375 microns or more, 400 microns or more, 425 microns or more, 450 microns or more, 465 microns or more, 480 microns or more, 490 microns or more, 500 microns or more, 510 microns or more, 520 microns or more, 530 microns or more, 540 microns or more, 550 microns or more, 560 microns or more, 570 microns or more, 580 microns or more, 590 microns or more, 600 microns or more, 610 microns or more, 620 microns or more, 630 microns or more, 640 microns or more, 650 microns or more, 660 microns or more, 670 microns or more, 680 microns or more, 690 microns or more, 700 microns or more, 710 microns or more, 720 microns or more, 730 microns or more, 740 microns or more, 750 microns or more, 760 microns or more, 7 or less, or even 450 microns or more, while 500 microns or less, 475 microns or less, 450 microns or less, 425 microns or less, 400 microns or less, 375 microns or less, 350 microns or less, 325 microns or less, 300 microns or less, 275 microns or less, 250 microns or less, 225 microns or less, 200 microns or less, 175 microns or less, 150 microns or less, 125 microns or less, 100 microns or less, 75 microns or less, 50 microns or less, 25 microns or less, 20 microns or less, or even 10 microns or less.

[0052] The following elastomer microparticle screening method is used to measure the average particle size of the solvent-swollen elastomer microparticles. The elastomer microparticle screening method is a laser diffraction method using Mastersize 3000 (from Malvern Panalytical). The sample of the elastomer paste is prepared by placing 1.00 grams (g) of solvent-swollen elastomer into a 20g dental mixing cup and mixing for 30 seconds at 3500 revolutions per minute (RPM) using a speed mixer. Add 0.5g of isododecane and mix for 30 seconds at 3500RPM. Add another 0.5g of isododecane and mix for 30 seconds at 3500RPM. Add another 1.0g of isododecane and mix for 30 seconds at 3500RPM. Add another 2.0g of isododecane and mix for 30 seconds at 3500RPM. Add another 2.0g of isododecane and mix for 30 seconds at 3500RPM. An additional 4.0 g of isododecane was added and mixed at 3500 RPM for 10 seconds to obtain an elastomer paste - a solvent swollen elastomer containing solvent swollen elastomer microparticles. A sample of the elastomer paste was added to a hydro SV fluid cell and the average particle size was determined using a Masterizer 3000. Data was collected and analyzed using Mastersizer v. 3.81 software and assuming non-spherical particles, a material refractive index of 1.5 (standard olefin), a dispersant refractive index of 1.42 (isododecane) and tested at an obscuration between 2% and 25%.

[0053] The composition may contain sunscreens, colorants and / or sunscreen additives, such as titanium dioxide, zinc oxide or combinations thereof, in a concentration of up to 20 wt % based on the weight of the composition.

[0054] The present invention also includes a method for preparing the composition of the present invention by providing a crosslinked elastomer by performing a hydrosilylation reaction with a reaction composition, wherein the reaction composition comprises: (a) a hydrosilane-functional polyolefin that does not contain Si-O-Si bonds; (b) a polyether crosslinker that contains at least two terminal alkenyl groups and does not contain Si-O-Si bonds; (c) a hydrosilylation catalyst; and (d) an organic solvent.

[0055] Hydrosilane-functional polyolefins that do not contain Si-O-Si bonds can be prepared according to the teachings of US6624254. Hydrosilane-functional polyolefins form the polyolefin backbone of the crosslinked elastomer and can therefore be characterized as described above for the polyolefin backbone of this article. Ideally, the hydrosilane-functional polyolefin has a number average molecular weight (Mn) of 15,000 or greater, 20,000 or greater, 25,000 or greater, 30,000 or greater, 35,000 or greater, 40,000 or greater, 45,000 or greater, or even 50,000 or greater. (GPC)), while desirably having an Mn of 150,000 or less, 146,000 or less, 140,000 or less, 120,000 or less, 100,000 or less, 80,000 or less, 70,000 or less, 60,000 or less, 55,000 or less, 50,000 or less, 45,000 or less, or even 40,000 or less. (GPC) .

[0056] The hydrosilane-functional polyolefin is a random interpolymer (as opposed to a block interpolymer). Ideally, the hydrosilane-functional polyolefin is a random interpolymer comprising or consisting essentially of the following interpolymeric segments (excluding possible end groups on the interpolymer): -(CH2CHR')-, -R"-, and -(CH2CHG)-; wherein:

[0057] Each R' may be the same or different relative to the other R' groups, and each R' at each occurrence is independently selected from the group consisting of: having one or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, or even 7 or more carbon atoms, while typically having 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less carbon atoms.

[0058] Alkyl groups with carbon atoms;

[0059] Each R" may be the same or different with respect to the other R" groups, and each R" at each occurrence is independently selected from the following: an alkylene group having one or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, or even 7 or more carbon atoms, while typically having 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less carbon atoms;

[0060] Each G may be the same or different relative to the other G groups, and each G at each occurrence is independently a group selected from those having the following average chemical structure: -R 3 S i 4 2H, where

[0061] Each R 3 Compared with other R 3 The groups may be the same or different, and each R 3independently selected from the group consisting of: an alkylene group having one or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, even 7 or more, while typically 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, even 2 or less carbon atoms; and

[0062] Each R 4 Compared with other R 4 The groups may be the same or different, and each R 4 is independently selected at each occurrence from the group consisting of hydrogen and an alkyl group having one or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, even 7 or more, while typically 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, even 2 or less carbon atoms.

[0063] The -(CH2CHR')- segments are typically present in the hydrosilane-functional polyolefin at a concentration of 20 mole percent (mol%) or more, 25 mol% or more, or even 30 mol% or more, and typically 35 mol% or less, 30 mol% or less, or even 25 mol% or less; wherein the mol% is relative to the total moles of the interpolymerized segments.

[0064] The -R"- segments are typically present in the hydrosilane-functional polyolefin at a concentration of 65 mol% or more, 70 mol% or more, or even 75 mol% or more, and typically 80 mol% or less, 75 mol% or less, or even 70 mol% or less; wherein the mol% is relative to the total moles of interpolymerized segments.

[0065] The -(CH2CHG)- segments are typically present in the hydrosilane-functional polyolefin at a concentration of 1 mol% or more, 5 mol% or more, or even 7.5 mol% or more, and typically 10 mol% or less, 7.5 mol% or less, or even 5 mol% or less; wherein the mol% is relative to the total moles of the interpolymerized segments.

[0066] The hydrosilane-functional polyolefin can be an interpolymer of: (a) 20 mol% to 35 mol% 1-octene; (b) 65 mol% to 80 mol% ethylene; and (c) 1 mol% to 10 mol% of any combination of one or both of 7-octenyldimethylsilane and 5-hexenyldimethylsilane, wherein the mole percentages are relative to the total moles of 1-octene, ethylene, 7-octenyldimethylsilane and 5-hexenyldimethylsilane; wherein the mol% are relative to the total moles of (a), (b) and (c).

[0067] The polyether crosslinking agent contains polyether units selected from -RO- groups, wherein R is an alkylene group having 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, or even 7 or more carbon atoms, and at the same time typically having 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, or even 3 or less carbon atoms. Typically, the polyether crosslinking agent contains 3 or more, 5 or more, 10 or more, 15 or more, or even 20 or more -RO- groups, and typically contains 100 or less, 75 or less, 60 or less, 50 or less, 45 or less, 40 or less, 30 or less, 25 or less, or even 20 or less -RO- groups.

[0068] The polyether crosslinking agent may be, for example, any one or any combination of more than one selected from the group consisting of: bisallyl propylene glycol, bisallyl ethylene glycol and propylene glycol, α, Ω-unsaturated hydrocarbons such as those having the chemical formula CH2=CH(CH2) d Those of CH═CH2, wherein the subscript d has an average value of zero or greater, and can be 1 or greater, 2 or greater, 3 or greater, 4 or greater, 5 or greater, 6 or greater, 7 or greater, 8 or greater, 9 or greater, 10 or greater, 11 or greater, 12 or greater, 13 or greater, or even 14 or greater, while typically is 20 or less, and can be 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, or even 4 or less.

[0069] The hydrosilylation catalyst can be any catalyst that can be used to catalyze the hydrosilylation reaction. Typically, the hydrosilylation catalyst is a platinum-based catalyst. Platinum-based hydrosilylation catalysts include compounds and complexes such as platinum (0) -1,3-divinyl-1,1,3,3-tetramethyldisiloxane (Karstedt's catalyst), H2PtCl6, di-μ.-carbonyldi-.π.-cyclopentadienyl dinickel, platinum-carbonyl complexes, platinum-divinyltetramethyldisiloxane complexes, platinum cyclovinylmethylsiloxane complexes, acetylacetonate platinum (acac), platinum black, platinum compounds (such as chloroplatinic acid, hexahydrate chloroplatinic acid, the reaction product of chloroplatinic acid and a monohydric alcohol, bis (ethyl acetoacetate) platinum, bis (acetylacetonate) platinum, platinum dichloride) and complexes of platinum compounds with olefins or low molecular weight organopolysiloxanes or platinum compounds microencapsulated in a matrix or core-shell structure. The hydrosilylation catalyst may be part of a solution comprising a complex of platinum and a low molecular weight organopolysiloxane, including a complex of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane and platinum. These complexes may be microencapsulated in a resin matrix. The catalyst may be a complex of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane and platinum.

[0070] Typical solvents include hydrocarbons, esters and ethers. Examples of suitable solvents include any one or a combination of more than one selected from isohexadecane, isododecane, undecane, tridecane, dioctyl carbonate, isodecyl neopentanoate and di-n-octyl ether.

[0071] Example

[0072] Synthesis of Hydrosilane Functional Polyolefin (HFP)

[0073] Ethylene / octene / silane interpolymerization was carried out in a 2L autoclave batch reactor designed for ethylene homopolymerization and copolymerization. The reactor was equipped with electric heating tape and internal cooling coils containing cooling diol. Both the reactor and the heating / cooling system were controlled and monitored by a process computer. The bottom of the reactor was equipped with a dump valve, which emptied the reactor contents into a dump pan connected to the atmosphere.

[0074] All chemicals and catalyst solutions used for polymerization were passed through purification columns before use. ISOPAR-E, 1-octene, ethylene and silane monomers were also passed through the column. Ultra-high purity grades of nitrogen (Airgas) and hydrogen (Airgas) were used. The catalyst mixture was prepared by mixing a scavenger (MMAO-3A), an activator (bis(hydrogenated tallow alkyl)methyltetrakis(pentafluoro-phenyl)borate amine) and a precatalyst (zirconium, dimethyl[[2,2"'-[1,3-propanediylbis(oxy-κO)]bis[3",5,5"-tris(1,1-dimethylethyl)-5'-methyl[1,1':3',1"-terphenyl]-2'-olato-κO]](2-)]-(ACI)) with an appropriate amount of toluene to obtain a solution of the desired molar concentration in an inert glove box. The solution was then diluted with ISOPAR-E or toluene to achieve the amount required for polymerization and drawn into a syringe for transfer to the catalyst injection tank.

[0075] In a typical polymerization, ISOPAR-E and 1-octene are loaded into the reactor via separate flow meters. The silane monomer is then added via an injection tank input through an adjacent glove box. After the addition of solvent / comonomer, hydrogen is added (if necessary) while the reactor is heated to a polymerization set point of 120°C. Ethylene is then added to the reactor via a flow meter at the desired reaction temperature to maintain a predetermined reaction pressure set point. The catalyst solution is transferred to an injection tank via a syringe and then added to the reactor via a high pressure nitrogen stream after the reactor pressure set point is reached. The run timer is started upon injection of the catalyst, after which an exotherm and a decrease in reactor pressure are observed to indicate a successful run.

[0076] Ethylene is then added using a pressure controller to maintain the reaction pressure set point in the reactor. The polymerization runs to set ethylene absorption, after which the agitator is stopped, and the bottom dump valve is opened to empty the reactor contents into a dump tank. The tank contents are poured into a tray placed in a fume hood, and the solvent is allowed to evaporate overnight. The tray containing the remaining polymer is then transferred to a vacuum oven and heated to 100 ° C under reduced pressure to remove any residual solvent. After cooling to ambient temperature, the polymer is weighed to obtain a yield / efficiency, transferred to a container for storage and submitted for analysis and testing. The polymerization conditions are shown in Table 1. The polymer properties are shown in Table 2.

[0077] Table 1: Polymerization conditions for producing HFP

[0078]

[0079] Table 2: Polymer properties

[0080]

[0081] *Mol% is based on the total moles of monomers in the polymer. 1 H NMR determination.

[0082] A ODMS = 7-octenyldimethylsilane.

[0083] B HDMS = 5-hexenyldimethylsilane.

[0084] Number average molecular weight (Mn), weight average molecular weight (Mw) and polydispersity (Mw / Mn) are determined by gel permeation chromatography (GPC) according to the gel permeation chromatography method described herein above for molecular weight.

[0085] The monomer ratio information was obtained by proton nuclear magnetic resonance spectroscopy ( 1 H NMR). The samples were dissolved in tetrachloroethane-d2 (with or without 0.001M Cr(acac)3) in 8mm NMR tubes. The concentration was about 100mg / 1.8mL. The tubes were then heated in a heating block set at 110°C. The sample tubes were repeatedly vortexed and heated to obtain a uniformly flowing fluid. The data were collected on a BRUKER AVANCE 600MHz spectrometer equipped with a 10mm C / H DUAL cryogenic probe. 1 H NMR spectroscopy. Standard single pulse 1 H NMR experiments. The following acquisition parameters were used: 70 s relaxation delay, 17.2 μs 90 degree pulse, 32 scans. The spectrum was centered at 1.3 ppm with a spectral width of 20 ppm. All measurements were performed at 110 °C without sample rotation. For the resonance peak of the solvent (residual protonated tetrachloroethane), 1 The H NMR spectrum was located at "5.99 ppm". For samples containing Cr, data were collected at "16 sec relaxation delay" and 128 scans.

[0086] The glass transition temperature (Tg) and melting temperature (Tm) were determined using differential scanning calorimetry (DSC) according to the following method: Each sample (0.5 g) was compression molded into a film at 5000 psi, 190°C for two minutes. About 5 mg to 8 mg of the film sample was weighed and placed in a DSC pan. The lid was screwed on the pan to ensure a closed atmosphere. Unless otherwise stated, the sample pan was placed in a DSC unit and then heated to a temperature of 180°C for PE at a rate of 10°C / min (to 230°C for PP). The sample was kept at this temperature for three minutes. Then, the sample was cooled to -90°C for PE at a rate of 10°C / min (to -60°C for PP) and kept isothermally at the temperature for three minutes. The sample was then heated at a rate of 10°C / min until completely melted (second heating). Unless otherwise stated, the melting point (Tm) of each polymer was 10°C / min. m ) and glass transition temperature (T g ) is determined from the second heating curve, and the crystallization temperature (T c ) is determined by the first cooling curve. Record T m and T c The corresponding peak temperature can be determined by the heat of fusion (H f ) divided by the theoretical heat of fusion of 292 J / g for PE (165 J / g for PP) and multiplying this number by 100 to calculate the percent crystallinity (e.g., % crystallinity = (Hf / 292 J / g) x 100 (for PE)). In DSC measurements, it is common to observe multiple T m peak and is recorded here as the T m The highest temperature peak.

[0087] Table 3 provides information on the materials used to prepare HFP1 and HFP2.

[0088] Table 3

[0089]

[0090]

[0091] Preparation of cross-linked elastomer and elastomer gel paste

[0092] Table 4 lists the components used to prepare the crosslinked elastomers

[0093] Table 4

[0094]

[0095] SYL-OFF is a trademark of Dow Silicones Corporation

[0096] Example 1. First, a 10.0 wt% solution of HFP1 in isododecane was prepared by adding 10 g HFP1 and 90 g isododecane to a first glass jar, sealing the jar and rolling on a three-roll drum for 48 hours to form a uniform solution. Then, 29.71 g of the uniform solution from the first glass jar was added to a second glass jar, along with 0.56 g of diallyl propylene glycol crosslinker and 29.71 g of isododecane. A stirring cross was added. The jar was placed in an 80°C hot water bath and stirring was started. Once the contents reached a temperature of 75°C-80°C, 0.12 g of catalyst was injected into the jar, and mixing continued until gelation occurred. The jar was placed in a 70°C oven for 4 hours to obtain a crosslinked elastomer Example 1.

[0097] An elastomer gel paste was prepared from Example 1 by placing 59.08 g of Example 1 in a Waring Blender and shearing for 20 seconds each at settings 1, 3, and 5 without scraping or stopping between settings. 5.91 g of isododecane was added and sheared for 30 seconds each at settings 1, 2, and 3. Good mixing was ensured between settings. The resulting material was an elastomer gel paste of Example 1 having an average particle size of 45 microns for the solvent swollen Example 1 crosslinked elastomer.

[0098] Example 2. First, a 10.0 wt% solution of HFP1 in isododecane was prepared by adding 10 g HFP2 and 90 g isododecane to a first glass jar, sealing the jar and rolling on a three-roll drum for 48 hours to form a uniform solution. Then, 20.21 g of the uniform solution from the first glass jar was added to a second glass jar, along with 0.38 g of diallyl propylene glycol crosslinker and 9.41 g of isododecane. A stirring cross was added. The jar was placed in an 80°C hot water bath and stirring was started. Once the contents reached a temperature of 75°C-80°C, 0.06 g of catalyst was injected into the jar, and mixing continued until gelation occurred. The jar was placed in a 70°C oven for 4 hours to obtain a crosslinked elastomer Example 2.

[0099] An elastomer gel paste was prepared from Example 2 by placing 26.25 g of Example 2 in a Waring blender and shearing for 20 seconds each at settings 1, 3, and 5 without scraping or stopping between settings. 6.06 g of isododecane was added and sheared for 30 seconds each at settings 1, 2, and 3. Good mixing was ensured between settings. The resulting material was the elastomer gel paste of Example 2.

[0100] Sensory evaluation

[0101] The elastomer gel paste of Example 2 and DOWSIL TM 9045 silicone elastomer blend (DOWSIL is a trademark of The Dow Chemical Company) was subjected to sensory evaluation. TM The 9045 silicone elastomer blend is recognized in the industry as having desirable silky, smooth and powdery sensory attributes and is used as a benchmark for sensory performance.

[0102] The sensory evaluation was conducted by four researchers who were familiar with cross-linked elastomeric pastes and had experience in sensory evaluation on skin. Each researcher tested the elastomer gel paste of Example 2 and DOWSIL TM 9045 silicone elastomer blends were evaluated, one sample was identified as "Sample A" and the other was identified as "Sample B". The researchers evaluated seven attributes and rated each sample on a scale of 1 to 5 for each attribute. Table 5 gives the seven attributes, equivalent materials with values ​​of 1 and 5 for each attribute (values ​​between 1 and 5 have sensory properties between the sensory properties of the equivalent materials), the ideal value of the sensory property, and the average sensory value for each sample assigned by the four researchers:

[0103] Table 5

[0104]

[0105]

[0106] The paste of Example 2 performed similarly and in some cases better than DOWSIL TM 9045 Silicone elastomer blend.

[0107] Organic solvent compatibility

[0108] By mixing 8-10 gram batches of 25 wt% of Example 1 paste or DOWSIL TM 9045 silicone elastomer blend or DOWSIL TM EL-8040 ID silicone organic blend, evaluating the elastomer gel paste of Example 1 (Example 1 paste) relative to DOWSIL TM 9045 silicone elastomer blend and DOWSIL TMSolvent compatibility of EL-8040 ID silicone organic blend with 7 different organic solvents, mixed on a speed mixer for one minute and then transferred to a clear vial. The samples were allowed to stand at 25°C for 12 hours and then evaluated for clarity and relative thickening according to the following evaluation scale. Table 6 lists the results for Example 1 and DOWSIL TM Seven solvents and results for 9045 silicone elastomer blends.

[0109] Transparency Level

[0110] A. Transparent

[0111] B Slightly turbid

[0112] C Turbid

[0113] D Turbidity

[0114] E Opaque

[0115] F Incompatible-inhomogeneous mixture

[0116] Viscosity Grade

[0117] Assess viscosity by inverting the vial and observing how the mixture flows:

[0118] 1 Liquid (equivalent to DOWSIL TM 245 fluid)

[0119] 3 Pourable (equivalent to 10,000 square millimeters per second (cst) of polydimethylsiloxane)

[0120] 5 Pourable (equivalent to 60,000 square millimeters per second (cst) of polydimethylsiloxane)

[0121] 9 Almost non-pourable (equivalent to 300,000 square millimeters per second (cSt) of polydimethylsiloxane)

[0122] 10 Does not flow when inverted.

[0123] Table 6

[0124]

[0125] Crodamol is a trademark of Croda, INC.

[0126] *NM = Not measured due to heterogeneous mixture.

[0127] The material of the present invention has better TM 9045 silicone elastomer blend or DOWSILTM 8040 silicone organic elastomer blend has a wider range of solvent compatibility, as demonstrated by obtaining homogeneous mixtures with all seven solvents. TM Thickens in more solvents than 9045 silicone elastomer blend.

[0128] Oil-in-water formulations

[0129] Use the paste of Example 1 and DOWSIL TM 9045 Silicone Elastomer Blends were evaluated for their ability to form oil-in-water systems.

[0130] An initial mixture was formed by combining the following ingredients and mixing with a marine propeller at 500 revolutions per minute (RPM), stopping as needed to scrape the sides / bottom of the beaker with a spatula until a uniform mixture was obtained: 2 g XIAMETER TM PMX-200 silicone fluid (200 square millimeters per second (centistokes) viscosity), 5 g XIAMETER PMC-0245 cyclopentasiloxane, 3.8 g Dow Corning RM 2051 thickener and 10 g of the paste of Example 1 or DOWSIL TM 9045 Silicone Elastomer Blend. XIAMETER is a trademark of Dow Corning Corporation.

[0131] In a separate container, mix 74g of water and 2g of glycerin. Add the resulting mixture as a constant stream to the initial mixture while mixing, increasing the mixing rate to 1000 RPM. While mixing, add 3g of DOWSIL TM 9509 silicone elastomer suspension (DOWSIL is a trademark of Dow Chemical Company), and then add 0.2g GLYDANT TM Plus preservative (GLYDANT is a trademark of Lonza, LLC).

[0132] With Example 1 paste and DOWSIL TM Both formulations of the 9045 silicone elastomer blend produced white lotions that demonstrated the ability to readily form an oil-in-water system. The viscosity and skin feel of the two formulations when rubbed in were similar.

[0133] Transparent sunscreen formulation

[0134] A transparent sunscreen formulation was prepared using the elastomer gel paste of Example 2 (Example 2 paste) and DOWSIL TM9045 Silicone Elastomer Blend Another clear sunscreen formulation was prepared to compare the results.

[0135] 67.45 g of the paste of Example 2 or DOWSIL TM 9045 Silicone Elastomer Blend is added to the speed mixer cup. While mixing at 2300 RPM, add each of the following components in sequence while mixing for one minute after each addition to obtain a uniform mixture: 7.5 g Octyl Methoxycinnamate, 5 g Ethylhexyl Salicylate, 8 g Crodamol TM GTCC mixed ester, 12g Cetiol TM OE emollient (Cetiol is a trademark of Cognis IPmanagement GMBH) and 0.05 g DOWSIL TM VM-2270 aerogel fine particles (average particle size of 5 microns to 15 microns, surface area of ​​600 m2 / g to 800 m2 / g, and porosity greater than 90).

[0136] Both formulations were colorless. However, only Example 2 paste was transparent and stable. TM The formulation of the 9045 silicone elastomer blend was cloudy and unstable. This shows that the materials of the present invention are capable of preparing clear sunscreen formulations, even better than DOWSIL TM 9045 silicone elastomer blend is better.

Claims

1. A composition comprising a crosslinked elastomer comprising a polyolefin backbone crosslinked by polyether chains, wherein the crosslinked elastomer has carbon-silicon-carbon bonds between the polyolefin backbone and the polyether chains, and wherein the crosslinked elastomer does not contain Si-O-Si bonds.

2. The composition of claim 1, wherein the polyolefin backbone is an interpolymer of ethylene, octene, and at least one of 7-octenyldimethylsilane and 5-hexenyldimethylsilane, and wherein the polyether chains are crosslinked by bonding to the silane.

3. The composition of claim 2, wherein the polyolefin backbone is an interpolymer consisting of polymerized monomer segments: (a) 20 to 35 mole percent of octene; (b) 65 to 80 mole percent ethylene; and (c) 1 to 10 mol % of one or any combination of more than one of 7-octenyldimethylsilane and 5-hexenyldimethylsilane.

4. A composition according to any preceding claim, wherein the polyether chain comprises polyether units selected from -RO- groups, wherein R is an alkylene group having 2 to 8 carbon atoms.

5. The composition of claim 4, wherein the polyether chain comprises polypropylene oxide.

6. A composition according to any preceding claim, wherein the crosslinked elastomer is composed of interpolymerized polymer segments composition: (a) 20 to 35 mole percent of a molecule having an average chemical structure of -CH 2 A combination of more than one of the segments of CHR'-; (b) 65 to 80 mole percent of -CH 2 CH 2 -;and (c) 1 to 10 mol% of -CH 2 CHA-; Wherein the mole percentage is relative to the mole number of the interpolymerized polymer segments in the crosslinked elastomer, R' is an alkyl group having one or more and at the same time 8 or less carbon atoms, and A has the following average chemical structure (I): -(CH 2 ) n Si(CH 3 ) 2 -B-D(I) And among them n is a value ranging from 4 to 6; B is -(CH 2 ) 3 O(RO) p’ (CH 2 ) 3 -; wherein R is an alkylene group having 2 or more and at the same time 8 or fewer carbon atoms and the subscript p' has a value in the range of 15-25; and D is another A group -Si(CH 3 ) 2 (CH 2 ) n -group.

7. A composition according to any preceding claim, wherein the composition further comprises a solvent and the cross-linked elastomer is solvent swollen, thereby becoming a solvent swollen elastomer.

8. The composition of claim 7, wherein the solvent swollen elastomer has an average particle size in the range of 1 micron to 500 microns.

9. A method for producing a composition according to claim 1, the method comprising providing a crosslinked elastomer by a hydrosilylation reaction with a reaction composition comprising: (a) Hydrosilane-functional polyolefins without Si-O-Si bonds; (b) a polyether crosslinker comprising at least two terminal alkenyl groups and no Si—O—Si bonds; (c) a hydrosilylation catalyst; and (d) Organic solvents.

10. The method of claim 9, wherein the hydrosilane-functional polyolefin is an interpolymer of: (a) 20 to 35 mole percent of 1-octene; (b) 65 to 80 mole percent ethylene; and (c) 1 to 10 mol % of one or any combination of 7-octenyldimethylsilane and 5-hexenyldimethylsilane, The mole percentages are relative to the total moles of 1-octene, ethylene, 7-octenyldimethylsilane and 5-hexenyldimethylsilane.