Method for producing graphene

By using a heating source to heat the carbon base and supply components in a high vacuum environment, the sublimation of silicon atoms is suppressed, and the problem of difficulty in controlling graphene lamination at low temperatures is solved, and the uniform stacking and crystallization defects of graphene layer are achieved. avoid.

CN118922380APending Publication Date: 2024-11-08ROHM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380029753.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When heating the silicon carbide substrate in a high vacuum environment, low temperatures will lead to excessive thermal decomposition and sublimation of silicon atoms, making it difficult to control the stacking of graphene, which may cause crystallization defects.

Method used

By placing a semiconductor substrate on a carbon base and heating the carbon base and the supply member using at least one heating source, sublimation of silicon atoms is suppressed to form a uniform graphene layer. The supply member may be a silicon nitride substrate or a nitride film, which provides silicon and nitrogen atoms by heating, adjusts the atmosphere on the substrate, inhibits the sublimation of silicon atoms and controls the growth of graphene.

Benefits of technology

A uniform stacking of graphene layers is achieved, which avoids the occurrence of crystallization defects and improves the stacking control accuracy of graphene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922380A_ABST
    Figure CN118922380A_ABST
Patent Text Reader

Abstract

A method for producing graphene in which a semiconductor substrate is placed on a carbon susceptor, a supply member is placed on the carbon susceptor or above the semiconductor substrate, the supply member and the carbon susceptor are heated by at least one of a first heating source and a second heating source, and the semiconductor substrate is heated by heating the carbon susceptor. And forming one or more graphene layers on the semiconductor substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This embodiment relates to a method for manufacturing graphene. Background Art

[0002] It is known that in the method for producing graphene, a silicon carbide substrate is formed at 1×10 -1 ~1×10 -5 Pa, silicon (Si) atoms sublime and the remaining carbon (C) elements self-organize to form graphene stacked on the silicon carbide substrate.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent document 1: International Publication No. 2010 / 023934. Summary of the invention

[0006] Problems to be solved by the invention

[0007] However, when the SiC substrate is placed at 1×10 -1 ~1×10 -5 When heating in a high vacuum of 1000 Pa, thermal decomposition occurs at low temperatures, so that silicon atoms sublimate violently, making it difficult to control the stacking of graphene, which may cause crystal defects.

[0008] Technical solutions to the problem

[0009] The present invention provides a method for manufacturing graphene by stacking to form uniform graphene.

[0010] According to one aspect of the present embodiment, a method for manufacturing graphene is provided, wherein a semiconductor substrate is placed on a carbon base, a supply component is placed above the carbon base or the semiconductor substrate, the supply component and the carbon base are heated by at least one of a first heating source and a second heating source, the semiconductor substrate is heated by heating the carbon base, and one or more graphene layers are formed on the semiconductor substrate.

[0011] Effects of the Invention

[0012] According to the present embodiment, a method for producing graphene by stacking uniformly can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a cross-sectional view of graphene on a semiconductor substrate formed by the manufacturing method of the first embodiment.

[0014] Figure 2 This is a cross-sectional view showing one step of the process of producing graphene according to the first embodiment.

[0015] Figure 3A It means next Figure 2 A cross-sectional view of a process.

[0016] Figure 3B yes Figure 3A Top view of the .

[0017] Figure 4 It means next Figure 3A A cross-sectional view of a process.

[0018] Figure 5 It is a cross-sectional view showing one step of the process of producing graphene according to the second embodiment.

[0019] Fig. 6A It means next Figure 5 A cross-sectional view of a process.

[0020] Figure 6B yes Fig. 6A Top view of the .

[0021] Figure 7 It means next Fig. 6A A cross-sectional view of a process.

[0022] Figure 8 It is a cross-sectional view showing one step of the process of producing graphene according to a modification of the second embodiment. DETAILED DESCRIPTION

[0023] Next, the present embodiment will be described with reference to the accompanying drawings. In the description of the drawings described below, the same or similar parts are marked with the same or similar reference numerals. However, the drawings are only schematic, and it should be noted that the relationship between the thickness and plane dimensions of each component is different from the actual situation. Therefore, the specific thickness and size should be determined by referring to the following description. In addition, of course, the drawings also include parts with different dimensional relationships and proportions.

[0024] In addition, the embodiments described below exemplify devices and methods for realizing technical ideas, and do not specify the material, shape, structure, arrangement, etc. of each component. Various modifications can be added to the technical scheme of this embodiment.

[0025] [First embodiment]

[0026] The method for producing graphene according to the first embodiment will be described with reference to the drawings.

[0027] Figure 1 1 is a cross-sectional view of a graphene layer 10 on a semiconductor substrate 1 formed by the manufacturing method of the first embodiment.

[0028] like Figure 1As shown, the semiconductor substrate 1 has a first main surface 1a and a second main surface 1b on the opposite side of the first main surface 1a. As the semiconductor substrate 1, for example, single crystal silicon carbide (SiC) can be applied. In the following description, the semiconductor substrate 1 is also referred to as the SiC substrate 1. In addition, the SiC substrate 1 can be either a silicon terminal surface or a carbon terminal surface on the first main surface 1a. In addition, the thickness of the SiC substrate 1 is not limited, for example, it can also be 350μm.

[0029] The graphene layer 10 has a single-layer structure or a stacked structure of multiple layers or more. The graphene layer 10 is disposed on the SiC substrate 1. Here, multiple layers refers to two or more graphene layers 10.

[0030] Next, an example of the method for producing graphene according to the first embodiment will be described.

[0031] Figures 2 to 4 This is a cross-sectional view showing one step of the process of producing graphene according to the first embodiment.

[0032] First, on the first main surface 1 a of the SiC substrate 1 , a natural oxide film (not shown) is removed from the SiC substrate 1 using hydrofluoric acid.

[0033] Then, if Figure 2 As shown, the SiC substrate 1 is placed on the carbon base 2. Specifically, the diameter L2 of the carbon base 2 is longer than the diameter L1 of the SiC substrate 1. In addition, the thickness of the carbon base 2 is, for example, about 500 μm. The carbon base 2 is a general term for a substrate holder of a semiconductor substrate that is heated using, for example, an infrared lamp annealing device (RTA: Rapid Thermal Annealing).

[0034] Then, if Figure 3A As shown, a supply component 3 is placed above the carbon base 2. Specifically, the supply component 3 is arranged at a distance from the SiC substrate 1. The supply component 3 has silicon (Si) atoms and nitrogen (N) atoms. Specifically, the supply component 3 can be applied to a silicon nitride (Si3N4) substrate, for example. The silicon nitride substrate is formed by, for example, powder sintering. Silicon atoms and nitrogen atoms are sublimated by heating the supply component 3. Since silicon atoms and nitrogen atoms are supplied from the supply component 3, sublimation of silicon atoms from the SiC substrate 1 can be suppressed. In the following description, the supply component 3 is also referred to as the Si3N4 substrate 3.

[0035] like Figure 3A As shown in FIG. 1 , the diameter L3 of the Si3N4 substrate 3 is longer than the diameter L1 of the SiC substrate 1. Figure 3BAs shown, when looking down at the first main surface 1a of the SiC substrate 1, the area of ​​the carbon base 2 or the supply component 3 is larger than the area of ​​the SiC substrate 1. In addition, the thickness t1 of the Si3N4 substrate 3 is, for example, about 0.5 to 5 mm. The distance d1 between the SiC substrate 1 and the Si3N4 substrate 3 can also be, for example, about 1 to 5 cm. Here, the distance d1 between the SiC substrate 1 and the Si3N4 substrate 3 is a distance at which the first main surface 1a of the SiC substrate 1 can be adjusted to an atmosphere containing silicon atoms and nitrogen atoms by heating to sublimate the silicon atoms and nitrogen atoms contained in the Si3N4 substrate 3. In addition, as Figure 3B As shown, the SiC substrate 1 has an orientation flat surface 1 c.

[0036] Then, if Figure 4 As shown, it is introduced into a chamber having a first heating source 4 and a second heating source 5 to be heated. Specifically, the supply component 3 and the carbon base 2 are heated by at least one of the first heating source 4 and the second heating source 5. In addition, the first heating source 4 and the second heating source 5 are arranged at a distance. In addition, the carbon base 2, the SiC substrate 1 and the supply component 3 are arranged between the first heating source 4 and the second heating source 5. In addition, infrared lamps can be applied to the first heating source 4 and the second heating source 5. That is, the chamber having the first heating source 4 and the second heating source 5 can, for example, be applied with an infrared lamp annealing device. In addition, the infrared lamp annealing device can also exhaust the atmospheric components in the chamber after introduction, and then heat it. In addition, the pressure after exhausting the atmospheric components in the chamber only needs to be 1×10 -6 ~1×10 6 Alternatively, after exhausting the atmospheric components in the chamber, argon (Ar) gas may be supplied to perform heating.

[0037] The SiC substrate 1 is heated by heating the carbon base 2. Specifically, the heating temperature of the first heating source 4 and the second heating source 5 can be about 1000°C to 2300°C. In addition, the lamp outputs of the first heating source 4 and the second heating source 5 do not need to be equal and can be different. Here, the lamp output of the first heating source 4 and the second heating source 5 refers to, for example, the infrared lamp output of an infrared lamp annealing device. In addition, the heating conditions of the carbon base 2 and the Si3N4 substrate 3 can be, for example, about 1600°C and 10 minutes. Here, the heating conditions of the carbon base 2 and the Si3N4 substrate 3 refer to the temperature at which silicon atoms of the SiC substrate 1 sublimate and silicon atoms and nitrogen atoms of the Si3N4 substrate 3 sublimate.

[0038] In the case where heating is performed by the first heating source 4 and the second heating source 5, as Figure 4As shown, the carbon base 2 and the Si3N4 substrate 3 are heated simultaneously. By heating, silicon atoms and nitrogen atoms in the Si3N4 substrate 3 are sublimated and supplied to the first main surface 1a of the SiC substrate 1. Therefore, the sublimation of silicon atoms from the SiC substrate 1 is suppressed, and the growth rate of the graphene layer 10 is suppressed. By suppressing the growth rate of the graphene layer 10, the occurrence of step aggregation can be suppressed.

[0039] By heating the SiC substrate 1, one or more graphene layers 10 are formed on the SiC substrate 1. Specifically, Si is sublimated from the first main surface 1a of the SiC substrate 1, and the graphene layer 10 is formed on the SiC substrate 1. In addition, the Si3N4 substrate 3 can also be used to add sublimated nitrogen atoms to the SiC substrate 1 or one or more layers of the graphene layer 10 formed on the SiC substrate 1.

[0040] Through the above steps, the graphene layer 10 of the first embodiment is completed.

[0041] According to the first embodiment, by supplying silicon atoms and nitrogen atoms from the Si3N4 substrate 3 using the first heating source 4 and the second heating source 5, sublimation of silicon atoms of the SiC substrate 1 can be suppressed, and a uniformly stacked graphene layer 10 can be formed on the SiC substrate 1.

[0042] [Second embodiment]

[0043] The graphene production method according to the second embodiment will be described with reference to the drawings.

[0044] Figures 5 to 7 It is a cross-sectional view showing one step of the process of producing graphene according to the second embodiment.

[0045] In the manufacturing process of graphene of the second embodiment, a nitride film (Si3N4) 3A is provided instead of the Si3N4 substrate 3, which is an example of a supply component in the manufacturing process of graphene of the first embodiment. The nitride film 3A is another example of a supply component. Here, the nitride film 3A refers to a film having silicon atoms and nitrogen atoms, for example, also referred to as a silicon nitride film, silicon nitride, or silicon nitride (SiN). In the following description, the nitride film 3A, which is another example of a supply component, is described. Hereinafter, the description of the same process as the first embodiment is omitted.

[0046] First, if Figure 5As shown, a nitride film 3A is formed on the SiC substrate 1. Specifically, as for the film forming method of the nitride film 3A, for example, plasma chemical vapor deposition (plasma CVD: Chemical Vapor Deposition), thermal chemical vapor deposition (thermal CVD), atomic layer deposition (ALD: Atomic Layer Deposition) and the like can be cited. In addition, as for the film forming method of the nitride film 3A, the ALD method is preferred because it can form a regular and uniform film along the first main surface 1a on the SiC substrate 1.

[0047] The film thickness t2 of the nitride film 3A only needs to be, for example, about 1 to 5 nm. That is, the film thickness t2 of the nitride film 3A only needs to be a film thickness to the extent that the silicon atoms and nitrogen atoms are sublimated by heating and the nitride film 3A disappears. In addition, in the manufacturing process of graphene in the first embodiment, the SiC substrate 1 and the Si3N4 substrate 3 are arranged at a distance d1, but in the manufacturing process of graphene in the second embodiment, the SiC substrate 1 and the nitride film 3A are arranged in contact. That is, the distance d2 between the SiC substrate 1 and the nitride film 3A is 0, and the SiC substrate 1 and the nitride film 3A can also be directly in contact.

[0048] Then, if Fig. 6A As shown in FIG. 1 , a SiC substrate 1 is placed on a carbon base 2A, which is an example of a carbon base. Specifically, a diameter L2A of the carbon base 2A is longer than a diameter L1 of the SiC substrate 1. In addition, a diameter L3A of the nitride film 3A is equal to a diameter L1 of the SiC substrate 1. That is, Figure 6B As shown in FIG. 1 , when the first main surface 1a of the SiC substrate 1 is viewed from above, the area of ​​the carbon base 2A is larger than the area of ​​the SiC substrate 1. In addition, the area of ​​the nitride film 3A is equal to the area of ​​the SiC substrate 1. Although not shown in the figure, when the first main surface 1a of the SiC substrate 1 is viewed from above, the area of ​​the carbon base 2A may be equal to the area of ​​the SiC substrate 1. In addition, as Figure 6B As shown, the SiC substrate 1 has an orientation flat surface 1 c.

[0049] Then, if Figure 7 As shown, it is introduced into a chamber having a first heating source 4 and a second heating source 5 for heating. Specifically, the first heating source 4 and the second heating source 5 are arranged at a distance. In addition, a carbon base 2, a SiC substrate 1 and a supply component 3 are arranged between the first heating source 4 and the second heating source 5. In addition, infrared lamps can be applied to the first heating source 4 and the second heating source 5. That is, the chamber having the first heating source 4 and the second heating source 5 can, for example, be applied with an infrared lamp annealing device. In addition, the infrared lamp annealing device can also exhaust the atmospheric components in the chamber after introduction and then heat. In addition, the pressure after exhausting the atmospheric components in the chamber only needs to be 1×10 -6 ~1×106 Alternatively, after exhausting the atmospheric components in the chamber, argon (Ar) gas may be supplied to perform heating.

[0050] The SiC substrate 1 is heated by heating the carbon base 2A. Specifically, the heating temperature of the first heating source 4 and the second heating source 5 can be about 1000°C to 2300°C. In addition, the lamp outputs of the first heating source 4 and the second heating source 5 do not need to be equal and can be different. Here, the lamp output of the first heating source 4 and the second heating source 5 refers to, for example, the infrared lamp output of an infrared lamp annealing device. In addition, the heating conditions of the carbon base 2A and the nitride film 3A can also be, for example, about 1600°C and 10 minutes. Here, the heating conditions of the carbon base 2A and the nitride film 3A refer to the temperature at which silicon atoms of the SiC substrate 1 sublimate, silicon atoms and nitrogen atoms of the nitride film 3A sublimate, and the entire nitride film 3A sublimate.

[0051] In the case of heating by the first heating source 4 and the second heating source 5, as Figure 7 As shown, the carbon base 2A and the nitride film 3A are heated at the same time. By heating, silicon atoms and nitrogen atoms in the nitride film 3A sublime and are supplied to the first main surface 1a of the SiC substrate 1. Therefore, the sublimation of silicon atoms from the SiC substrate 1 is suppressed, and the growth rate of the graphene layer 10 is suppressed. By suppressing the growth rate of the graphene layer 10, the occurrence of step aggregation can be suppressed.

[0052] By heating the SiC substrate 1, one or more graphene layers 10 are formed on the SiC substrate 1. Specifically, Si sublimates from the first main surface 1a of the SiC substrate 1, and the graphene layer 10 is formed on the SiC substrate 1. In addition, the sublimated nitrogen atoms can also be added to the SiC substrate 1 or one or more layers of the graphene layer 10 formed on the SiC substrate 1 by using the nitride film 3A.

[0053] Through the above steps, the graphene layer 10 of the second embodiment is completed.

[0054] According to the second embodiment, silicon atoms and nitrogen atoms are supplied from the nitride film 3A using the first heat source 4 and the second heat source 5 , so that sublimation of silicon atoms in the SiC substrate 1 can be suppressed and a uniformly stacked graphene layer 10 can be formed on the SiC substrate 1 .

[0055] [Modification of the Second Embodiment]

[0056] A method for producing graphene according to a modification of the second embodiment will be described with reference to the drawings.

[0057] Figure 8 It is a cross-sectional view showing one step of the process of producing graphene according to the modification example of the second embodiment.

[0058] like Figure 8 As shown, in the manufacturing process of graphene of the second embodiment modification, heating is performed by the first heating source 4 instead of the first heating source 4 and the second heating source 5 in the manufacturing process of graphene of the second embodiment. That is, the carbon base 2A and the nitride film 3A are heated simultaneously by the first heating source 4. Hereinafter, the other manufacturing methods and other effects of the second embodiment are the same, and therefore the description thereof is omitted.

[0059] (Other embodiments)

[0060] As described above, an embodiment is described, but the discussion and drawings as part of the disclosure are only illustrative and should not be understood as limiting. According to the present disclosure, a person skilled in the art will know various alternative embodiments, examples and application techniques. Thus, the present embodiment includes various embodiments not described herein, etc.

[0061] <Example of Implementation>

[0062] Examples of this embodiment are given below. This embodiment is not limited to the following examples.

[0063] [Supplementary Note 1]

[0064] A method for producing graphene, wherein:

[0065] A semiconductor substrate is placed on a carbon base.

[0066] placing a supply component above the carbon base or the semiconductor substrate,

[0067] The supply component and the carbon base are heated by at least one of a first heating source and a second heating source,

[0068] The semiconductor substrate is heated by heating the carbon base.

[0069] One or more graphene layers are formed on the semiconductor substrate.

[0070] [Appendix 2]

[0071] The method for producing graphene according to [Supplement 1], wherein:

[0072] The supply member comprises silicon atoms and nitrogen atoms,

[0073] The silicon atoms and the nitrogen atoms are sublimated by heating the supply member.

[0074] The semiconductor substrate is adjusted to an atmosphere containing silicon atoms and nitrogen atoms.

[0075] 〔Supplementary Note 3〕

[0076] The method for producing graphene according to [Supplement 1] or [Supplement 2], wherein:

[0077] The supply member is arranged at a distance from the semiconductor substrate.

[0078] [Appendix 4]

[0079] The method for producing graphene according to [Supplementary Note 3], wherein:

[0080] The distance between the semiconductor substrate and the supply member is 1 to 5 cm.

[0081] 〔Appendix 5〕

[0082] The method for producing graphene according to [Supplementary Note 3], wherein:

[0083] The thickness of the supply member is 0.5 to 5 mm.

[0084] [Appendix 6]

[0085] The method for producing graphene according to [Supplementary Note 3], wherein:

[0086] The supply component is a silicon nitride substrate.

[0087] [Appendix 7]

[0088] The method for producing graphene according to [Supplement 1] or [Supplement 2], wherein:

[0089] The supply component is arranged in contact with the semiconductor substrate.

[0090] [Appendix 8]

[0091] The method for producing graphene according to [Supplementary Note 7], wherein:

[0092] The supply member has a thickness of 1 to 5 nm.

[0093] 〔Supplementary Note 9〕

[0094] The method for producing graphene according to [Supplementary Note 7], wherein:

[0095] The supply member is a nitride film.

[0096] [Appendix 10]

[0097] The method for producing graphene according to any one of [Supplement 1] to [Supplement 9], wherein:

[0098] When the first main surface of the semiconductor substrate is viewed in plan, an area of ​​the carbon base or the supply member is larger than an area of ​​the semiconductor substrate.

[0099] [Supplementary Note 11]

[0100] The method for producing graphene according to any one of [Supplement 1] to [Supplement 9], wherein:

[0101] When the first main surface of the semiconductor substrate is viewed in plan, the area of ​​the carbon base or the supply member is equal to the area of ​​the semiconductor substrate.

[0102] [Appendix 12]

[0103] The method for producing graphene according to any one of [Appendix 1] to [Appendix 11], wherein:

[0104] The semiconductor substrate is formed of single-crystal silicon carbide.

[0105] [Appendix 13]

[0106] The method for producing graphene according to any one of [Supplement 1] to [Supplement 12], wherein:

[0107] The sublimated nitrogen atoms are added to the semiconductor substrate or one or more layers of the graphene layer formed on the semiconductor substrate by using the supply member.

[0108] [Appendix 14]

[0109] The method for producing graphene according to any one of [Appendix 1] to [Appendix 13], wherein:

[0110] The lamp outputs of the first heating source and the second heating source are equal.

[0111] [Appendix 15]

[0112] The method for producing graphene according to any one of [Appendix 1] to [Appendix 13], wherein:

[0113] The first heating source and the second heating source have different lamp outputs.

[0114] [Appendix 16]

[0115] The method for producing graphene according to any one of [Appendix 1] to [Appendix 15], wherein:

[0116] The carbon base, the semiconductor substrate, and the supply member are arranged between the first heating source and the second heating source.

[0117] According to [Appendix 1] to [Appendix 16], by supplying silicon atoms and nitrogen atoms from the supply member, sublimation of silicon atoms in the semiconductor substrate is suppressed, and a uniformly stacked graphene layer can be formed on the semiconductor substrate.

[0118] Description of Reference Numerals

[0119] 1 Semiconductor substrate

[0120] 2 Carbon base

[0121] 3 Supply components

[0122] 4. First heating source

[0123] 5 Second heating source

[0124] 10 Graphene layers

[0125] 1a First main surface

[0126] 1b Second main surface

Claims

1. A method for producing graphene, characterized in that: A semiconductor substrate is placed on a carbon base. placing a supply component above the carbon base or the semiconductor substrate, heating the supply member and the carbon susceptor by at least one of a first heating source and a second heating source, The semiconductor substrate is heated by heating the carbon base, One or more graphene layers are formed on the semiconductor substrate.

2. The method for producing graphene according to claim 1, characterized in that: The supply member has silicon atoms and nitrogen atoms, The silicon atoms and the nitrogen atoms are sublimated by heating the supply member, The semiconductor substrate is adjusted to an atmosphere containing silicon atoms and nitrogen atoms.

3. The method for producing graphene according to claim 1 or 2, characterized in that: The supply member is arranged at a distance from the semiconductor substrate.

4. The method for producing graphene according to claim 3, characterized in that: The distance between the semiconductor substrate and the supply component is 1 to 5 cm.

5. The method for producing graphene according to claim 3, characterized in that: The thickness of the supply component is 0.5-5 mm.

6. The method for producing graphene according to claim 3, characterized in that: The supply component is a silicon nitride substrate.

7. The method for producing graphene according to claim 1 or 2, characterized in that: The supply component is arranged in contact with the semiconductor substrate.

8. The method for producing graphene according to claim 7, characterized in that: The supply member has a thickness of 1 to 5 nm.

9. The method for producing graphene according to claim 7, characterized in that: The supply member is a nitride film.

10. The method for producing graphene according to claim 1, characterized in that: When the first main surface of the semiconductor substrate is viewed in plan, the area of ​​the carbon base or the supply member is larger than the area of ​​the semiconductor substrate.

11. The method for producing graphene according to claim 1, characterized in that: When the first main surface of the semiconductor substrate is viewed in plan, the area of ​​the carbon base or the supply member is equal to the area of ​​the semiconductor substrate.

12. The method for producing graphene according to claim 1, characterized in that: The semiconductor substrate is formed of single-crystal silicon carbide.

13. The method for producing graphene according to claim 1, characterized in that: The sublimated nitrogen atoms are added to the semiconductor substrate or one or more layers of the graphene layer formed on the semiconductor substrate using the supply member.

14. The method for producing graphene according to claim 1, characterized in that: The lamp outputs of the first heating source and the second heating source are equal.

15. The method for producing graphene according to claim 1, characterized in that: The first heating source and the second heating source have different lamp outputs.

16. The method for producing graphene according to claim 1, characterized in that: The carbon susceptor, the semiconductor substrate, and the supply member are arranged between the first heating source and the second heating source.

Citation Information

Patent Citations

  • Method for producing graphene / sic composite material and graphene / sic composite material obtained by same