Polypropylene-based heat-shrinkable film

By adjusting the composition of polypropylene resin and the tensile heat treatment technology, the problems of insufficient shrinkage properties of the heat-shrinkable film at low temperatures and poor openness of the perforated wire are solved, and efficient PET bottle recycling and reuse are achieved.

CN118922482APending Publication Date: 2024-11-08TOYOBO CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202280094117.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-20
Filing Date
2022-08-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing heat-shrinkable polypropylene films lack sufficient shrinkage at low temperatures, have a large natural shrinkage rate, and have poor perforated wire opening, which affects the recycling and reuse efficiency of PET bottles.

Method used

By adjusting the composition of the polypropylene resin, the specific gravity of the film is controlled to be between 0.87-0.95, high shrinkage rate and excellent natural shrinkage at 90°C, and the perforated wire opening is improved through stretching and heat treatment techniques.

Benefits of technology

It achieves high shrinkage, excellent perforated wire opening and small natural shrinkage, which improves the recycling and reuse efficiency of PET bottles and reduces the burden on floating and sinking separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922482A_ABST
    Figure CN118922482A_ABST
Patent Text Reader

Abstract

Provided is a heat-shrinkable polypropylene film having a specific gravity of 0.95 or less, excellent low-temperature shrinkage, small natural shrinkage, and excellent perforation line unsealing properties. Provided is a polypropylene-based heat-shrinkable film which is a stretched film comprising a polypropylene-based resin composition and which is characterized by satisfying the following requirements (1)-(4) and the like. (1) When the film is immersed in 90 DEG C hot water for 10 seconds, the hot-water thermal shrinkage is 40-80% in the width direction of the film. (2) The hot-water thermal shrinkage rate when the film is immersed in 90 DEG C hot water for 10 seconds is from 1% to 12% (inclusive) in the longitudinal direction of the film. (3) The specific gravity of the film is from 0.87 to 0.95 (inclusive). And (4) the right-angle tear strength in the longitudinal direction per unit thickness after being shrunk by 10% in the width direction in hot water at 80 DEG C is 100 mN / mm or more and 330 mN / mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polypropylene-based heat-shrinkable film suitable for a heat-shrinkable label, a label using the film, and a package using the label. Background Art

[0002] Heat-shrinkable films are widely used as labels for the contents of glass bottles and plastic bottles to prevent stains and tampering, and to protect both packaged items and commodities. In particular, the most common use is for labeling PET bottles for beverages. Usually, when heat-shrinkable films are formed into labels and installed on PET bottles, the PET bottles covered with labels are conveyed to a tunnel filled with steam in a pipeline attached to a conveyor, and steam is blown in the tunnel to heat the film to about 70°C to 100°C, thereby shrinking it for installation. Therefore, films made by stretching polyester, polystyrene, and polyvinyl chloride, which have excellent heat shrinkability at low temperatures, are widely used.

[0003] On the other hand, PET bottles for beverages are attracting attention as a renewable resource. PET bottles are collected after use and recycled into resin for remolding, but labels need to be separated from bottles because they use plastics different from those used for PET bottles and because they are printed.

[0004] That is, if the label is mixed in, the quality of the PET bottle will be reduced when it is recycled. Therefore, it is necessary to peel the label from the bottle and reuse it, but in fact, there are many cases where the label is not peeled off and is directly recycled. At present, it is necessary for the recycler to peel them off, which increases the burden of recycling. This is because the difference in specific gravity between polystyrene, polyester, polyvinyl chloride and PET bottles is small, so it is difficult to separate them in water. Floating and sinking separation based on specific gravity difference is extremely easy in industry, especially since the specific gravity of PET bottles is about 1.3 or more, and the specific gravity of the label can be separated based on water as long as the specific gravity is less than 1.0. If such a label is used, even if the label is mixed in when the PET bottle is recycled, it can be classified very efficiently. Therefore, not only can the burden during recycling be greatly reduced, but also the quality of the recycled resin obtained from the recycled PET bottles can be improved.

[0005] In this case, polypropylene has a specific gravity as light as about 0.9, and can achieve floating separation with PET based on water, so there is expectation for its use, but there is a problem that the shrinkage at 90°C required for shrinkage under steam is insufficient. In addition, compared with polyester and polystyrene, there are problems such as large post-shrinkage (natural shrinkage) at room temperature, changes in film size, and easy deformation in the wound state of the film, which causes printing misalignment and wrinkles during secondary processing.

[0006] In order to improve the shrinkage property, various proposals have been made so far.

[0007] For example, in Patent Document 1, petroleum resin and cyclic polyolefin resin with a high glass transition temperature are added to improve low-temperature shrinkage and reduce natural shrinkage. However, due to the addition of resin with a high glass transition temperature, the shrinkage at 90°C is still insufficient, and the shrinkage finishing is poor. In addition, if petroleum resin and cyclic olefin are added, the specific gravity increases, which reduces the efficiency of floating and sinking separation. In addition, polypropylene is softer than polyester and polystyrene, and therefore has the characteristic of strong viscosity when torn along the perforation line. Furthermore, the above-mentioned film is a film that is stretched only in the width direction, and therefore, there is a problem that the perforation line of the so-called label is not easy to tear along the perforation line in the direction orthogonal to the main shrinkage direction, that is, the length direction. The opening property is poor.

[0008] In addition, Patent Document 2 proposes a film in which the molecular weight distribution of polypropylene is controlled to be small or laminated with a non-crystalline resin having a high glass transition temperature such as a cyclic olefin resin in order to reduce the natural shrinkage. However, the shrinkage of these films at low temperatures (90° C.) is insufficient for the shrinkage required for beverage labels. In addition, as mentioned above, there is the problem of the large specific gravity of cyclic olefin resins.

[0009] Patent Document 3 states that low-temperature stretching is possible by adding petroleum resin and polyethylene, thereby improving low-temperature shrinkage. However, if petroleum resin is added, the specific gravity increases, which not only reduces the efficiency of floating and sinking separation, but also the film obtained by stretching at low temperature has a large post-shrinkage (natural shrinkage) at room temperature, which makes it easy to cause the film size to change, or the film in the wound state to deform, causing printing misalignment and wrinkles during secondary processing.

[0010] On the other hand, the inventors found that stretching is performed not only in the width direction but also in the length direction, thereby improving the opening property of the perforated line in the length direction, but the shrinkage rate in the length direction orthogonal to the main shrinkage direction will also increase, and when the label is formed and shrunk and installed, there is a problem that the strain of the label (so-called longitudinal shrinkage) will increase. Furthermore, the natural shrinkage in the length direction will increase due to stretching, and for the film in the rolled state, there is also the problem that deformation and relaxation caused by the shrinkage of the roll are easy to occur during storage.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent No. 4380330

[0014] Patent Document 2: Japanese Patent No. 4574462

[0015] Patent Document 3: Japanese Patent No. 5690103 Summary of the invention

[0016] Problem that the invention aims to solve

[0017] The present invention aims to overcome the above problems and to provide a heat-shrinkable polypropylene film having a specific gravity of 0.95 or less, excellent low-temperature shrinkage, small natural shrinkage, and excellent perforation line opening properties.

[0018] Solutions for solving problems

[0019] The present inventors have conducted intensive studies and, as a result, have found that the above-mentioned problems can be solved by the means described below, thereby arriving at the present invention.

[0020] That is, the present invention includes the following configurations.

[0021] 1. A polypropylene-based heat-shrinkable film, characterized in that it is a stretched film composed of a polypropylene-based resin composition and satisfies the following (1) to (7).

[0022] (1) When the film is immersed in hot water at 90° C. for 10 seconds, the hot water heat shrinkage ratio in the width direction of the film is 40% or more and 80% or less.

[0023] (2) When the film is immersed in hot water at 90° C. for 10 seconds, the hot water heat shrinkage ratio in the longitudinal direction of the film is 1% or more and 12% or less.

[0024] (3) The specific gravity of the film is 0.87 or more and 0.95 or less.

[0025] (4) a right-angle tear strength in the longitudinal direction per unit thickness after shrinking by 10% in the width direction in hot water at 80°C of 100 mN / mm or more and 330 mN / mm or less,

[0026] (5) The difference Ny-Nx between the refractive index in the width direction (Ny) and the refractive index in the length direction (Nx) is 0.005 or more and 0.028 or less.

[0027] (6) The natural shrinkage rate in the width direction of the polypropylene-based heat-shrinkable film after aging for 672 hours in an atmosphere of 40° C. and 65% RH is 0.1% or more and 3.0% or less.

[0028] (7) The natural shrinkage rate in the longitudinal direction of the polypropylene-based heat-shrinkable film after aging for 672 hours in an atmosphere of 40° C. and 65% RH is 0.1% or more and 1.0% or less.

[0029] 2. The polypropylene heat-shrinkable film according to 1., wherein the value obtained by dividing the maximum tensile stress in the range of 0 to 10% of elongation in a tensile test in the longitudinal direction by the tensile stress at an elongation of 30% is 0.5 or more and 1.9 or less.

[0030] 3. The polypropylene-based heat-shrinkable film according to 1. or 2., wherein the haze of the film is 1% to 12%.

[0031] 4. The polypropylene heat-shrinkable film according to any one of 1. to 3., characterized in that it has one or more melting peak temperatures measured by a differential scanning calorimeter in the range of 70°C to 100°C and in the range of more than 100°C to 170°C.

[0032] 5. The polypropylene-based heat-shrinkable film according to any one of 1. to 4., characterized in that the irreversible heat flow measured by a temperature modulation scanning calorimeter has a peak in the range of 20°C to 60°C, and the endothermic amount of the peak is 0.3 J / g to 0.95 J / g.

[0033] 6. The polypropylene-based heat-shrinkable film according to any one of 1. to 5., wherein the refractive index Ny in the width direction is 1.490 or more and 1.530 or less.

[0034] 7. The polypropylene heat-shrinkable film according to any one of 1. to 6., wherein the thickness of the polypropylene heat-shrinkable film is 12 μm or more and 100 μm or less.

[0035] 8. The polypropylene heat-shrinkable film according to any one of 1. to 7., wherein the polypropylene resin composition constituting the polypropylene heat-shrinkable film contains ethylene or 1-butene as a copolymer component.

[0036] 9. A label comprising the polypropylene heat-shrinkable film according to any one of 1. to 8. as a base material and provided with a perforated line or a pair of incisions.

[0037] 10. A packaging body characterized by having a label formed by forming the polypropylene heat-shrinkable film according to any one of 1. to 8. into a ring shape on at least a part of the outer periphery of a packaging object.

[0038] 11. A packaging body, characterized in that the label described in 9. above is provided on at least a portion of the outer periphery of an object to be packaged.

[0039] Effects of the Invention

[0040] The polypropylene-based heat-shrinkable film of the present invention has a high shrinkage rate at 90°C, and can not only present a good finish without wrinkles or insufficient shrinkage as a beverage label, but also has excellent perforation line opening properties, and furthermore, the natural shrinkage rate in both the width direction and the length direction is small, so that the film is stored for a period of time and the dimensional change and wrinkle generation are small, and the practicality is excellent. In addition, due to the small specific gravity, the floating and sinking separation from the PET bottle can be performed efficiently, and therefore, the recyclability is excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is an explanatory diagram showing the shape of a test piece in the measurement of right-angle tear strength (it should be noted that the unit of the length of each part of the test piece in the figure is mm). DETAILED DESCRIPTION

[0042] The polypropylene-based heat-shrinkable film obtained by stretching the polypropylene resin composition used in the present invention preferably has at least one melting point (melting peak temperature) measured by a differential scanning calorimeter (DSC) in the range of 70°C to 100°C and in the range of more than 100°C to 170°C. The heat-shrinkable film for PET bottle labels is usually heated and shrunk at a temperature of 70°C to 100°C by steam, so it has a melting point in the range of 70°C to 100°C, so that the oriented crystals in the partially stretched film melt and the shrinkage characteristics are reflected. On the other hand, it is preferred to have a melting point in the range of 100°C to 170°C, so that the heat resistance can be improved and the welding and adhesion during heating can be suppressed. In addition, it is more preferred to have a melting point in the range of 75°C to 97°C and in the range of 110°C to 165°C, and it is particularly preferred to have a melting point in the range of 80°C to 95°C and in the range of 115°C to 160°C.

[0043] As the polypropylene resin used in the present invention, not only propylene homopolymers can be used, but also copolymers of propylene and other α-olefins, polypropylene with low stereoregularity, etc. can be suitably used. As the α-olefin copolymer component used in the copolymer of propylene and other α-olefins, α-olefins with a carbon number of 2 to 8, such as ethylene and 1-butene, are particularly preferred. 1-pentene, 1-hexene, 1,4-methyl-1-pentene, etc. can also be used. In addition, the copolymer is preferably a random or block copolymer obtained by polymerizing one or more of the above-mentioned α-olefins in propylene. There is no particular restriction on the stereostructure of these polymers, and they can be isotactic, atactic, syndiotactic or a mixed structure thereof. In addition, it is desired that the resin composition obtained by using the propylene homopolymer or propylene-α-olefin copolymer is 0.85 or more and 0.95 or less, preferably 0.86 or more and 0.93 or less, and particularly preferably 0.87 or more and 0.92 or less. Polypropylene resins with a specific gravity of 0.85 or less generally have very low crystallinity, and therefore, even when formed into a stretched film, it is difficult to obtain the desired shrinkage, which is not preferred. In addition, if the specific gravity is 0.95 or more, the specific gravity of the film obtained after film formation will become greater than 0.95, which is not preferred.

[0044] It should be noted that, as described above in the present invention, cyclic olefin resin increases specific gravity and reduces low temperature shrinkage, and therefore, it is preferably not contained. In addition, petroleum resin (sometimes also referred to as hydrocarbon resin) and its hydrogenated resin also increase specific gravity and increase natural shrinkage as described above, and therefore, it is preferably not contained.

[0045] The specific gravity of the polypropylene heat-shrinkable film obtained by stretching the unstretched sheet obtained from the above-mentioned polypropylene resin composition must be 0.87 or more and 0.95 or less. In addition, the specific gravity is more preferably 0.88 or more and 0.94 or less, and the specific gravity is particularly preferably 0.88 or more and 0.93 or less. If a raw material with a specific gravity of less than 0.87 is used, the shrinkage rate is reduced due to reduced crystallinity, or the heat resistance is reduced, so it is not preferred. In addition, if the specific gravity is greater than 0.95, the efficiency of floating and sinking separation when printing, etc. when the heat-shrinkable film is used as a label is sometimes reduced, so it is not preferred.

[0046] In addition, the melting point of the polypropylene resin can be controlled by adjusting the type and amount of α-olefin. In order to obtain a polypropylene resin composition having different melting point peaks in the above two temperature ranges, it is preferred to use a mixture of copolymers having different melting points at an appropriate ratio, or a block copolymer with α-olefin. In addition, when mixing polypropylene resins having different melting points, the weight ratio of the resin with a low melting point is preferably 30wt% or more and 85% or less, more preferably 35% or more and 80% or less. In addition, the copolymerization ratio of the total α-olefin contained in the polypropylene resin composition is preferably 8 mol% or more and 24 mol% or less, more preferably 10 mol% or more and 22 mol% or less.

[0047] In addition, the melt flow rate (MFR) of the polypropylene resin composition at 230°C is preferably in the range of 0.1 to 30 g / 10 minutes, more preferably in the range of 0.5 to 20 g / 10 minutes, and particularly preferably in the range of 1.0 to 15 g / 10 minutes. If the MFR is less than 0.1 g / minute, the pressure during extrusion becomes high, and it becomes easy to generate streaks from the die, so it is not preferred. In addition, if it is greater than 30 g / 10 minutes, the discharge becomes unstable, or the stress during stretching is reduced, the thickness unevenness becomes larger, and in addition, the viscosity is reduced, and it becomes easy to break during stretching, so it is not preferred. It should be noted that the melt flow rate can be measured according to the method according to JIS-K-7210.

[0048] In the present invention, in the range of not hindering characteristics, various additives, filling materials, such as heat stabilizers, antioxidants, light stabilizers, antistatic agents, lubricants, nucleators, flame retardants, pigments, dyes, calcium carbonate, barium sulfate, magnesium hydroxide, mica, talcum, clay, zinc oxide, magnesium oxide, aluminum oxide, antibacterial agents, antifogging agents, additives that give natural degradability, etc. can be added as needed in the resin used. For the aspect of operability and the meaning of giving slidability, antistatic property, and heat-resistant adhesion, it is particularly preferred to add organic lubricants represented by fatty acid amide, surfactants represented by fatty acid alkylamine, fatty acid alkylamine ester, and fatty acid monoglyceride, and antiblocking agents represented by silicon dioxide and PMMA. In the case of adding surfactant, it is suitably adjusted in the mode of obtaining the antistatic property required for making 20000ppm as the upper limit. In addition, in the case of adding antiblocking agent, it is adjusted in the range of more than 300ppm and below 10000ppm. It should be noted that if their addition amount exceeds the above upper limit, the haze is reduced and the transparency is impaired, so it is not preferred. Furthermore, other thermoplastic resins, thermoplastic elastomers, rubbers, etc. can be blended within the range that does not hinder the properties of the film of the present invention.

[0049] The film of the present invention may be laminated on its surface with the same polypropylene resin layer and other resin layers, such as a gas barrier resin layer of polyethylene, saponified ethylene-vinyl acetate copolymer, polyvinyl alcohol, etc., within the range not impairing its properties.

[0050] The film of the present invention can be surface treated as required within the range that does not hinder the characteristics of the present invention. As the method of surface treatment, corona discharge treatment, plasma treatment, flame treatment, acid treatment, etc. can be exemplified, without particular limitation. Preferably, corona discharge treatment, plasma treatment, and flame treatment that can be processed continuously and can be easily implemented before the winding process of the manufacturing process of the film are implemented. As a scheme for improving the wetting tension of the surface, corona discharge treatment is particularly preferred.

[0051] The polypropylene-based heat-shrinkable film of the present invention can also be made into a single-layer film, but can also be formed into a laminated structure consisting of a skin layer and a core layer, or a large number of layers above it. As a laminated method, a multilayer coextrusion method can be cited. When forming a laminated structure of more than two layers, it is preferred that each layer is composed of a polypropylene-based resin composition.

[0052] Furthermore, the thickness of the polypropylene-based heat-shrinkable film of the present invention is preferably in the range of 12 μm or more and 100 μm or less. Furthermore, the thickness of the film is more preferably in the range of 15 μm or more and 80 μm or less. If the thickness of the film is less than 12 μm, the stiffness is reduced, and therefore, wrinkles are easily generated when the film is installed as a label, which is not preferred. In addition, if the thickness is more than 100 μm, the cost of the raw materials of the film will increase, which is not preferred.

[0053] The packaging body of the present invention is formed by covering at least a portion of the outer periphery of a packaging object with a label preferably having perforated lines or cuts obtained from the heat-shrinkable polyester film of the present invention and heat shrinking it. Examples of packaging objects include various bottles, cans, snacks, bento boxes, and other plastic containers represented by PET bottles for beverages, and paper boxes. It should be noted that, usually, when a label obtained from a heat-shrinkable polypropylene film is heat-shrunk and covered on these packaging objects, the label heat shrinks by about 5 to 40% and is closely attached to the packaging body. It should be noted that the label covering the packaging object may be printed or not.

[0054] As a method for making a label, there can be used: a method of applying an organic solvent slightly inside the end of one side of a rectangular film when the ends are rolled up and overlapped, or a method of overlapping the ends and heat-sealing by heat sealing, melt-cut sealing, etc.; a method of heat-sealing by ultrasonic sealing, etc. In addition, various adhesives such as hot melt adhesives, ultraviolet curing adhesives, solvent-based adhesives using low molecular weight polyolefins, chloroprene, acid-modified polyolefins, chlorinated polyolefins, etc., water-based adhesives using phenolic resins, polyvinyl acetate, etc., and chemical reaction adhesives using epoxy resins, polyurethane resins, silicone resins, etc. can be applied to the ends of the film and adhered, and these various methods can also be used according to the processing method of the film. When using an organic solvent or a liquid adhesive that can be applied to various films to bond the ends together, the following method can be used: apply the solvent or adhesive slightly to the inside of the end of a single side of a film that is rolled up, immediately roll up the film so that the ends overlap and bond to form a tubular body, and cut it into a label shape.

[0055] As the organic solvent used for bonding when forming the polypropylene film of the present invention into a label, aliphatic hydrocarbons such as n-hexane, n-heptane, cyclohexane, and methylcyclohexane, aromatic hydrocarbons such as toluene, xylene, and trimethylbenzene, halogenated hydrocarbons such as dichloromethane and chloroform, phenols such as phenol, furans such as tetrahydrofuran, etc., or mixed solvents thereof can be used. If cyclohexane is used as the bonding solvent, higher solvent bonding strength can be achieved, so it is preferred.

[0056] For the polypropylene-based heat-shrinkable film of the present invention, when treated in hot water at 90°C for 10 seconds in a no-load state, the heat shrinkage rate in the width direction of the film calculated according to the following formula 1 from the lengths before and after shrinkage (i.e., the hot water heat shrinkage rate at 90°C) must be 40% or more and 80% or less.

[0057] Thermal shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} × 100 (%) ·· Formula 1

[0058] If the hot water heat shrinkage rate in the width direction at 90°C is less than 40%, the shrinkage amount is small, so wrinkles and looseness will occur in the label after heat shrinkage, which is not preferred. There is no particular upper limit to the hot water heat shrinkage rate, but 80% that can be technically achieved in the present invention is the upper limit. It should be noted that the lower limit of the hot water heat shrinkage rate in the width direction at 90°C is preferably 42% or more, more preferably 45% or more, and particularly preferably 50% or more.

[0059] In addition, for the polypropylene-based heat-shrinkable film of the present invention, the hot water heat shrinkage rate in the longitudinal direction when treated in hot water at 90°C for 10 seconds in a no-load state must be 1% or more and 12% or less. In addition, if the hot water heat shrinkage rate in the longitudinal direction at 90°C is higher than 13%, the longitudinal shrinkage is large when used as a label, and it becomes easy to generate strain, so it is not preferred. In addition, the hot water heat shrinkage rate in the longitudinal direction is preferably close to 0%, but the technical lower limit of the present invention is 1%. In addition, the more preferred range of the shrinkage rate in the longitudinal direction is 1% or more and 11% or less, and particularly preferably 1% or more and 10% or less.

[0060] The haze of the polypropylene-based heat-shrinkable film of the present invention is preferably 1% or more and 12% or less. If the haze is 12% or more, the transparency is low, and therefore, it is not suitable as an appearance and is not preferred. In addition, the technical lower limit of the haze of the present invention is 1%, and the practical lower limit is 2%, which is sufficient. Regarding the upper limit of the haze, it is more preferably 11% or less, and particularly preferably 10% or less. It should be noted that the haze varies depending on the amount of additives such as lubricants. In addition, the use of polypropylene copolymerized with α-olefins in the above-mentioned polypropylene resin composition can inhibit and reduce the occurrence of spherulites. The haze is measured by a method based on JIS K7136.

[0061] For the polypropylene heat-shrinkable film of the present invention, the natural shrinkage (dimensional change rate) in the width direction after aging for 672 hours at 40°C 65% RH atmosphere must be 3.0% or less. Preferably 2.5% or less, more preferably 2.0% or less. By making the natural shrinkage at 40°C 65% RH less than 3.0%, it is possible to reduce the dimensional change of the film over time when stored in a warehouse at room temperature and in summer, the occurrence of wrinkles caused by shrinkage over time when stored in a roll state, and the failure during secondary processing such as printing misalignment. If the natural shrinkage in the width direction is large, the width of the film that can be used during storage is reduced, which deteriorates the yield during processing. In addition, if it is in a roll state, the two ends of the film in the width direction are not clamped. Therefore, due to the natural shrinkage during storage, the film is bent and deformed in the roll, and corrugated wrinkles are easily generated, which is not preferred. In addition, the closer the lower limit of the natural shrinkage is to 0%, the more preferred it is, but in the case of the present invention, 0.1% is the technical lower limit.

[0062] For the polypropylene heat-shrinkable film of the present invention, the natural shrinkage (dimensional change rate) in the longitudinal direction after aging for 672 hours at 40°C 65% RH atmosphere must be 1.0% or less. Preferably, it is 0.8% or less, and more preferably, it is 0.6% or less. By making the natural shrinkage at 40°C 65% RH less than 1.0%, the occurrence of wrinkles, relaxation, and deformation of the roll caused by the tightness of the roll caused by natural shrinkage when stored in a roll state in a warehouse at room temperature in summer can be reduced. In addition, the closer the lower limit of the natural shrinkage is to 0%, the more preferred, but in the case of the present invention, 0.1% is the technical lower limit.

[0063] For the polypropylene-based heat-shrinkable film of the present invention, the endothermic heat of the irreversible heat flow visible at 20°C or above and 60°C or below, as measured by a temperature-modulated differential scanning calorimeter (temperature-modulated DSC), is preferably 0.30 J / g or above and 0.95 J / g or below. If the endothermic heat is 0.95 J / g or below, the natural shrinkage can be reduced to 3.0% or below. When the endothermic heat is small, the natural shrinkage can be further reduced, so it is preferred, but the lower limit of the technology of the present invention is 0.30 J / g. In addition, as for the upper limit, it is further preferred to be 0.90 J / g or below, and particularly preferred to be 0.85 J / g or below. The details of the endothermic component are described below.

[0064] The present inventors have studied methods for reducing the natural shrinkage of a polypropylene heat-shrinkable film obtained by stretching at low temperature over time, and have determined that the melting point and heat of fusion, which are generally related to the thermal shrinkage rate at high temperatures above 70°C, are not related to the natural shrinkage rate. In addition, since the natural shrinkage takes time and occurs irreversibly at room temperature far below the melting point of the resin, it is believed that this is related to the irreversible thermal characteristics that are observed below room temperature and originate from amorphous molecular chains.

[0065] This irreversible change was investigated, and therefore, the irreversible heat flow of the temperature-modulated DSC was analyzed for the polypropylene heat-shrinkable film studied by the present inventors. As a result, it was confirmed that there was an endothermic peak in the temperature range of 20°C to 60°C, which is lower than the crystal melting point, and it was further found that the natural shrinkage rate showed a positive correlation with the endothermic heat amount derived from the endothermic peak. That is, it was found that the natural shrinkage rate can be controlled by controlling the endothermic heat amount visible in the range of 20°C to 60°C, and the present invention was completed. The method of controlling the endothermic heat amount is described in the description of the film-making method described later.

[0066] For the polypropylene heat-shrinkable film of the present invention, the refractive index (Ny) in the width direction measured by an Abbe refractometer is preferably 1.490 or more and 1.530 or less, and more preferably 1.500 or more and 1.520 or less. If Ny is 1.490 or less, orientation is basically not carried out, so the desired hot water shrinkage cannot be obtained, which is not preferred. In addition, if Ny is 1.530 or more, orientation is high, so the number of high melting point crystals increases due to directional crystallization, and the hot water shrinkage in the width direction decreases, which is not preferred.

[0067] For the polypropylene-based heat-shrinkable film of the present invention, the value (Ny-Nx) obtained by subtracting the refractive index (Nx) in the length direction from the refractive index (Ny) in the width direction measured with an Abbe refractometer must be 0.005 or more and 0.028 or less. In addition, preferably 0.006 or more and 0.026 or less, more preferably 0.007 or more and 0.023 or less. The upper limit is further preferably 0.015 or less. By stretching in a manner such that the balance of the refractive index in the length direction and the width direction becomes within the above-mentioned range, it is possible to take into account the desired length direction, the hot water shrinkage in the width direction and the perforation line opening property in the length direction.

[0068] For the polypropylene heat shrinkable film of the present invention, the ratio (F10max / F30) of the maximum value of the tensile stress (F10max) in the range of elongation of 0 to 10% to the tensile stress (F30) at an elongation of 30% in the tensile test along the longitudinal direction is preferably 0.5 or more and 1.9 or less. When the tensile stress in the range of elongation of 0 to 10% is large and the tensile stress at an elongation of 30% is small, when the film is torn along the perforation line, the film is stretched compared to the tearing along the perforation line, and the film is cut in the middle of the tearing, or it is easy to tear from the perforation line in the opposite direction. That is, if the above-mentioned tensile stress ratio is greater than 1.9, the perforation line opening property deteriorates, so it is not preferred. In addition, if the tensile stress ratio is less than 0.5, when used as a packaging label, the film becomes easy to crack under the impact of falling during transportation, so it is not preferred. The above-mentioned tensile stress ratio is more preferably 0.6 or more and 1.8 or less, and further preferably 0.7 or more and 1.7 or less.

[0069] For the polypropylene heat-shrinkable film of the present invention, the right-angle tear strength in the length direction when shrinking 10% in hot water at 80°C along the width direction must be 100mN / mm or more and 330N / mm or less. If the right-angle tear strength is lower than 100mN / mm, it is not preferred because it may be easily damaged due to impacts such as falling during transportation. On the contrary, if the right-angle tear strength in the direction orthogonal to the main shrinkage direction of the label is higher than 330N / mm, the cutting property (easiness of tearing) in the initial stage of tearing becomes poor, so it is not preferred. It should be noted that the lower limit of the right-angle tear strength is preferably 120N / mm or more, more preferably 140N / mm or more, and particularly preferably 150N / mm or more. In addition, the upper limit of the right-angle tear strength is preferably 315N / mm or less, more preferably 300N / mm or less, and particularly preferably 280N / mm or less.

[0070] The inventors of the present invention have conducted in-depth research and found that: under specified conditions, stretching and heat treatment in the length direction are performed to achieve both perforation line openability and reduced shrinkage in the length direction. It was further discovered that: the film is controlled in a manner to produce a crystalline component in a low melting point range of more than 70°C and less than 100°C in the width direction, and from this state, it is stretched in the width direction at a low temperature to form a structure of low melting point crystals oriented in the stretching direction, thereby obtaining a high shrinkage rate. Furthermore, a method for reducing the natural shrinkage rate of the film after stretching by the aforementioned method has also been studied, and it has been found that, for the film after stretching, a relaxation treatment (relaxation) is performed under appropriate conditions, thereby reducing the natural shrinkage rate without damaging the shrinkage rate obtained by stretching. Moreover, based on these insights, the inventors of the present invention came up with the present invention. The specific method is described below.

[0071] When the raw material resin is melt-extruded, it is preferred to dry the polypropylene resin raw material using a hopper dryer, a paddle dryer or a vacuum dryer. After the polyolefin resin raw material is dried in this way, it is melt-extruded into a film at a temperature of 200 to 300° C. using an extruder. When extruding, any existing method such as a T-die method or a tubular method can be used.

[0072] Then, the extruded sheet-shaped molten resin is quenched to below 30° C., thereby obtaining an unstretched film. It should be noted that as a method for quenching the molten resin, the following method can be suitably adopted: the molten resin is poured from a nozzle onto a rotating drum controlled to a low temperature by a cooler or the like and quenched and solidified, thereby obtaining a substantially unoriented resin sheet.

[0073] An unstretched sheet is obtained, and then the unstretched sheet preheated with a heating roller is stretched in the length direction by utilizing the speed difference of the roller. The stretching is preferably implemented in two stages. It is preferably implemented when the temperature of the stretching roller is above 50°C and below 100°C, and it is further preferred that the temperature of the stretching roller in the first stage is higher than the temperature of the stretching roller in the second stage by more than 10°C. Stretching is divided into two stages in such a temperature mode, thereby reducing the stress on the film in the stretching process, reducing the increase in the shrinkage rate in the length direction, and improving the perforation line opening property. In addition, by increasing the temperature of the first stage and lowering the temperature of the second stage, the tensile stress at the yield point can be reduced, and the stress in the second half of the stretching can be increased. Therefore, in the obtained film, the tensile stress ratio described above can also be reduced, and it becomes easy to improve the perforation line opening property. In addition, if the roller temperature is lower than 50°C, the film will slip and the stretching is not easy to be stable, so it is not preferred. In addition, if it is higher than 100°C, the film becomes easy to be fused to the heating roller, and it becomes easy to cause failures such as the film winding around the roller, so it is not preferred. A more preferred range of the roller temperature is 55° C. or higher and 90° C. or lower.

[0074] In addition, the stretching ratio in the length direction is preferably adjusted in a range of 1.1 times or more and 1.8 times or less in the first stage, 1.2 times or more and 3.0 times or less in the second stage, and the stretching ratio in the second stage becomes higher than the stretching ratio in the first stage. By setting the stretching ratio in the second stage to be higher than the first stage, it is easy to reduce the uneven thickness in the length direction. In addition, the stretching ratio in the first stage is more preferably 1.15 times or more and 1.6 times or less, more preferably 1.2 times or more and 1.5 times or less. The stretching ratio in the second stage is preferably 1.3 times or more and 2.7 times or less, more preferably 1.5 times or more and 2.3 times or less. In addition, it is preferably adjusted in a manner that the total stretching ratio of the first stage and the second stage becomes 1.2 times or more and 5.0 times or less. If the total stretching ratio is greater than 4.5 times, it becomes difficult to reduce the shrinkage and natural shrinkage in the length direction, and the shrinkage finishing and the appearance during roll storage are easily deteriorated, so it is not preferred. If the stretch ratio is less than 1.2 times, the perforation line opening property is likely to deteriorate, which is not preferred. The total stretch ratio is more preferably 1.3 times or more and 4.2 times or less, and further preferably 1.4 times or more and 4.0 times or less.

[0075] In order to reduce the hot water shrinkage and natural shrinkage in the length direction, it is preferred to implement a relaxation treatment in the length direction (MD relaxation). The MD relaxation treatment can be suitably used in the following methods: a method of reducing the speed between the rollers and shrinking while heating the film on the conveying roller with hot air, infrared heaters, etc.; a method of shrinking the distance between the clamps while heating in a tenter; a method of shrinking the speed of the clamps in a tenter with a driven clamp; etc. In addition, the MD relaxation treatment can be implemented before stretching in the width direction or after stretching in the width direction. The relaxation rate is preferably adjusted appropriately within the range of 3% to 50%, more preferably 5% to 40%. If the relaxation rate is less than 3%, the natural shrinkage in the length direction will increase, so it is not preferred. In addition, if the relaxation rate is more than 50%, the perforation line opening property will deteriorate. In addition, the heating time required for the relaxation treatment becomes longer, and the equipment becomes larger, so the equipment cost becomes larger, which is not preferred.

[0076] Hereinafter, preferred conditions for stretching in the width direction and the steps before and after the stretching will be described in detail.

[0077] (1) Heat treatment before stretching in the width direction

[0078] In the manufacture of the film of the present invention, it is preferred that: before stretching in the width direction, heat treatment is performed at a temperature of 100°C or more and 140°C or less for 3.0 seconds or more and 50.0 seconds or less. The heat treatment can be performed by heating the film during transport, by setting a pipeline for heat treatment using hot air, ceramic heaters, etc., or by clamping the two ends in the width direction in a tenter before stretching in the width direction. By performing the above-mentioned heat treatment, a crystalline component with a melting point is selectively generated in a low temperature range of 70°C or more and 100°C or less, thereby, after stretching in the width direction, a crystalline component with a low melting point can also remain, and therefore, a heat-shrinkable film with a high shrinkage rate can be obtained. In addition, by this heat treatment, the hot water shrinkage rate and the natural shrinkage rate in the length direction are also reduced.

[0079] If the temperature of the intermediate heat treatment is higher than 140°C, it becomes easy to form a high melting point crystalline component above 100°C, and the shrinkage after stretching in the width direction is reduced, so it is not preferred. On the contrary, if the temperature of the heat treatment is lower than 100°C, it becomes difficult to reduce the shrinkage in the length direction. In addition, the formation of low melting point crystalline components based on the heat treatment does not proceed, so the shrinkage during stretching in the width direction becomes easy to decrease, which is not preferred. In addition, the lower limit of the heat treatment temperature is preferably above 105°C, and more preferably above 110°C. On the other hand, the upper limit of the heat treatment temperature is preferably below 135°C, and more preferably below 130°C. On the other hand, the heat treatment time is preferably adjusted appropriately in the range of 1.0 seconds to 50.0 seconds according to the raw material composition.

[0080] (2) Cooling after heat treatment and stretching in the width direction

[0081] After the above heat treatment, the film is preferably cooled to 70°C or less before being stretched in the width direction. By cooling in this way, the low melting point crystalline components can be left. After the above cooling, it is preferred that the film be stretched in the width direction at a ratio of 2.5 times or more and 10.0 times or less in a state where both ends in the width direction are clamped by a clamp in a tenter. In addition, the upper limit of the ratio of the transverse stretching is more preferably 9.0 times or less, and particularly preferably 8.0 times or less.

[0082] Furthermore, stretching can also be carried out in two or more stages. That is, after stretching once in the width direction inside the tenter, an area where stretching is not implemented is set, and then stretching is carried out again in the width direction in the tenter. The stretching ratio of the first stage is preferably 1.5 times or more and 7 times or less, more preferably 2 times or more and 5.5 times or less. Regarding the stretching ratio of the second stage, it is preferably 1.5 times or more and 5 times or less, more preferably 1.8 times or more and 3.5 times or less. In addition, the ratio of each stage is adjusted within the above range in such a way that the total ratio becomes 2.5 times or more and 10.0 times or less. By implementing the stretching separately by the above method, the breakage during stretching can be reduced, and in addition, the increase in the natural shrinkage rate based on stretching can be easily reduced.

[0083] In addition, it is preferable to carry out the stretching at a temperature in the range of 50° C. to 100° C. If the stretching temperature is lower than 50° C., minute voids are generated during stretching, the haze becomes high, or the film becomes easily broken, which is not preferable. On the contrary, if the stretching temperature is higher than 100° C., the low-melting-point crystalline components melt, and not only the shrinkage in the width direction is reduced, but also the thickness unevenness in the width direction is increased, which is not preferable.

[0084] The lower limit of the stretching temperature in the width direction is more preferably 55° C. or higher, particularly preferably 60° C. or higher. The upper limit of the transverse stretching temperature is more preferably 90° C. or lower, particularly preferably 85° C. or lower.

[0085] (3) Relaxation in the width direction (TD relaxation)

[0086] In addition, in the manufacture of a film based on the transverse stretching method of the present invention, as described above, after stretching in the width direction, in a state where the film is clamped at both ends in the width direction by clamps in a tenter, it is necessary to: at a temperature of not less than 60°C and not more than 100°C, within a time of not less than 0.5 seconds and not more than 20.0 seconds, reduce the tenter in the width direction in such a way that the relaxation rate calculated by Formula 2 becomes within the range of not less than 13% and not more than 40% of the length in the width direction, thereby relaxing and shrinking the film (TD relaxation).

[0087] TD relaxation rate = {(length before relaxation - length after relaxation) / length before relaxation} × 100 (%) ·· Formula 2

[0088] If the temperature for the relaxation treatment is lower than 60°C, the film will not shrink sufficiently during relaxation and wrinkles will be generated, which is not preferred. On the other hand, if the temperature is higher than 100°C, the shrinkage rate will be greatly reduced, and the shrinkage will be insufficient when used as a heat shrinkable film, which is not preferred. The more preferred temperature for the relaxation treatment is 65°C to 95°C, and particularly preferably 70°C to 90°C.

[0089] In addition, if the length in the width direction reduced during the relaxation treatment is less than 13% of the length before the treatment, the natural shrinkage rate becomes high, which is not preferred. In addition, if it is greater than 40%, the 90°C shrinkage rate decreases, and the productivity decreases, which is not preferred. The relaxation treatment is preferably carried out in the range of more preferably 15% to 35%, particularly preferably 17% to 33%.

[0090] By performing the relaxation treatment, the low melting point crystal components of the final film remain, and the shrinkage required as a heat shrinkable film is maintained unchanged, the amount of heat absorbed in the irreversible heat flow can be reduced, and the natural shrinkage can be reduced. In addition, when the relaxation treatment is performed by dividing the stretching in the width direction into two or more stages, the relaxation treatment can also be performed separately after each stretching. In addition to shrinking the tenter in the width direction, the relaxation treatment can also be performed by opening the clamps that clamp the ends of the film in a state where heat is applied near the tenter outlet, shrinking the film in the width direction and winding the film.

[0091] Example

[0092] The present invention is described in more detail below based on the examples, but the present invention is not limited to the embodiments and can be appropriately changed without departing from the gist of the present invention. The raw materials used in the examples and comparative examples, the raw material formulations used in the examples and comparative examples, and the film production conditions (stretching / heat treatment conditions, etc.) are shown in Tables 1 and 2. It should be noted that the resin raw materials PP1 to PP4 in Table 1 are as follows.

[0093] Resin raw material PP1: polypropylene-butene random copolymer (trade name "TAFMERXM7070" manufactured by Mitsui Chemicals, Inc., MFR = 7.0 g / 10 min, melting point 77° C., specific gravity 0.88)

[0094] Resin raw material PP2: polypropylene-butene random copolymer (trade name "TAFMERXM7080" manufactured by Mitsui Chemicals, Inc., MFR = 7.0 g / 10 min, melting point 83° C., specific gravity 0.88)

[0095] Resin raw material PP3: polypropylene-ethylene random copolymer (trade name "Novatec EG6D" manufactured by Japan Polypropylene Corporation, MFR = 1.9 g / 10 minutes, melting point 145°C, specific gravity 0.90)

[0096] Resin raw material PP4: polypropylene (manufactured by Sumitomo Chemical Co., Ltd., trade name "FS2011DG3", MFR = 2.5 g / 10 min, melting point 159°C, specific gravity 0.91)

[0097] In addition, MFR describes the value at 230°C.

[0098] In addition, the film evaluation method is as follows.

[0099] [Tm (melting point)]

[0100] Using a differential scanning calorimeter (model: DSC60) manufactured by Shimadzu Corporation, 5 mg of the film was collected in an aluminum pan, and the heat flow (unit: W / g) at each temperature was measured when the temperature was increased from -40°C to 200°C at a heating rate of 10°C / min with a sampling interval of 0.5 seconds. The vertical axis is the heat flow (with the negative direction being endothermic) and the horizontal axis is the temperature (unit: °C), and a heat flow curve was obtained.

[0101] A regression line was prepared using the values ​​of the heat flow curve in the range of 55 to 60°C. With regard to the heat flow, the difference obtained by subtracting the value on the heat flow curve from the value on the regression line was obtained at each temperature from 60°C to 175°C from the low temperature side, and the temperature at which the difference first exceeded 0.001 W / g was defined as the melting start temperature.

[0102] Similarly, a regression line was prepared using the values ​​of 175°C to 180°C of the heat flow curve. With respect to the heat flow from 175°C to 60°C, the difference obtained by subtracting the value on the heat flow curve from the value on the regression line was obtained sequentially from the high temperature side, and the temperature at which the difference first exceeded 0.001 W / g was defined as the melting end temperature.

[0103] The straight line passing through the points on the heat flow curve at the melting start temperature and the melting end temperature is used as the baseline. For the heat flow at each temperature of 70°C to 170°C, the difference obtained by subtracting the value on the heat flow curve from the value on the baseline is calculated. Among the values ​​of these differences at each temperature, the point where the value is greater than 0.02W / g and becomes the maximum value for the temperature is taken as the melting peak of the heat flow curve, and the temperature of the melting peak is taken as the melting point.

[0104] [Endothermic heat in irreversible heat flow of temperature-modulated DSC]

[0105] Using a temperature modulated differential scanning calorimeter (TM DSC) "DSC250" (manufactured by TA instruments), 5 mg of the film was weighed in a T-ZERO pan. In heating-only mode, the temperature was raised from -40°C to 200°C at an average heating rate of 2°C / min and a modulation period of 40 seconds. The irreversible heat flow was measured with a sampling interval of 0.1 seconds to obtain an irreversible heat flow curve with the vertical axis being the irreversible heat flow (unit: W / g, with the negative direction being endothermic) and the horizontal axis being the temperature (unit: °C).

[0106] For the irreversible heat flow curve, a regression line was drawn from the values ​​at 18 to 20° C. For the irreversible heat flow, the difference obtained by subtracting the value on the irreversible heat flow curve from the value on the regression line was obtained in order from the low temperature side in the range of 20° C. to 60° C., and the temperature at which the value first became 0.0005 W / g or more was taken as the endothermic start temperature.

[0107] Similarly, a regression line was prepared from the values ​​of the irreversible heat flow curve at 60° C. to 62° C. The difference obtained by subtracting the value on the irreversible heat flow curve from the value on the regression line was successively calculated from 60° C. to 20° C., and the temperature at which the difference first became 0.0005 W / g or more was taken as the end temperature of the endothermic reaction.

[0108] A straight line connecting points on the irreversible heat flow curve at the endothermic start temperature and the endothermic end temperature was used as a baseline, and the area of ​​the portion enclosed by the irreversible heat flow curve and the baseline was determined as the peak endothermic heat (unit: J / g).

[0109] [Identification of α-olefin components]

[0110] The types of α-olefins such as ethylene and butene in the propylene-α-olefin copolymer are determined by 13C NMR spectroscopy according to the method described in the Handbook of Polymer Analysis (published by Kinokuniya Bookstore in 1995), pages 615 to 617. It should be noted that it can also be determined by IR spectroscopy according to the method described in the item "(i) Random Copolymer" on page 256 of the same book.

[0111] [Heat shrinkage (hot water heat shrinkage)]

[0112] The film was cut into a 10 cm × 10 cm square in a manner parallel to the unwinding direction (hereinafter, for the cut film, the unwinding direction before cutting is referred to as the length direction, and the direction perpendicular to the unwinding direction on the film surface is referred to as the width direction), immersed in hot water at a specified temperature ±0.5°C for 10 seconds in a no-load state and heat shrunk, then immersed in water at 23°C ±0.5°C for 10 seconds, pulled out of the water, and the length and width dimensions of the film were measured. The heat shrinkage rates were calculated according to Formula 1.

[0113] [Natural shrinkage]

[0114] The film was cut into a 210 mm × 210 mm square in parallel with the unwinding direction, and a 200 mm mark was drawn in the length direction and width direction of the cut sample, and aged for 672 hours in an atmosphere of 40°C and 65% RH. The natural shrinkage rate was calculated using the following formula 3 for the length direction and width direction, respectively.

[0115] Natural shrinkage rate = {(marking line length before aging - marking line length after aging) / width direction marking line length before aging} × 100 (%) ·· Formula 3

[0116] [Haze]

[0117] The measurement was performed using a haze meter (300A, manufactured by Nippon Denshoku Industries, Ltd.) in an atmosphere at 23° C. in accordance with JIS K 7136. The measurement was performed twice, and the average value was calculated.

[0118] [Tensile test]

[0119] According to JIS-K-7127, the film was sampled into a sample with a width of 15 mm and a length of 100 mm as a test piece. A universal tensile testing machine (Autograph manufactured by Shimadzu Corporation) was used, and the chuck spacing was adjusted to 20 mm. The two ends of the test piece (in the length direction of the film) were clamped, and a tensile test was carried out at a tensile speed of 200 mm / min. The maximum value (F10 max) of the tensile stress at an elongation of 0 to 10% and the stress value (F30) at an elongation of 30% were calculated.

[0120] [Right-angle tear strength]

[0121] After the film was shrunk by 10% in the width direction in hot water adjusted to 80°C, a test piece of a specified size was formed and sampled according to JIS-K-7128. Then, a universal tensile tester (Autograph manufactured by Shimadzu Corporation) was used to clamp both ends of the test piece and measure the strength at the time of tensile fracture in a direction perpendicular to the main shrinkage direction of the label at a tensile speed of 200 mm / min. Then, the right-angle tear strength per unit thickness was calculated using the following formula 4.

[0122] Right-angle tear strength = tensile strength at break ÷ thickness ··Formula 4

[0123] [proportion]

[0124] The specific gravity of the film was calculated from the ratio of the density of the film measured by the density gradient tube method to the density of water at a temperature of 23° C. in accordance with JIS K7112.

[0125] [Refractive index]

[0126] Using "Abbe Refractometer 4T" manufactured by ATAGO CO., LTD., each sample film before shrinkage was left in an atmosphere of 23±2°C and 65±5%RH for more than 2 hours, and then the refractive index (Nx, Ny) in the longitudinal direction and the width direction was measured.

[0127] [Shrinkage finishing properties]

[0128] [Shrinkage strain of labels]

[0129] The two ends of the heat-shrinkable film with a grid pattern pre-added with 10mm intervals were overlapped by 5mm, and heat-seal cut was performed using a high-frequency welding machine "HAKKO311" (manufactured by Hakuko Co., Ltd.) to produce a cylindrical label (a label in which the main shrinkage direction of the heat-shrinkable film is the circumferential direction). On the label, the label was covered on a 500ml PET bottle (body diameter 67mm, minimum neck diameter 25mm, trade name "Sixteen Tea"), and passed through a steam tunnel (model; SH-1500-L) made by Fuji Astec Inc. with a zone temperature of 85°C for 10.0 seconds, thereby causing the label to be heat-shrunk and installed on the bottle. It should be noted that when installing, the neck was adjusted so that the portion with a diameter of 43mm became one end of the label. As an evaluation of the finishing properties after shrinkage, the deviation of the grid pattern from the horizontal plane in the 360-degree direction of the installed label body, excluding the grid including the fused portion, was measured as strain, and the maximum value of the strain was obtained. The evaluation was performed according to the following criteria.

[0130] ◎: Maximum strain less than 1.0 mm

[0131] ○: Maximum strain 1.0 mm or more and less than 2.0 mm

[0132] ×: Maximum strain 2.0 mm or more

[0133] [Tag folds]

[0134] Under the same conditions as those for the shrinkage strain of the label described above, the label was attached to a PET bottle, and the occurrence of wrinkles was evaluated based on the following criteria.

[0135] ◎: The number of wrinkles larger than 2 mm was 0.

[0136] ○: The number of wrinkles with a size of 2 mm or more is 1 or more and 2 or less.

[0137] ×: The number of wrinkles with a size of 2 mm or more is 3 or more.

[0138] [Perforation line opening]

[0139] Under the same conditions as the shrinkage strain of the above-mentioned label, a label with perforated lines introduced in advance in a direction orthogonal to the main shrinkage direction is installed on a PET bottle. The perforated lines are formed by introducing holes with a length of 1 mm at intervals of 1 mm, and two lines are set along the longitudinal direction (height direction) of the label with a width of 22 mm and a length of 170 mm. After that, fill the bottle with 500 ml of water and refrigerate at 5°C. Use fingertips to tear the perforated lines of the bottle label just taken out of the refrigerator, count the number of lines that are not beautifully cracked along the perforated lines in the longitudinal direction, or the label is cut in the middle of tearing and the label cannot be torn off the bottle, and calculate the perforated line unsealing defective rate (%) relative to all 50 samples. If the perforated line unsealing defective rate is 20% or less, it is practically qualified.

[0140] [Evaluation of coil appearance after time]

[0141] (Appearance change after storage at 40℃ for 672 hours)

[0142] The film was slit into rolls of 300 mm in width and 300 m in length and rolled up. The roll was placed in a constant temperature chamber adjusted to an atmosphere of 40°C and 65±10% RH. After being stored for 672 hours, the film was taken out from the constant temperature chamber and the state of the wrinkles when 3 m of the film was unrolled from the roll was evaluated according to the following criteria.

[0143] ◎: The number of wrinkles with a width of 1 cm or more is 0.

[0144] ○: The number of wrinkles of 1 cm or more is 1 or more and 2 or less.

[0145] ×: The number of wrinkles of 1 cm or more is 3 or more.

[0146] [Floating and sinking separation suitability evaluation]

[0147] Cut the film into a 100 mm × 100 mm square shape, put 2 L of water in a cylindrical container with a bottom diameter of 130 mm, adjust to 23°C ± 2°C, take care not to allow bubbles to adhere, and let the film sink to the bottom. Visually evaluate whether the film floats from the water according to the following criteria.

[0148] ○: The film floats to the water surface

[0149] ×: The film does not float to the water surface

[0150] [Example 1]

[0151] 500 ppm of SiO2 (Sylysia 266 manufactured by FUJI SILYSIA CHEMICAL LTD.) was added as a lubricant to a dry blend of polypropylene resins PP1 and PP3 at a weight ratio of 60 / 40 from an extruder, melt extruded at 230° C., and quenched by winding around a rotating metal roll cooled to 20° C. to obtain an unstretched film (polypropylene resin sheet) having a thickness of 370 μm. The pulling speed of the unstretched film (rotation speed of the metal roll) at this time was about 5.0 m / min.

[0152] Then, the obtained unstretched film was introduced into a longitudinal stretching machine in which a plurality of roller groups were continuously arranged, and preheated on a preheating roller until the film temperature reached 65°C. Then, the first stage of stretching was performed to 1.3 times between stretching rollers whose surface temperature was set to 75°C, with the roller speed on the high-speed side set to 6.5 m / min. Then, the film was further stretched to 2.0 times between stretching rollers whose surface temperature was set to 60°C, with the roller speed on the high-speed side set to 13.0 m / min. The total stretching was performed to 2.6 times. Thereafter, the film was conveyed by a roller whose surface temperature was set to 60°C, and the roller was decelerated to 11.0 m / min while blowing hot air set to 95°C, and a 15% relaxation treatment was performed in the longitudinal direction to obtain a longitudinal uniaxially stretched film having a thickness of 168 μm.

[0153] The obtained longitudinal uniaxially stretched film is heat treated with hot air in a heat treatment zone provided on a conveyor line continuously equipped with a plurality of roller groups until the film temperature reaches 125°C, and then air-cooled to 60°C and introduced into a tentering machine continuously equipped with a transverse stretching zone and a relaxation treatment zone.

[0154] After preheating until the film temperature reaches 60°C, the first stage of stretching is carried out at 60°C in the width direction at 3.0 times, and then the second stage of stretching is carried out at 60°C at 2.2 times. In the relaxation treatment area, a 20% relaxation treatment is carried out at 75°C within 7 seconds, thereby obtaining a biaxially stretched film with a thickness of 30 μm.

[0155] The film after transverse stretching as described above was cut at the ends and wound on a paper tube to obtain a film roll of a biaxially stretched film (polypropylene heat shrinkable film) with a width of 500 mm and a thickness of 30 μm wound only at a predetermined length. Then, the properties of the obtained film were evaluated according to the above method. The evaluation results are shown in Table 2.

[0156] [Example 2]

[0157] The discharge amount was adjusted so that the thickness of the unstretched sheet was 439 μm, and the stretching ratio in the first stage in the longitudinal direction was changed to 1.5 times so that the total stretching ratio was 3.0 times. Film formation was carried out in the same manner as in Example 1 to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0158] [Example 3]

[0159] The discharge amount was adjusted so that the thickness of the unstretched sheet was 521 μm, and the first-stage stretching ratio in the longitudinal direction was changed to 1.8 times, so that the total stretching ratio was 3.6 times. Film formation was carried out in the same manner as in Example 1 to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0160] [Example 4]

[0161] The discharge amount was adjusted so that the thickness of the unstretched sheet was 252 μm, the stretching ratio in the first stage in the longitudinal direction was changed to 1.2 times, the stretching ratio in the second stage was changed to 1.3 times, the total stretching ratio was changed to 1.6 times, and the relaxation rate in the longitudinal direction was changed to 5%, and a film was formed in the same manner as in Example 1 to obtain a biaxially stretched film with a thickness of 30 μm. The evaluation results are shown in Table 2.

[0162] [Example 5]

[0163] The film was formed in the same manner as in Example 1 except that the discharge rate was adjusted so that the thickness of the unstretched sheet was 353 μm and the relaxation rate in the longitudinal direction was changed to 20% to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0164] [Example 6]

[0165] The film was formed in the same manner as in Example 1 except that the discharge rate was adjusted so that the thickness of the unstretched sheet was 393 μm and the relaxation rate in the longitudinal direction was changed to 10% to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0166] [Example 7]

[0167] The film was formed in the same manner as in Example 1 except that the polypropylene resin used was changed to one obtained by dry blending PP1 and PP4 at a weight ratio of 60 / 40 to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0168] [Example 8]

[0169] The film was formed in the same manner as in Example 1 except that the polypropylene resin used was changed to one obtained by dry blending PP2 and PP3 at a weight ratio of 60 / 40 to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0170] [Example 9]

[0171] The film was formed in the same manner as in Example 1 except that the polypropylene resin used was changed to one obtained by dry blending PP1 and PP3 at a weight ratio of 70 / 30 to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0172] [Example 10]

[0173] The film was made into an unstretched film in the same manner as in Example 1, and the film was stretched in the longitudinal direction. After that, the obtained longitudinal uniaxially stretched film was heat-treated by hot air in a heat treatment zone provided on a conveyor line continuously provided with a plurality of roller groups until the film temperature reached 125°C. After that, the film was air-cooled until 60°C, and the film was introduced into a tenter provided with a lateral stretching zone and a relaxation treatment zone continuously. After preheating until the film temperature reached 60°C, the first stage of stretching was performed at 60°C in the lateral stretching zone at 3.0 times in the width direction, and then the second stage of stretching was performed at 60°C at 2.2 times. In the relaxation treatment zone, a 15% relaxation treatment was performed in the width direction at 75°C within 7 seconds, and a 15% relaxation treatment was performed in the longitudinal direction by reducing the distance between the clamps, thereby obtaining a biaxially stretched film with a thickness of 30 μm. The evaluation results are shown in Table 2.

[0174] [Example 11]

[0175] The film was formed in the same manner as in Example 1 except that the temperature of the relaxation treatment after the widthwise stretching was changed to 80° C. to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0176] [Example 12]

[0177] The film was formed in the same manner as in Example 1 except that the temperature of the relaxation treatment after the widthwise stretching was changed to 85° C. to obtain a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2.

[0178] [Comparative Example 1]

[0179] Under the same conditions as in Example 1, only the discharge amount was changed to form an unstretched sheet with a thickness of 168 μm. The obtained unstretched film was heat-treated with hot air in a heat treatment area provided on a conveyor line continuously provided with a plurality of roller groups until the film temperature reached 125°C, and then air-cooled to 60°C and introduced into a tentering machine continuously provided with a transverse stretching area and a relaxation treatment area. After that, preheating was performed until the film temperature reached 60°C, and then the first stage of stretching was performed at 3.0 times at 60°C in the transverse stretching area along the width direction, and then the second stage of stretching was performed at 2.2 times at 60°C. In the relaxation treatment area, a 15% relaxation treatment was performed at 75°C within 7 seconds, thereby obtaining a transverse uniaxially stretched film with a thickness of 30 μm. The evaluation results are shown in Table 2. Since no stretching in the longitudinal direction was applied, it was a film with a high defect rate when the perforated line was opened.

[0180] [Comparative Example 2]

[0181] Film formation was performed in the same manner as in Example 1 except that the temperature of the heat treatment performed before stretching in the width direction was changed to 95° C., thereby obtaining a biaxially stretched film having a thickness of 30 μm. The evaluation results are shown in Table 2. The hot water shrinkage rate in the longitudinal direction was high, and therefore the strain caused by the longitudinal shrinkage during shrinkage finishing was large, resulting in a film having a poor appearance during shrinkage finishing.

[0182] [Comparative Example 3]

[0183] Under the same conditions as in Example 1, except that the discharge rate was changed to form an unstretched sheet having a thickness of 437 μm, and no relaxation treatment in the longitudinal direction was performed, a biaxially stretched film having a thickness of 30 μm was obtained by film formation in the same manner as in Example 1. The evaluation results are shown in Table 2. The natural shrinkage in the longitudinal direction was high, so wrinkles were generated when the film roll was unwound after a period of time, and the film was poor in practicality.

[0184] [Comparative Example 4]

[0185] Under the same conditions as in Example 1, except that the discharge amount was changed and an unstretched sheet with a thickness of 437 μm was formed, and no relaxation treatment in the width direction was performed, a biaxially stretched film with a thickness of 30 μm was obtained by film formation in the same manner as in Example 1. The evaluation results are shown in Table 2. The natural shrinkage in the width direction was high, so that when the film roll after storage was unrolled after a period of time, corrugated wrinkles were generated in the width direction, and the film was poor in practicality.

[0186] Table 2 shows that the films obtained in Examples 1 to 12 have high shrinkage in the width direction and low shrinkage in the orthogonal length direction, so the shrinkage is also good when the shrinkage is completed. In addition, the perforation line is also good. Furthermore, by implementing a relaxation treatment, the natural shrinkage rate can be reduced, and the occurrence of wrinkles after aging is basically not observed, which satisfies practical requirements as a heat shrinkable film. Only polypropylene resin is used, so the specific gravity is very small, and it is a film suitable for floating and sinking separation of PET bottles. In contrast, the films obtained in Comparative Examples 1 to 4 are described in Table 2 and the items of the above-mentioned comparative examples, and they are not films whose characteristics satisfy practical requirements as heat shrinkable films.

[0187] [Table 1]

[0188]

[0189] [Table 2A]

[0190]

[0191] [Table 2B]

[0192]

[0193] Industrial Applicability

[0194] The polypropylene-based heat-shrinkable film of the present invention has excellent shrinkage characteristics and perforation line opening properties as described above, and can therefore be suitably used for packaging of various articles, such as labels for PET bottles. In addition, since the specific gravity is less than 1.0, it is suitable for floating and sinking separation from PET bottles, and can contribute to the efficiency of recycling PET bottles.

Claims

1. A polypropylene heat-shrinkable film, characterized in that: It is a stretched film composed of a polypropylene resin composition and satisfies the following (1) to (7), (1) when the film is immersed in hot water at 90° C. for 10 seconds, the hot water heat shrinkage ratio in the width direction of the film is 40% or more and 80% or less, (2) when the film is immersed in hot water at 90° C. for 10 seconds, the hot water heat shrinkage ratio in the longitudinal direction of the film is 1% or more and 12% or less, (3) The specific gravity of the film is 0.87 or more and 0.95 or less, (4) a right-angle tear strength in the longitudinal direction per unit thickness after shrinking by 10% in the width direction in hot water at 80°C of 100 mN / mm or more and 330 mN / mm or less, (5) The difference Ny-Nx between the refractive index in the width direction (Ny) and the refractive index in the length direction (Nx) is 0.005 or more and 0.028 or less, (6) the polypropylene heat-shrinkable film has a natural shrinkage in the width direction of 0.1% or more and 3.0% or less after aging for 672 hours in an atmosphere of 40° C. and 65% RH, (7) The natural shrinkage rate in the longitudinal direction of the polypropylene-based heat-shrinkable film after aging for 672 hours in an atmosphere of 40° C. and 65% RH is 0.1% or more and 1.0% or less.

2. The polypropylene heat-shrinkable film according to claim 1, characterized in that: The value obtained by dividing the maximum tensile stress in the range of elongation of 0 to 10% in the tensile test in the longitudinal direction by the tensile stress at an elongation of 30% is 0.5 or more and 1.9 or less.

3. The polypropylene heat-shrinkable film according to claim 1, characterized in that: The haze of the film is 1% or more and 12% or less.

4. The polypropylene heat-shrinkable film according to claim 1, characterized in that: The melting point of the present invention has one or more melting peak temperatures measured by a differential scanning calorimeter in the range of 70°C to 100°C and in the range of more than 100°C to 170°C.

5. The polypropylene heat-shrinkable film according to claim 1, characterized in that: The irreversible heat flow measured by a temperature modulation scanning calorimeter has a peak in the range of 20° C. to 60° C., and the endothermic amount of the peak is 0.3 J / g to 0.95 J / g.

6. The polypropylene-based heat-shrinkable film according to claim 1, characterized in that: The refractive index Ny in the width direction is 1.490 or more and 1.530 or less.

7. The polypropylene heat-shrinkable film according to claim 1, characterized in that: The polypropylene-based heat-shrinkable film has a thickness of 12 μm or more and 100 μm or less.

8. The polypropylene-based heat-shrinkable film according to claim 1, characterized in that: The polypropylene resin composition constituting the polypropylene heat shrinkable film contains ethylene or 1-butene as a copolymer component. 9 . A label comprising the polypropylene heat-shrinkable film according to claim 1 as a base material and provided with a perforated line or a pair of incisions.

10. A packaging body, characterized in that: The heat-shrinkable polypropylene film according to any one of claims 1 to 8 is provided with a label in a loop shape on at least a portion of the outer periphery of the packaging object.

11. A packaging body, characterized in that: The label according to claim 9 is provided on at least a portion of the outer periphery of the packaging object.

Citation Information

Cited By

  • Low-density high-shrinkage film as well as preparation method and application thereof

    CN119773335A