Conductive resin composition-metal laminate
By using conductive resin composition containing styrene-type thermoplastic elastomers, adhesive layer and metal laminate technology in the medical surgical technique training model, the problem of insufficient adhesion strength of the electrode plate is solved, and the stability of the energy equipment is achieved Use and train efficiently.
Patent Information
- Application Number
- CN202380027435.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-01
- Publication Date
- 2024-11-08
AI Technical Summary
The existing model for training medical surgical techniques cannot stick the electrode plate with sufficient strength, resulting in the electrode plate being easily peeled off when using energy equipment, and the medical surgical techniques cannot be effectively trained.
The base material layer formed by a conductive resin composition containing a styrene-based thermoplastic elastomer and an adhesive layer is used, and a conductive resin composition-metal laminate is formed to enhance the electrode The adhesion strength and conduction ability of the board.
It realizes stable adhesion and conduction of electrode plates, which can be effectively used for medical surgical techniques training, especially in endoscopic hemostasis and other operations, improving the reliability and safety of training.
Smart Images

Figure CN118922876A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a conductive resin composition-metal laminate and an organ model using the conductive resin composition-metal laminate. Background Art
[0002] In recent years, there has been a growing expectation for low-invasive surgeries that are less burdensome to the human body and that can expect early recovery, such as surgeries using endoscopes and laparoscopy, and the number of cases has increased. For example, by removing a tumor formed in the lower layer of the mucosa inside an organ under an endoscope (endoscopic submucosal dissection), surgery can be performed on a smaller wound than in a conventional laparotomy. In addition, by stopping bleeding in the digestive tract under an endoscope (endoscopic hemostasis), it is possible to prevent shock caused by bleeding and avoid emergency surgery. Therefore, the burden on the body is reduced for the patient, and it is expected that the patient will return to society at an early stage with a short hospitalization period.
[0003] Therefore, there is a growing demand for surgical technique training models for doctors and medical students who are dealing with surgeries using endoscopes and laparoscopy, and medical surgical technique training models have been proposed to improve technology and the quality of medical practice (Patent Documents 1, 2, 3).
[0004] In addition, there is an increasing number of cases where surgical energy devices are used as instruments.
[0005] Patent Document 1: Japanese Patent Application Publication No. 2006-116206
[0006] Patent Document 2: Japanese Patent Application Publication No. 2008-197483
[0007] Patent Document 3: Japanese Patent Application Publication No. 2015-085017 Summary of the invention
[0008] When the electrode plate is attached to the skin, an adhesive gel is used in which electrolytes are dispersed in polyacrylic acid, etc. However, in the conventional medical surgical technique training model, the electrode plate cannot be connected with sufficient strength, and when an energy device, an endoscope or other instrument contacts the medical surgical technique training model, the electrode plate may be easily peeled off.
[0009] Therefore, there is a demand for an organ model to which a counter electrode plate can be attached with a certain strength or more and which can be used for training of medical surgery techniques using energy devices.
[0010] An object of the present invention is to provide a conductive resin composition-metal laminate and an organ model that can be used for training of medical surgery techniques using energy devices, to which a counter electrode plate can be bonded with a certain strength or more.
[0011] The inventors of the present invention studied various methods and found that by laminating a metal layer on a base layer formed by a conductive resin composition containing a styrene-based thermoplastic elastomer with the aid of an adhesive layer, the electrode plates can be adhered with a certain strength and made conductive, thereby being used for training medical surgical techniques using energy equipment, thereby completing the present invention.
[0012] The present invention relates to the following technical solutions.
[0013] (1) A conductive resin composition-metal laminate comprising: a substrate layer formed of a conductive resin composition containing a styrene-based thermoplastic elastomer; and a metal layer laminated on one surface of the substrate layer via an adhesive layer.
[0014] (2) The conductive resin composition-metal laminate according to (1), wherein the volume resistivity is 1.0×10 2 ~1.0×10 7 Ω·cm.
[0015] (3) The conductive resin composition-metal laminate according to (1) or (2), wherein the adhesive layer contains one or more adhesives selected from the group consisting of epoxy adhesives, olefin adhesives, cyanoacrylate adhesives, urethane adhesives and silicone adhesives.
[0016] (4) The conductive resin composition-metal laminate according to any one of (1) to (3), which is connected to a counter electrode plate.
[0017] (5) An organ model for training medical surgical techniques, comprising the conductive resin composition-metal laminate according to any one of (1) to (4).
[0018] (6) The organ model according to (5), wherein the medical surgery technique training is medical surgery technique training using an energy device.
[0019] (7) The organ model according to (5) or (6), wherein the energy device is any one selected from the group consisting of a high-frequency hemostatic forceps, an electric scalpel, an ultrasonic scalpel, and a high-frequency radio scalpel.
[0020] (8) The organ model according to any one of (5) to (7), comprising a simulated blood vessel connected to a device capable of supplying simulated blood.
[0021] (9) The organ model according to any one of (5) to (8), wherein the medical surgery technique training is endoscopic hemostasis training.
[0022] (10) The organ model according to (9), wherein the training of endoscopic hemostasis is training of hemostasis based on a thermal coagulation method using an energy device.
[0023] According to the present invention, it is possible to provide a conductive resin composition-metal laminate and an organ model to which a counter electrode plate can be bonded with a certain strength or more and which can be used for training of medical surgical techniques such as hemostasis using energy devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a view showing a cross section of a conductive resin composition-metal laminate according to the first embodiment of the present invention.
[0025] Figure 2 It is a diagram showing a cross section of an organ model according to a second embodiment of the present invention.
[0026] Figure 3 It is a diagram showing a cross section of a modified example of the organ model according to the second embodiment of the present invention. DETAILED DESCRIPTION
[0027] Hereinafter, one embodiment of the present invention will be described in detail. The present invention is not limited to the following embodiment, and can be implemented by appropriately adding changes within a range that does not hinder the effects of the present invention.
[0028] [First embodiment]
[0029] The conductive resin composition-metal laminate according to the first embodiment of the present invention includes a substrate layer formed of a conductive resin composition containing a styrene-based thermoplastic elastomer, and a metal layer laminated on one surface of the substrate layer via an adhesive layer. Figure 1 1 is a diagram showing a conductive resin composition-metal laminate 1 according to the present embodiment, which includes a base material layer 2, an adhesive layer 3, and a metal layer 4 in this order.
[0030] The volume resistivity of the conductive resin composition-metal laminate is preferably 1.0×10 2 ~1.0×10 7 Ω·cm, more preferably 1.0×10 2 ~5.0×10 5 Ω·cm. The volume resistivity can be obtained by conditioning a test piece of any shape at a temperature of 23±2°C and a relative humidity of 50±5% for more than 24 hours according to JIS C2139, and then measuring the volume resistivity of the PSP probe 20 seconds after the power is turned on at a voltage of 10V using a commercially available machine (e.g., a resistivity meter Loresta-GP (model: MCP-T610) manufactured by Mitsubishi Chemical Analysis Co., Ltd.). By setting the volume resistivity to 1.0×107 Ω·cm or less, so that it can be cut using energy equipment.
[0031] [Base material layer]
[0032] like Figure 1 As shown, the base material layer of the present embodiment is one layer constituting the conductive resin composition-metal laminate, and is a structure formed of a conductive resin composition containing a styrene-based thermoplastic elastomer.
[0033] The shape of the substrate layer is not particularly limited and can be set according to its application. In addition, the molding method of the substrate layer can be appropriately selected from extrusion molding, injection molding, injection molding, compression molding, etc. according to the molded shape.
[0034] In one embodiment of the present invention, the thickness of the substrate layer may be set to 0.1 to 30 mm or 1 to 20 mm.
[0035] (Conductive resin composition)
[0036] In one embodiment of the present invention, the conductive resin composition is a conductive resin composition containing a styrene-based thermoplastic elastomer, and its volume resistivity is preferably 1.0×10 2 ~1.0×10 7 Ω·cm, more preferably 1.0×10 2 ~1.0×10 6 Ω·cm. The volume resistivity of the conductive resin composition was measured by the same method as the method for measuring the volume resistivity of the conductive resin composition-metal laminate described above.
[0037] (Styrene thermoplastic elastomer)
[0038] The conductive resin composition of this embodiment contains a styrene-based thermoplastic elastomer. The styrene-based thermoplastic elastomer of one embodiment of the present invention is an aromatic vinyl / conjugated diene block copolymer composed of a block polymerized unit (X) derived from an aromatic vinyl group and a block polymerized unit (Y) derived from a conjugated diene, or a hydrogenated product thereof.
[0039] Such a structure of an aromatic vinyl / conjugated diene block copolymer is in the form of, for example, X(YX): n or (XY) n [n is an integer greater than or equal to 1], wherein X(YX) nThe XYX form is particularly preferred. The XYX form of the copolymer is preferably one or more copolymers selected from the group consisting of polystyrene-polybutadiene-polystyrene block copolymers, polystyrene-polyisoprene-polystyrene block copolymers, and polystyrene-polyisoprene-butadiene-polystyrene block copolymers.
[0040] In this aromatic vinyl / conjugated diene block copolymer, the aromatic vinyl block units (X) of the hard segment exist as crosslinking points of the conjugated diene rubber block units (Y) to form simulated crosslinks (domains). The conjugated diene rubber block units (Y) existing between the aromatic vinyl block units (X) are soft segments and have rubber elasticity.
[0041] Examples of the aromatic vinyl group forming the block polymer unit (X) include styrene, α-methylstyrene, 3-methylstyrene, p-methylstyrene, 4-propylstyrene, 4-dodecylstyrene, 4-cyclohexylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, etc. Among them, styrene is preferred.
[0042] As the conjugated diene forming the block polymerization unit (Y), butadiene, isoprene, pentadiene, 2,3-dimethylbutadiene and combinations thereof can be cited. Among them, it is preferred to select one or more conjugated dienes from the group consisting of butadiene, isoprene, and a combination of butadiene and isoprene (copolymerization of butadiene·isoprene). Among them, one or more conjugated dienes can also be used in combination. The conjugated diene block polymerization unit (Y) composed of butadiene·isoprene copolymerization units can be any of random copolymerization units, block copolymerization units, and tapered copolymerization units of butadiene and isoprene.
[0043] Regarding the aromatic vinyl / conjugated diene block copolymer as described above, the content of the aromatic vinyl block polymerization unit (X) is preferably 5% by mass or more and 50% by mass or less, more preferably 20% by mass or more and 40% by mass or less. The content of the aromatic vinyl unit can be measured by common methods such as infrared spectroscopy and NMR spectroscopy.
[0044] In one embodiment of the present invention, the melt flow rate (MFR) (temperature of 230°C, load of 2.16 kg) of the styrene-based thermoplastic elastomer is 1 g / 10 minutes or less, preferably 0.1 g / 10 minutes or less. MFR (temperature of 230°C, load of 2.16 kg) refers to the MFR measured under the conditions of temperature of 230°C and load of 2.16 kg based on JIS K7210. By setting the MFR to a certain value or less, it is suppressed that the oil is easily oozed out or the mechanical strength is reduced when the oil is added.
[0045] The aromatic vinyl / conjugated diene block copolymer as described above can be produced by various methods. Examples of the production method include (1) a method in which an aromatic vinyl group and a subsequent conjugated diene are polymerized sequentially using an alkyl lithium compound such as n-butyl lithium as an initiator, (2) a method in which an aromatic vinyl group and a subsequent conjugated diene are polymerized using an alkyl lithium compound as an initiator and the conjugated diene is coupled using a coupling agent, and (3) a method in which a conjugated diene and a subsequent aromatic vinyl group are polymerized sequentially using a lithium compound as an initiator.
[0046] In one embodiment of the present invention, it is preferred to use a substance that the aromatic vinyl / conjugated diene block copolymer as described above is hydrogenated by a known method. The preferred hydrogenation rate is 90 mol% or more. The hydrogenation rate is the value when the total amount of carbon-carbon double bonds in the conjugated diene block polymerization unit (Y) is set to 100 mol%. As this hydrogenated styrene-based thermoplastic elastomer, polystyrene-poly (ethylene / propylene) block (SEP), polystyrene-poly (ethylene / propylene) block-polystyrene (SEPS), polystyrene-poly (ethylene / butylene) block-polystyrene (SEBS), polystyrene-poly (ethylene-ethylene / propylene) block-polystyrene (SEEPS) etc. can be cited. More specifically, SEPTON (manufactured by Kuraray Co., Ltd.), Kraton (manufactured by Shell Chemicals Co., Ltd.), Kraton G (manufactured by Shell Chemicals Co., Ltd.), TAFTEC (manufactured by Asahi Kasei Corporation) (these are trade names) and the like can be cited.
[0047] The hydrogenation rate is measured by a known method such as nuclear magnetic resonance spectroscopy (NMR).
[0048] In the present invention, SEEPS is preferred as the styrene-based thermoplastic elastomer. From the viewpoint of the oil absorption work before kneading, the shape of the styrene-based thermoplastic elastomer is preferably powder or amorphous (particle) form.
[0049] (Oil)
[0050] In one embodiment of the present invention, the conductive resin composition contains oil. As oil, it is not particularly limited, and mineral oils such as paraffin processing oil, naphthenic processing oil, aromatic processing oil, liquid paraffin, silicone oil, castor oil, linseed oil, olefin wax, mineral wax, etc. can be cited. Among them, paraffin and / or naphthenic processing oils are preferred. As processing oil, DIANA processing oil series (manufactured by Idemitsu Kosan Co., Ltd.), JOMO PROCESS P (manufactured by Japan Energy Co., Ltd.) and the like can be cited.
[0051] For example, the oil is used to soften the resin composition and adjust the elastic modulus and hardness of the organ model. One or more of the above oils may be used in combination.
[0052] From the viewpoint of workability, it is preferred to allow the hydrogenated styrene-based thermoplastic elastomer to absorb the oil in advance.
[0053] The content of oil is preferably 100 to 1000 parts by mass, more preferably 100 to 700 parts by mass, further preferably 100 to 600 parts by mass, and most preferably 200 to 500 parts by mass relative to 100 parts by mass of the styrene-based thermoplastic elastomer. The content of oil is adjusted within the above range according to the part of the organ to be actually modeled, etc. The lack of flexibility can be suppressed by setting the content of oil to 100 parts by mass or more relative to 100 parts by mass of the styrene-based thermoplastic elastomer. By setting the content of oil to 1000 parts by mass or less, the inability to form a composite due to the inability of the hydrogenated styrene-based thermoplastic elastomer to completely absorb the oil can be suppressed.
[0054] (Conductive agent)
[0055] In one embodiment of the present invention, the conductive resin composition further contains a conductivity-imparting agent. As the conductivity-imparting agent, a polymer antistatic agent, an ionic liquid, etc. can be used.
[0056] Polymer antistatic agent
[0057] Examples of the polymer antistatic agent include copolymers of a hydrophobic polymer and a hydrophilic polymer, carbon nanomaterials, and conductive polymers.
[0058] ··Copolymers of hydrophobic polymers and hydrophilic polymers
[0059] In one embodiment, it is not particularly limited as a polymer antistatic agent, but preferably a copolymer of a hydrophobic polymer and a hydrophilic polymer, more preferably a copolymer having more than one hydrophobic polymer block and a hydrophilic polymer block, respectively. Hydrophilicity means having a functional group or polarity that forms a hydrogen bond between molecules, and hydrophobicity means non-hydrophilicity. Here, the bonding pattern of each block can be a block copolymer in which a hydrophobic polymer block and a hydrophilic polymer block are linearly connected, or a graft copolymer in which a graft chain is connected to a polymer chain on either side as a branched chain, more preferably a block copolymer. For example, the antistatic agent described in JP-A-2001-278985, JP-A-2013-213195, JP-A-2015-096595, JP-A-2016-166332, JP-A-2017-101217, and International Publication No. 2016 / 084954 can be used as the polymer antistatic agent in one embodiment of the present invention.
[0060] More specifically, polyethers having a hydrophilic group and block copolymerization (nonionic types such as polyether ester amides, ethylene oxide-epichlorohydrin, and polyether esters, anionic types such as polystyrene sulfonic acid, and cationic types such as quaternary ammonium-containing poly (meth) acrylates) can be cited. Among them, diblock copolymers having a structure in which polyethylene glycol blocks and polypropylene glycol blocks, polyether blocks and polyolefin blocks are bonded via at least one bond selected from ester bonds, amide bonds, ether bonds, urethane bonds, and imide bonds, and block copolymers having a structure in which the blocks are repeatedly and alternately bonded can be used. As an example thereof, a polyether ester having a volume resistivity of 10 5 ~10 11 A block copolymer having a structure in which a polyether block and a polyolefin block of a hydrophilic block with a molecular weight of Ω·cm are repeatedly and alternately bonded. The number average molecular weight (Mn) of the block copolymer is preferably 2,000 to 60,000.
[0061] In addition, as a commercially available copolymer, for example, the products manufactured by Sanyo Chemical Industry Co., Ltd. under the trade names "Towers (registered trademark)" ("Towers 300" and "Towers 300") can be cited. "Tower 230", "Tower NC6321", "Tower NC6322", "Tower NC7350", "Tower HC25" 0", etc.), "ペレクトロン (registered trademark)" ("ペレクトロンPVH", "Torotron PVL", "Torotron HS", "Torotron LM" P-FS", etc.), trade names of "Sonko Chemical Industry Co., Ltd. (registered trademark)" ("Sunnoon TBX-65", etc.), Mitsui DuPont Co., Ltd. The copolymers are named “Entera (registered trademark) AS” manufactured by AERO Corp., “Pebacks (registered trademark)” manufactured by Alchema Co., Ltd., “Starter Line (registered trademark)” manufactured by Lubrizol Co., Ltd., “IonPhasE (registered trademark) IPE (registered trademark) U2” manufactured by IonPhasE Co., Ltd., “Pluronic (registered trademark) L-31” and “Pluronic (registered trademark) L-41” manufactured by ADEKA Co., Ltd., and “Alcox (registered trademark) EP1010N” and “Alcox (registered trademark) CP-A1H” manufactured by Meisei Chemical Co., Ltd. These copolymers may be used alone or in combination.
[0062] In addition, polyolefin blocks, polyisobutylene blocks, and polyolefin blocks having a volume resistivity of 1×10 5 ~1×10 11The block polymer obtained by bonding blocks of hydrophilic polymers with a density of Ω·cm is used as the copolymer of this embodiment.
[0063] In addition, a block polymer having a hydrophobic polymer block without polyether, a hydrophilic polymer block, a block polymer having a block of an aromatic ring-containing hydrophobic polyether as a constituent unit, a polyolefin block, and a volume resistivity of 10 5 ~10 11 A block polymer having a structure in which blocks of hydrophilic polymers with a diameter of Ω·cm are repeatedly and alternately bonded, a block polymer having as structural units a block of at least one hydrophobic polymer selected from the group consisting of polyamide, polyolefin and polyamideimide, a block of a hydrophilic polymer, and a block of an aromatic ring-containing hydrophobic polyether, etc.
[0064] The Mn and weight average molecular weight (hereinafter abbreviated as Mw) of the copolymer of the present invention can be measured by gel permeation chromatography (GPC) under the following conditions.
[0065] Device (example): HLC-8321GPC / HT [manufactured by Tosoh Corporation], PL-GPC220 [manufactured by Agilent Technologies Co., Ltd.], SSSC-7100 [manufactured by Seiko Scientific Co., Ltd.]
[0066] Column (one example): "TSK GEL GMH HR-H (20) HT" [manufactured by Tosoh Corporation] 2 pieces
[0067] Measuring temperature: 140℃
[0068] Sample solution: 0.3 wt% o-dichlorobenzene solution
[0069] Solution injection volume: 100μl
[0070] Detection device: FT-IR detector
[0071] Reference material: Standard polystyrene (TSKstandard POLYSTYRENE) 12 points (molecular weight: 500, 1050, 2800, 5970, 9100, 18100, 37900, 96400, 190000, 355000, 1090000, 2890000) [manufactured by Tosoh Corporation]
[0072] ··Carbon nanomaterials
[0073] As the carbon nanomaterial, carbon nanotubes, carbon nanofibers, and the like can be used.
[0074] The content of the carbon nanomaterial is preferably 10 to 1000 parts by mass, more preferably 100 to 800 parts by mass, and further preferably 200 to 800 parts by mass relative to 100 parts by mass of the styrene-based thermoplastic elastomer. By setting the content of the carbon nanomaterial to 10 parts by mass or more relative to 100 parts by mass of the styrene-based thermoplastic elastomer, a volume resistivity below a certain level is achieved, and by setting the content to 1000 parts by mass or less, a decrease in flexibility can be suppressed.
[0075] ··Conductive polymer
[0076] As the conductive polymer, a water-soluble polymer hydrogel, a polythiophene-based conductive polymer, or the like can be used.
[0077] The content of the conductive polymer is preferably 50 to 1000 parts by mass, more preferably 100 to 800 parts by mass, and still more preferably 200 to 800 parts by mass relative to 100 parts by mass of the styrene-based thermoplastic elastomer. By setting the content of the conductive polymer to 50 parts by mass or more relative to 100 parts by mass of the styrene-based thermoplastic elastomer, a volume resistivity below a certain level is achieved, and by setting the content to 1000 parts by mass or less, a decrease in mechanical strength can be suppressed.
[0078] The content of the polymer antistatic agent is preferably 10 to 200 parts by mass, more preferably 100 to 150 parts by mass, relative to 100 parts by mass of the styrene-based thermoplastic elastomer. When the content of the polymer antistatic agent is 10 parts by mass or more relative to 100 parts by mass of the styrene-based thermoplastic elastomer, an increase in volume resistivity can be suppressed, and when the content is 200 parts by mass or less, an increase in hardness of the material can be suppressed.
[0079] -Ionic Liquids-
[0080] The ionic liquid is not particularly limited, and examples thereof include those composed of cations and anions. The ionic liquid according to one embodiment of the present invention does not contain a solvent such as water or ethylene glycol.
[0081] As the cation, an amidine cation, a pyridinium cation, a pyrazoline cation, a guanidinium cation, or the like can be used.
[0082] As the anion, an anion obtained by removing a proton from an acid such as carboxylic acid, sulfonic acid, inorganic acid, halogen-containing alkyl-substituted inorganic acid, halogen-containing sulfonyl imide, halogen-containing sulfonylmethane, halogen-containing carboxylic acid amide, nitrile-containing imide, nitrile-containing methane, halogen-containing alkylamine, cyanic acid, etc. can be used. The anion may be a mixture of two or more.
[0083] In addition, commercially available ionic liquids may be used. Examples of commercially available ionic liquids include CIL312 (N-butyl-3-methylpyridinium bistrifluoromethanesulfonimide, manufactured by Nippon Kakit Co., Ltd.), Amino AS100 (manufactured by Nippon Emulsifier Co., Ltd.), Amino AS300 (manufactured by Nippon Emulsifier Co., Ltd.), FC-4400 (tri-n-butylmethylammonium bistrifluoromethanesulfonimide, manufactured by 3M Co.), and Hi-Colin (dodecyltributylphosphonium chloride, manufactured by Nippon Chemical Industry Co., Ltd.).
[0084] The method for synthesizing ionic liquids is not particularly limited as long as the target ionic liquid can be obtained, and examples thereof include the halide method, hydroxide method, acid ester method, complex method, and neutralization method described in "Ionic Liquids - The Frontier and Future of Development" [Ono Hiroyuki, published in 2003, CMC Publishing].
[0085] The content of the ionic liquid is preferably 50 to 250 parts by mass, more preferably 50 to 240 parts by mass, and even more preferably 70 to 210 parts by mass relative to 100 parts by mass of the styrene-based thermoplastic elastomer. Setting the content of the ionic liquid to 50 parts by mass or more relative to 100 parts by mass of the styrene-based thermoplastic elastomer helps to suppress the increase in volume resistivity and impart flexibility, while setting it to 250 parts by mass or less can suppress the oozing of the ionic liquid from the material.
[0086] (Other additives)
[0087] The conductive resin composition of the present invention can be used in combination with the above-mentioned other resins, elastomers, rubbers, plasticizers, fillers, stabilizers, anti-aging agents, light resistance enhancers, ultraviolet absorbers, softeners, lubricants, processing aids, colorants, anti-fogging agents, anti-blocking agents, crystallization nucleating agents, foaming agents, etc. as needed.
[0088] In particular, when the conductive resin composition of the present embodiment is used as an organ model, it is preferred to color the organ model with a color similar to that of a biological organ using a colorant such as a pigment or a dye within a range not hindering the purpose.
[0089] In one embodiment of the present invention, the conductive resin composition contains a styrene-based thermoplastic elastomer, a polymer antistatic agent, an ionic liquid, and oil.
[0090] In order to manufacture the conductive resin composition of the present invention, a known appropriate mixing method can be used. For example, a single-screw or twin-screw screw extruder, a Banbury mixer, a sandblasting mill, a co-kneader, a heating roller, etc. can be used for melt mixing. Before melt mixing, each raw material can be uniformly mixed in advance using a Henschel mixer, a ribbon blender, a super mixer, a drum, etc. The melt mixing temperature is not particularly limited, and is generally 100 to 300° C., preferably 150 to 250° C.
[0091] [Adhesive layer]
[0092] The adhesive layer of this embodiment is a layer formed of an adhesive, such as Figure 1 As shown, it is one layer constituting the conductive resin composition-metal laminate, and is directly laminated on the base material layer.
[0093] In one embodiment of the present invention, the average thickness of the adhesive layer is 500 μm or less, preferably 350 μm or less, more preferably 200 μm or less, and further preferably 50 μm or less. The lower limit of the average thickness of the adhesive layer is not particularly limited within the scope of implementation, and can be set to 5 μm or more and 10 μm or more, or 20 μm or more. The thickness of the adhesive layer is set to 500 μm or less to suppress the volume resistivity, and the conductive resin composition-metal laminate becomes soft, which can improve the tracking property relative to the curved surface. In addition, the thickness of the adhesive layer is set to 5 μm or more, so that the bonding force between the conductive resin composition molded product and the metal layer can reach a certain degree or more.
[0094] As described later, the adhesive layer is usually formed by coating. When formed by coating, the thickness referred to here means the thickness after drying.
[0095] 20 mm square slices were cut from 5 locations at equal intervals in the width direction of the laminate, and the end faces were smoothed so that the layer structure could be determined. Then, the layer thickness was measured using a laser microscope (Keyence: VK-8510). The average thickness of the adhesive layer was measured at 5 locations, and the arithmetic mean was taken as the average thickness.
[0096] (Adhesive)
[0097] As the adhesive forming the adhesive layer, one or more adhesives selected from the group consisting of epoxy adhesives, olefin adhesives, cyanoacrylate adhesives, urethane adhesives, and silicone adhesives can be preferably used.
[0098] Epoxy adhesives include all adhesives of the type that cure compounds having two or more reactive epoxy groups using various curing agents such as amine compounds, polyamide compounds, dicyandiamide, and imidazole compounds. Specific examples of epoxy adhesives include adhesives composed of a main agent selected from liquid modified epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, and novolac epoxy resin, and an amine curing agent such as a chain aliphatic amine, a cyclic aliphatic amine, and an aromatic amine, an aminoamine curing agent, and the like.
[0099] Examples of olefin adhesives include homopolymers of olefins such as ethylene, propylene, butene, and hexene, and copolymers of the above monomers or the above monomers with non-olefin monomers. Specific examples of olefin adhesives include ethylene resins such as low-density polyethylene, linear polyethylene (ethylene-α-olefin copolymers), and high-density polyethylene, propylene resins such as polypropylene and ethylene-propylene copolymers, poly(4-methylpentene-1), poly(butene-1), ethylene-vinyl acetate copolymers, and acid-modified polyolefin resins obtained by modifying (treating) the above with maleic anhydride, and the like. The above may be used alone or in combination of two or more.
[0100] Cyanoacrylate adhesive refers to a composition containing 2-cyanoacrylate as a polymerized main component. As 2-cyanoacrylate, 2-cyanoacrylate alkyl esters, 2-cyanoacrylate cycloalkyl esters, 2-cyanoacrylate alkoxyalkyl esters, 2-cyanoacrylate alkenyl esters, 2-cyanoacrylate alkynyl esters, 2-cyanoacrylate fluoroalkyl esters, silicon-containing 2-cyanoacrylates, etc. can be cited. Among them, as specific examples of 2-cyanoacrylate alkyl esters, 2-cyanoacrylate methyl esters, 2-cyanoacrylate ethyl esters, various 2-cyanoacrylate propyl esters, various 2-cyanoacrylate butyl esters, various 2-cyanoacrylate pentyl esters, various 2-cyanoacrylate hexyl esters, various 2-cyanoacrylate octyl esters, etc. can be cited. As specific examples of 2-cyanoacrylate alkoxyalkyl esters, 2-cyanoacrylate ethoxyethyl esters, 2-cyanoacrylate methoxyethyl esters, 2-cyanoacrylate methoxyisopropyl esters, etc. can be cited.
[0101] The urethane adhesive is preferably an adhesive composed of at least one polyol component having at least two hydroxyl groups in the molecule and at least one polyisocyanate component having at least two isocyanate groups in the molecule and / or diisocyanate. The polyol component can be appropriately selected from polyester polyol, polyether polyol, acrylic polyol, polyolefin polyol, etc., and polyester polyol is particularly preferred because of its high function of suppressing the decrease in adhesion to the ink layer over time. As diisocyanates, aromatic diisocyanates such as 4,4'-, 2,4'- and 2,2'-diisocyanate diphenylmethane, 1,5-diisocyanate naphthalene, 4,4'-diisocyanate dicyclohexylmethane, 1,4-diisocyanate benzene, and / or 2,4- or 2,6-diisocyanate toluene, and aliphatic and alicyclic diisocyanates such as 1,6-diisocyanate hexane, 1,10-diisocyanate decane, 1,3-diisocyanate cyclopentane, 1,4-diisocyanate cyclohexane, 1-isocyanate-3,3,5-trimethyl-3 or -5-isocyanate methane cyclohexane can be exemplified. The polyisocyanate component can be prepared from the above diisocyanate monomers. Specific examples include "Ultra Multi-Purpose SU-Multimeter" manufactured by CORNIS Corporation under the trade name "UltraMulti-Purpose SU-Multimeter".
[0102] The silicone adhesive means an adhesive having a hydrolyzable silyl group as a reactive group and a modified silicone polymer having a polyoxyalkylene skeleton as a main chain as a main component. Examples thereof include a material composed of a polymer having hydrolyzable silyl groups at both ends of polyoxypropylene in the main chain. For example, commercially available silicone adhesives include SuperX Clean (manufactured by Semidyne Co., Ltd.) and the like.
[0103] In one embodiment of the present invention, the adhesive layer may contain metal particles such as copper, silver, gold, tin, nickel, titanium, platinum, and the above-mentioned additives. Its content is preferably 10 to 70% by mass in the composition constituting the adhesive layer, more preferably 15 to 60% by mass, and further preferably 20 to 50% by mass. When metal particles are added, the volume resistivity is set to 10% or more to a certain extent, and the volume resistivity is set to 70% or less to suppress the decrease in adhesion.
[0104] In one embodiment of the present invention, the average particle size of the metal particles is preferably 0.01 to 50 μm, more preferably 0.03 to 30 μm, and further preferably 0.03 to 10 μm. Here, the average particle size refers to the average primary particle size, which is a value measured by a laser diffraction / scattering particle size distribution measurement method, and is the particle size of 50% of the cumulative value in the volume-based particle size distribution. Two or more metal particles with different average particle sizes can be used, and metal particles can also be particles covered with metals.
[0105] [Metal layer]
[0106] A metal layer refers to a layer formed of metal, such as Figure 1 As shown, it is a layer constituting one surface of the conductive resin composition-metal laminate. As the metal layer, for example, metal foils or metal thin films of aluminum, nickel, stainless steel, iron, copper, titanium, etc. can be used.
[0107] In one embodiment of the present invention, the average thickness of the metal layer is preferably 5 to 500 μm, more preferably 5 to 200 μm, and further preferably 10 to 100 μm. The thickness of the metal layer is set to 5 μm or more to improve handling properties. In addition, the thickness of the metal layer is set to 500 μm or less to improve the followability of the conductive resin composition-metal laminate to a curved surface.
[0108] 20 mm square slices were cut from 5 locations at equal intervals in the width direction of the laminate, and the end faces were smoothed so that the layer structure could be determined. Then, the layer thickness was measured using a laser microscope (Keyence: VK-8510). The average thickness of the adhesive layer was measured at 5 locations, and the arithmetic mean was taken as the average thickness.
[0109] [Second Embodiment]
[0110] The organ model according to the second embodiment of the present invention is an organ model for medical surgery training, comprising the conductive resin composition-metal laminate according to the first embodiment. Figure 2 2 is a diagram showing a cross section of the organ model of the present embodiment. The organ model may have any shape selected from a circular shape, an elliptical shape, a polygonal shape, or an irregular shape.
[0111] The maximum width of the organ model in a direction perpendicular to the thickness direction can be set to a range corresponding to the spread of a general ulcer, for example, 10 to 150 mm. The thickness of the organ model is not particularly limited, and can be about 1 to 30 mm, or about 2 to 20 mm.
[0112] The organ model of this embodiment can be assembled into organ models of the stomach, esophagus, duodenum, small intestine, large intestine, liver, spleen, bile duct, pancreas, lung, heart, etc., and used for training medical surgical techniques such as endoscopic hemostasis.
[0113] In one embodiment of the present invention, the organ model can be embedded in a model assembly part provided on the organ model for use, or can be pasted to the inner wall of the organ model for use. The model assembly part of the organ model can be a frame or a recessed part formed by a part of the wall being missing, and the clamp for model assembly can be installed on the inner wall of the digestive organ model. The organ model can be pasted to the inner wall using adhesives, bonding agents, double-sided tape, etc.
[0114] The organ model of this embodiment can be formed by a known molding method. For example, in the case of injection molding using an internal mold (core) and an external mold in the space between them, when the internal mold is removed, a cut is sometimes formed in the resin molded body and the internal mold is removed from there, but at this time, the cut can also be bonded to complete the organ model. In addition, multiple organ parts can be molded separately by injection molding, etc., and then bonded to complete the organ model.
[0115] Medical surgical technique training refers to training used to improve the skills of doctors and medical students and improve the quality of medical practice, including, for example, medical surgical technique training conducted under endoscopic observation, medical surgical technique training conducted under ultrasonic observation, etc.
[0116] In one embodiment of the present invention, the organ model for medical surgical technique training is used for medical surgical technique training using energy devices, such as high-frequency hemostatic forceps, electric scalpels, ultrasonic scalpels, high-frequency radio scalpels, thermal probes, microwave scalpels, laser scalpels, etc.
[0117] Specific examples of medical procedures include endoscopic mucosal resection, endoscopic submucosal dissection, and endoscopic hemostasis.
[0118] An organ model according to one embodiment of the present invention includes a simulated blood vessel connected to a device capable of supplying simulated blood. Figure 3 : is a diagram showing a cross section of the organ model of this embodiment. The simulated blood vessel is a path for supplying simulated blood to the side surface of the base material layer of the organ model during hemostasis training, and penetrates the organ model. As any device capable of supplying simulated blood, for example, a tube pump or a syringe can be used.
[0119] In one embodiment of the present invention, the simulated blood vessel is a tubular structure including a tubular base material layer and a conductive layer disposed on the outer surface of the base material layer, and capable of being electrified by an energy device.
[0120] The simulated blood vessel according to one embodiment of the present invention has a 1.0×10 0 Ω / □ or more and 1.0×10 6 Surface resistivity below Ω / □.
[0121] In the present embodiment, the surface resistance value is measured at 23±1° C. according to JIS C2139 using Hiresta UX MCP-HT800 and Loresta-GP (MCP-T610) manufactured by Mitsubishi Chemical Analytical Science Co., Ltd. During the measurement, the thermoplastic resin composition is press-molded at a temperature of 160 to 200° C. to form a resin sheet of 2.5 cm×2.5 cm and 1.0 mm in thickness, and the evaluation is performed using a test body having a conductive layer formed on the surface.
[0122] The organ model according to one embodiment of the present invention can be used for training of endoscopic hemostasis. Endoscopic hemostasis includes so-called mechanical methods such as grasping a bleeding site with hemostats or clips, and thermal coagulation methods such as thermal coagulation methods using energy devices.
[0123] Example
[0124] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0125] Various raw materials and production methods used in Examples and the like are as follows.
[0126] (A) Base material layer
[0127] Hydrogenated styrene thermoplastic elastomer: SEEPS (SEPTON 4055, manufactured by Kuraray Co., Ltd.) (MFR (temperature: 230°C, load: 2.16 kg) 0.0 g / 10 min (0.0 g / 10 min means no flow), styrene content: 30% by mass, hydrogenation rate: 90 mol% or more)
[0128] ・Oil: Paraffin oil (ダイアナプロセスオイルPW90, manufactured by Idemitsu Kosan Co., Ltd.)
[0129] ·Polymer antistatic agent: polyolefin / polyether copolymer (ペレクトロン PVL, manufactured by Sanyo Chemical Industries, Ltd.) (MFR (measured at a temperature of 190°C and a load of 2.16 kg) 8 to 15 g / 10 minutes)
[0130] ·Ionic liquid as a conductivity imparting agent: CIL-312 (manufactured by Nippon Carit Co., Ltd.)
[0131] (B) Adhesive layer
[0132] Adhesive 1: Epoxy adhesive, Aram Cobond 556 (manufactured by Aram Projects, silver content 20 to 40% by mass, two-liquid mixed reaction type)
[0133] Adhesive 2: Olefin adhesive, TK-PS CN-7120 (manufactured by Kaken Tech Co., Ltd., silver content: 50 mass %)
[0134] Adhesive 3: Cyanoacrylate adhesive, PPX (manufactured by Semidine Co., Ltd.)
[0135] ·Adhesive 4: Urethane adhesive, Multi-Purpose SUプレレミアムソフト (manufactured by Kortex Co., Ltd.)
[0136] Adhesive 5: Silicone adhesive, Super X Clear (manufactured by Semidine Co., Ltd.)
[0137] (C) Metal layer
[0138] Aluminum foil, FOIL (Mitsubishi Aluminum Co., Ltd., thickness 12 μm)
[0139] (D) Adhesive gel
[0140] · Polyacrylic acid·polyvinyl alcohol (PVA) gel (TG-3, manufactured by Sekisui Chemicals Co., Ltd.)
[0141] (Manufacture and evaluation of conductive resin composition-metal laminate)
[0142] [Examples 1-10]
[0143] First, a conductive resin composition containing 100 parts by mass of a hydrogenated styrene-based thermoplastic elastomer, 500 parts by mass of oil, 40 parts by mass of a polymer antistatic agent, and 130 parts by mass of an ionic liquid was prepared.
[0144] As Examples 1-10, an adhesive layer was formed between the substrate layer and the metal layer using adhesives 1-5 with a thickness as shown in Table 1, and the 180° peel strength between the substrate layer and the adhesive layer, the tensile shear bonding strength between the substrate layer and the adhesive layer, and the volume resistivity of the conductive resin composition-metal laminate were measured by the following method.
[0145] 180° peel strength
[0146] Test piece 1 was prepared by bonding a conductive resin composition molded article (substrate layer) having a width of 10 mm, a length of 70 mm, and a thickness of 1 mm to an acrylic plate having a width of 25 mm, a length of 100 mm, and a thickness of 2 mm using an adhesive (PPX manufactured by Semidine Corporation).
[0147] Next, an OPP tape (manufactured by Nitomuz Co., Ltd., product name: Transparent Packaging Tape No. 3303) was attached to the aluminum foil (metal layer) so that air would not enter the gap, and a test piece 2 cut into a width of 10 mm and a length of 150 mm was prepared.
[0148] Adhesives 1 to 5 were uniformly applied to the aluminum foil surface of the test piece 2 using a Beka Precipitator (manufactured by Yoshimitsu Seiki Co., Ltd., model: YBA type). Immediately after applying adhesives 1 to 3, adhesives 4 and 5 were left for 10 minutes, and then bonded to the surface of the base material layer of the test piece 1 with a bonding area (width 10 mm, length 70 mm), and aged for 24 hours in an environment of a temperature of 23±2°C and a relative humidity of 50%±5% to cure the adhesives and form an adhesive layer, thereby producing a test piece 3.
[0149] According to JIS K6854-2, at a temperature of 23±2°C, the ends of the aluminum foil and the acrylic plate of the obtained test piece 3 were clamped respectively using a tensile testing machine (model: AUTOGRAPH AG-X plus) manufactured by Shimadzu Corporation, and the maximum force and the minimum force during 180° peeling were measured over a peeling length of at least 50 mm after removing the initial 10 mm at a distance between the chucks of 80 mm and a tensile speed of 50 mm / min, and the arithmetic mean of the maximum force and the minimum force was calculated.
[0150] Tensile shear bond strength
[0151] Test piece 1 was prepared by bonding a conductive resin composition molded product (substrate layer) having a width of 10 mm, a length of 70 mm, and a thickness of 1 mm to an acrylic plate having a width of 25 mm, a length of 100 mm, and a thickness of 2 mm using a cyanoacrylate adhesive (PPX manufactured by Semidine Corporation).
[0152] Next, an OPP tape (manufactured by Nitomuz Co., Ltd., product name: Transparent Packaging Tape No. 3303) was attached to the aluminum foil (metal layer) so that air would not enter the gap, and a test piece 2 cut into a width of 10 mm and a length of 100 mm was prepared.
[0153] Adhesives 1 to 5 were uniformly applied to the aluminum foil surface of the test piece 2 using a Beka Precipitator (manufactured by Yoshimitsu Seiki Co., Ltd., model: YBA type). Immediately after applying adhesives 1 to 3, adhesives 4 and 5 were left for 10 minutes, and then bonded to the surface of the base material layer of the test piece 1 with a bonding area (width 10 mm, length 10 mm), and aged for 24 hours in an environment of a temperature of 23±2°C and a relative humidity of 50%±5% to cure the adhesives and form an adhesive layer, thereby producing a test piece 3.
[0154] The ends of the aluminum foil and acrylic plate of the obtained test piece 3 were clamped at a temperature of 23±2°C using a tensile testing machine (model: AUTOGRAPHAG-X plus) manufactured by Shimadzu Corporation, and the maximum breaking force was measured at a distance between the clamps of 80 mm and a tensile speed of 50 mm / min. The value was calculated by dividing the strength by the bonding area (width: 10 mm, length: 10 mm).
[0155] Volume resistivity
[0156] Adhesives 1 to 5 were evenly applied to the aluminum foil (metal layer) using a bakelite (manufactured by Yoshimitz Seiki Co., Ltd., model: YBA type). Immediately after applying adhesives 1 to 3, adhesives 4 and 5 were left for 10 minutes. Then, a conductive resin composition molded product (substrate layer) having a width of 25 mm, a length of 25 mm, and a thickness of 1 mm was joined with a bonding area (width of 25 mm, length of 25 mm). The product was aged for 24 hours at a temperature of 23±2°C and a relative humidity of 50%±5% to cure the adhesive and form an adhesive layer, thereby producing a test piece (conductive resin composition-metal laminate). After the test piece was adjusted in an environment of temperature of 23±2°C and relative humidity of 50±5% for more than 24 hours, the volume resistivity of the surface on the substrate layer side of the test piece was measured using a resistivity meter Loresta-GP (model: MCP-T610) manufactured by Mitsubishi Chemical Analysis Co., Ltd. after power was turned on with a PSP probe at a voltage of 10 V for 20 seconds.
[0157] Table 1 shows the results.
[0158] [Table 1]
[0159]
[0160] As can be seen from Table 1, conductive resin composition-metal laminates can be produced using Adhesives 1 to 5.
[0161] In particular, the cyanoacrylate adhesive of Adhesive 3 has a 180° peel strength of 3.5 N / 10 mm or more and a tensile shear adhesive strength of 0.1 N / mm. 2 As described above, a significant increase in volume resistivity is not observed, and the composite can be preferably used.
[0162] In addition, in order to evaluate the adhesion between the conductive resin composition-metal laminate and the electrode plate, the 180° peel strength and tensile shear bonding strength of the metal layer side of the conductive resin composition-metal laminate of Example 3 and the electrode plate (Erbe Company, thickness 1.0 mm) were measured. The 180° peel strength was 1.6 N / 10 mm, and the tensile shear bonding strength was 0.06 N / mm 2 As described above, it was confirmed that the counter electrode plate can be attached to the surface of the metal layer side of the conductive resin composition-metal laminate of Example 3 with a certain degree of adhesive strength and used for medical surgery training using energy equipment.
[0163] [Comparative Example 1]
[0164] As Comparative Example 1, an adhesive gel used when sticking the electrode plate to the skin was used instead of the adhesive, and the 180° peel strength between the structure composed of the conductive resin composition and the adhesive gel and the tensile shear bonding strength between the structure composed of the conductive resin composition and the adhesive gel were measured by the same method as in Example 1.
[0165] Table 2 shows the results.
[0166] [Table 2]
[0167] Comparative Example 1 180 degree peel strength (N / 10mm) <0.1 <![CDATA[Tensile shear bond strength (N / mm 2 )]]> <0.01
[0168] It can be confirmed from Table 2 that the structure of the comparative example having no adhesive layer and no metal layer shows that the adhesive gel does not adhere with a certain degree of adhesive force and cannot be attached to the counter electrode plate with sufficient strength.
[0169] Industrial Applicability
[0170] The conductive resin composition-metal laminate of the present invention can be used for training of medical surgical techniques using energy devices.
[0171] Description of Reference Numerals
[0172] 1 Conductive resin composition-metal laminate
[0173] 2. Substrate layer
[0174] 3 Adhesive layer
[0175] 4 Metal Layer
[0176] 5. Blood vessel simulation
Claims
1. A conductive resin composition-metal laminate, comprising: a substrate layer formed of a conductive resin composition containing a styrene-based thermoplastic elastomer; and a metal layer laminated on one surface of the base material layer via the adhesive layer.
2. The conductive resin composition-metal laminate according to claim 1, wherein The volume resistivity is 1.0×10 2 ~1.0×10 7 Ω·cm.
3. The conductive resin composition-metal laminate according to claim 1 or 2, wherein: The adhesive layer contains one or more adhesives selected from the group consisting of epoxy adhesives, olefin adhesives, cyanoacrylate adhesives, urethane adhesives, and silicone adhesives.
4. The conductive resin composition-metal laminate according to claim 1 or 2, which is connected to a counter electrode plate.
5. An organ model for training medical surgical techniques, comprising the conductive resin composition-metal laminate according to claim 1 or 2.
6. The organ model according to claim 5, wherein: Medical surgery technique training is the training of medical surgery technique using energy equipment.
7. The organ model according to claim 6, wherein: The energy device is any one selected from the group consisting of high-frequency hemostatic forceps, electric scalpels, ultrasonic scalpels, and high-frequency radio scalpels.
8. The organ model according to claim 5, comprising a simulated blood vessel connected to a device capable of supplying simulated blood.
9. The organ model according to claim 5, wherein: Medical surgical technique training is endoscopic hemostasis training.
10. The organ model according to claim 9, wherein: Endoscopic hemostasis training is based on hemostasis training using thermal coagulation using an energy device.
Citation Information
Patent Citations
Ethylene-vinyl alcohol copolymer, resin composition, and molded article using same
CN106795232A
Laminate comprising low dielectric constant adhesive layer
CN107109182A
Conductive resin composition and model for manipulation training prepared therewith
JP2019065080A
Improved noise prevention shim