Structured CO2 alginate-based adsorbent and preparation method thereof

By using structured CO2 alginate-based adsorbents with organic amines loaded with sodium alginate and porous materials, the problems of low thermal stability and poor dispersion of solid amine adsorbents are solved, and efficient CO2 adsorption and circulation stability are achieved, which is suitable for the use of structured CO2 alginate and porous materials. Industrial application.

CN118925678APending Publication Date: 2024-11-12NANJING TECH UNIV +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411351050.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing solid amine adsorbents have problems in industrial applications with low thermal stability, poor dispersion and equipment corrosion, and the preparation method is complex, which limits the further development of their CO2 capture and storage technology.

Method used

Sodium alginate is used as the binder, porous material is used as the carrier, and organic amine is loaded with organic amines. Structured CO2 alginate-based adsorbent is prepared by impregnation method to form a molded solid amine adsorbent, which improves the adsorption amount and stability and simplifies preparation. process.

Benefits of technology

It significantly improves CO2 adsorption capacity and stability, reduces preparation costs, is suitable for industrial scale promotion, reduces CO2 mass transfer resistance, improves amine efficiency, and reaches 2.5mmol/g, with good cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925678A_ABST
    Figure CN118925678A_ABST
Patent Text Reader

Abstract

The invention discloses a structured CO2 alginate-based adsorbent and a preparation method thereof. The structured CO2 alginate-based adsorbent comprises the following main components: alginate serving as an adhesive, one or more porous material carriers and organic amine loaded on the carriers. The problem that the application of an existing powdery solid amine adsorbent is limited by pressure drop in industrial application is solved by adopting one-step forming, the existence of the carrier can effectively prevent amine from overflowing, the preparation process is milder at room temperature, and the prepared CO2 adsorbent has extremely high amine efficiency, can efficiently and rapidly adsorb CO2 molecules, and has a good application prospect. And the existence of sodium alginate in a sample can improve the adsorption and desorption cycle stability of the material. The material has excellent properties, so that the material has large-scale industrial application potential in CO2 adsorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to CO 2 Adsorbents, in particular, structured CO 2 Alginate-based adsorbent and method for preparing the same. Background Art

[0002] In recent years, with the continuous development of science and technology industry, the use of fossil fuels has continued to increase, making the earth's CO 2 The proportion is also gradually increasing, causing environmental and ecological problems such as global warming and ocean acidification. In response to global climate issues, the G8 proposed and popularized CO 2 Capture and storage (CCS) technology is the process of CO 2 It is separated from industrial or other emission sources such as power plants, enriched, compressed and transported to a specific location, and injected into the reservoir for storage to achieve the captured CO 2 Technology for long-term separation from the atmosphere. 2 In emission reduction technology, the adsorbent made by introducing organic amines on a porous substrate is used to 2 Cyclic adsorption and desorption is considered to be a promising technology. The adsorbent obtained by this method has high adsorption capacity and strong selectivity. However, the corrosion of liquid amine adsorbent to equipment and the difficulty of regeneration have always been a difficulty in the application process, limiting its further development. Compared with the liquid amine absorption method, solid amine adsorbent can treat CO 2 It has the advantages of good selectivity, no equipment corrosion, and simple operation, which has attracted great attention from the scientific and industrial communities.

[0003] However, existing solid amine adsorbents are in the form of powders, which often have problems such as pressure drop in industrial applications and limit their application. 2 Adsorbent and preparation method thereof (CN110548486A), the patent prepares a carrier by mixing a metal organic framework, an inorganic substance and a first molding aid, and then sequentially grinding, extruding and first drying, and then mixing an amino modified solution with the carrier, sequentially standing and second drying, to prepare CO 2Adsorbent. Although the prepared carrier can increase the specific surface area of ​​the adsorbent, which is beneficial to the dispersion of the active ingredients and thus increases the adsorption capacity of the adsorbent, the extrusion molding process is limited by the shape of the mold, the structural design of the extrudate cannot be flexibly changed, and objects with discontinuous structures cannot be prepared. Zhao Chen, Tian Jingqing and others disclosed a MOF molding material for low-temperature carbon dioxide capture (CN113663649A). The patent first makes MOF grow all over the surface of honeycomb ceramics, and then treats it with diamine to obtain an amine-modified molded high-performance adsorbent material. Compared with powder MOF, the monolithic adsorbent material grown in situ on porous ceramics has excellent mechanical strength, and the honeycomb porous structure significantly reduces the bed pressure drop of the adsorption bed. It also has high adsorption capacity and cycle stability, but the complex preparation method leads to high cost. Yan Guibin, Zuo Jianbo and others disclosed a CO 2 Adsorbent and preparation method thereof (CN114700043A), the patent prepares a mixture of organic amine and porous carrier, loads the organic amine on the surface and pores of the porous carrier in a few layers, and then granulates the mixture using a dry granulator. However, the above method requires specific machinery and equipment, which is not conducive to industrial application.

[0004] In order to solve the above problems, the present invention has developed a structured alginate-based CO 2 The adsorbent is sodium alginate (SA) as a binder, a carrier as a dispersant, and an organic amine as a CO 2 Adsorption active sites form a shaped solid amine adsorbent, which can provide better gas-solid contact and enhance CO 2 The diffusion of fluid in the bed enables solid amine adsorbents to exhibit better adsorption / desorption performance in industrial application devices. So far, there are few studies on the one-step preparation of structured adsorbents, and their application in the adsorption of CO 2 No research has been reported yet. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a structured CO 2 Alginate-based adsorbent and preparation method thereof; the invention improves the amine efficiency of solid amine adsorbent materials and solves the problems of low thermal stability and poor dispersibility of solid amine adsorbents.

[0006] The present invention is achieved through the following technical solutions:

[0007] A structured CO 2 The alginate-based adsorbent mainly comprises alginate as a binder, a porous material carrier and an organic amine loaded on the carrier.

[0008] Furthermore, the carrier is a three-dimensional, two-dimensional or one-dimensional nanomaterial, preferably one of porous silica nanoparticles, porous organic metal frameworks, graphene oxide, carbon nanorods or a mixture of any of them.

[0009] Furthermore, the organic amine is any one of polyethyleneimine (PEI), diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), triethanolamine (TEA), or a mixture of any of them.

[0010] More preferably, the organic amine is tetraethylenepentamine (TEPA).

[0011] Further, the mass ratio of the sodium alginate, the carrier, and the organic amine is 1:1-9:15-35; more preferably, the mass ratio of the sodium alginate, the carrier, and the organic amine is 1:2-8:20-28, and more preferably, the mass ratio of the sodium alginate, the carrier, and the organic amine is 1:3-5:23-28. In the process of implementing the present invention, the inventors found that under this ratio, the properties of the prepared adsorbent material better meet the requirements of the adsorbent, and have a better impact on the performance of the finally obtained adsorbent.

[0012] The above structured CO 2 The preparation method of alginate-based adsorbent comprises the following steps:

[0013] The organic amine is loaded on the carrier material by an impregnation method, and sodium alginate is used as a binder. After mixing with water, it is added dropwise to a calcium salt aqueous solution, and after washing and freeze-drying, the structured CO is obtained. 2 Alginate-based adsorbents.

[0014] Furthermore, the preparation method comprises the following specific steps:

[0015] (1) Weigh sodium alginate and carrier materials, add them into water and stir for 10 to 120 minutes;

[0016] (2) then adding an organic amine and stirring for 3 to 12 hours to fully mix;

[0017] (3) The solution in step (2) is then added dropwise to a calcium salt aqueous solution, the resulting pellets are collected and washed with water to remove excess calcium ions, followed by freeze drying to obtain structured CO 2 Alginate-based adsorbents.

[0018] Furthermore, the temperature used in step (1) to step (3) is 0-40° C., and more preferably 25° C. In the process of implementing the present invention, the inventors found that at this temperature, the active sites of the loaded amine can be retained to the greatest extent, and the stability of the obtained adsorbent material is better.

[0019] Furthermore, the stirring time of step (2) is 3 to 5 hours. In the process of implementing the present invention, the inventors found that adopting this condition can ensure that the organic amine is fully loaded.

[0020] Furthermore, in step (3), the calcium salt aqueous solution is CaCl 2 Aqueous solution.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0022] 1. The present invention uses sodium alginate as a binder, a carrier as a dispersant, and an organic amine as a CO 2 The solid amine adsorbent was prepared by a one-step method. 2 The adsorption capacity has been greatly improved, reaching 2.5mmol / g. Compared with the adsorbent synthesized by the conventional grafting method, the adsorption capacity has been increased and the stability has been improved. The adsorption capacity has not decreased significantly in 30 cycles, and it has super high amine efficiency.

[0023] 2. The preparation method of the present invention has low cost and mild synthesis conditions, which is conducive to the promotion of industrial scale. The presence of the porous carrier not only has a rich pore structure inside itself, but also generates large expansion between the carrier particles. These phenomena are conducive to the dispersion of viscous organic amines, improve the efficiency of amines and reduce CO 2 Mass transfer resistance. This effectively increases the CO 2 adsorption capacity.

[0024] 3. Compared with the traditional organic amine absorption method, with the increase of carrier content, the amine agglomeration phenomenon is effectively improved, and the amine efficiency is improved to 0.49mmol / N. At the same time, the addition of sodium alginate also improves the amine efficiency. SA contains a large number of hydroxyl groups, which can change the CO 2 The intermediate product when binding to the amine active site promotes CO 2 The adsorption of amines improves the efficiency.

[0025] 4. Water content increases the adsorbent's CO absorption to a certain extent. 2 The adsorption capacity is large, so the adsorbed gas containing a small amount of water does not need to be pretreated, reducing the process steps. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The adsorbent SA@SA prepared in Example 5 0.18 / T 0.8 Thermogravimetric analysis diagram of .

[0027] Figure 2 The adsorbent SA@SA prepared in Example 5 0.18 / T 0.8 CO2 Adsorption curve.

[0028] Figure 3 The adsorbent SA@SA prepared in Example 5 0.18 / T 0.8 Cyclic stability performance diagram. DETAILED DESCRIPTION

[0029] The present invention will be described in detail below in conjunction with examples, which are only used to describe embodiments of the present invention and should not be construed as limiting the scope of the present invention. In the examples, preparation and performance testing are all normal conditions, and the reagents and instruments used are conventional products that can be purchased commercially if the manufacturer is not indicated.

[0030] Example 1 Structured CO 2 Preparation of alginate-based adsorbents

[0031] 0.03 g of sodium alginate (SA) and 0.12 g of porous silica (referred to as SA) were added to 2 mL of water and stirred for 1 h. Then 0.8 g of tetraethylenepentamine (TEPA) was added to the obtained viscous solution and stirred for 3 h to fully mix the viscous solution. The above solution was taken with a rubber dropper and dropped into a 2 wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SA 0.12 / T 0.8 ).

[0032] Example 2 Structured CO 2 Preparation of alginate-based adsorbents

[0033] 0.03 g SA and 0.12 g porous organic metal framework (MIL-101) (denoted as SB) were added to 2 mL water and stirred for 1 h. Then 0.8 g TEPA was added to the obtained viscous solution and stirred for 3 h to fully mix the viscous solution. The above solution was taken with a rubber dropper and dropped into a 2 wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SB 0.12 / T 0.8 ).

[0034] Example 3 Structured CO 2 Preparation of alginate-based adsorbents

[0035] 0.03 g SA and 0.12 g graphene oxide (SC) were added to 2 mL water and stirred for 1 h. Then 0.8 g TEPA was added to the viscous solution and stirred for 3 h to fully mix the viscous solution. The above solution was taken with a rubber dropper and dropped into a 2 wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SC 0.12 / T 0.8 ).

[0036] Example 4 Structured CO 2 Preparation of alginate-based adsorbents

[0037] 0.03 g SA and 0.12 g carbon nanorods (denoted as SD) were added to 2 mL water and stirred for 1 h. Then 0.8 g TEPA was added to the obtained viscous solution and stirred for 3 h to fully mix the viscous solution. The above solution was taken with a rubber dropper and dropped into a 2 wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SD 0.12 / T 0.8 ).

[0038] Example 5 Structured CO 2 Preparation of alginate-based adsorbents

[0039] 0.03 g SA and 0.18 g porous silica (SA) were added to 2 mL water and stirred for 1 h. Then 0.8 g TEPA was added to the obtained viscous solution and stirred for 3 h to fully mix the viscous solution. The above solution was taken with a rubber dropper and dropped into a 2 wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SA 0.18 / T 0.8 ).

[0040] Example 6 Structured CO 2 Preparation of alginate-based adsorbents

[0041] 0.03 g SA and 0.24 g porous silica (SA) were added to 2 mL water and stirred for 1 h. Then 0.8 g TEPA was added to the obtained viscous solution and stirred for 3 h to fully mix the viscous solution. The above solution was taken with a rubber dropper and dropped into a 2 wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SA 0.24 / T 0.8 ).

[0042] Example 7 Structured CO 2 Preparation of alginate-based adsorbents

[0043] 0.03 g SA and 0.12 g porous silica (SA) were added to 2 mL water and stirred for 1 h. Then 0.8 g polyethyleneimine (PEI) was added to the obtained viscous solution and stirred for 3 h to fully mix the viscous solution. The above solution was taken with a rubber dropper and dropped into a 2 wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SA 0.12 / P 0.8 ).

[0044] Example 8 Structured CO 2 Preparation of alginate-based adsorbents

[0045] 0.03g SA and 0.12g porous silica (SA) were added to 2mL water and stirred for 1h. Then 0.8g diethylenetriamine (DETA) was added to the obtained viscous solution and stirred for 3h to make the viscous solution fully mixed. The above solution was taken with a rubber dropper and dropped into a 2wt.% CaCl 2 The resulting pellets were collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain structured CO 2 Alginate-based adsorbent beads (labeled as SA@SA 0.12 / D 0.8 ).

[0046] Adsorbent adsorption evaluation

[0047] CO 2 The adsorption performance was determined by thermogravimetric analysis. The adsorbent loading was 10.0 mg and the simulated gas was CO. 2After the adsorbent was loaded into the sample tube, it was activated in a nitrogen atmosphere at 100 °C for 0.5 h with a nitrogen flow rate of 50 mL / min. After the temperature in the sample chamber dropped to room temperature, simulated gas was introduced at a gas flow rate of 50 mL / min. 2 The mass change was detected by Mettler thermogravimetric analyzer.

[0048] CO 2 Cyclic stability performance was measured by a heat analyzer. After the adsorbent reached adsorption equilibrium under the adsorption conditions, the temperature was raised to 100 °C in a nitrogen atmosphere and maintained for 30 min. The nitrogen flow rate was 30 mL / min to remove the adsorbed gas, and then the temperature was lowered to the target temperature. 100% CO was repeatedly introduced. 2 , multiple adsorption–desorption cycles were performed to discuss the adsorbent regeneration ability.

[0049] The adsorption performance results of the adsorbents prepared in Examples 1-8 are shown in Table 1 below.

[0050] Table 1 Comparison of adsorption performance of adsorbents in Examples 1-8

[0051]

[0052] Figure 1 The adsorbent SA@SA prepared in Example 5 0.18 / T 0.8 The thermogravimetric curve shows that the weight loss of the sample before 120°C is mainly due to the desorption of water and gas adsorbed by the adsorbent pores. Calcium alginate will begin to decompose at around 150°C due to the destruction of glycosidic bonds. As the temperature continues to rise, the calcium alginate skeleton breaks and cracks to form stable intermediates. The hydroxyl groups are converted into water molecules and removed. The occurrence of dehydration reaction accelerates the destruction of glycosidic bonds. When the temperature rises further, the intermediates decompose, releasing carbon dioxide, and part of the product is carbonized.

[0053] Figure 2 The adsorbent SA@SA prepared in Example 5 0.18 / T 0.8 CO 2 From the adsorption curve in Table 1, it can be seen that Example 5 exhibits the best adsorption performance.

[0054] Figure 3 The adsorbent SA@SA prepared in Example 5 0.18 / T 0.8 Cyclic stability performance diagram of CO at the 1st and 30th cycles 2 The adsorption amounts were 2.49 and 2.24 mmol / g, respectively, which were 9.6% less than that of the first cycle. The decrease in adsorption amount may be due to the volatilization of the small molecule amine TEPA under high temperature conditions, which reduces the amine active sites and leads to a decrease in the adsorption amount.

[0055] It should be understood that the examples and implementation modes described herein are for illustrative purposes only and are not intended to limit the present invention. Those skilled in the art may make various modifications or changes based on the examples and implementation modes. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A structured CO2 alginate-based adsorbent, the main components of which include alginate as a binder, a carrier, and an organic amine loaded on the carrier.

2. The structured CO2 alginate-based adsorbent according to claim 1, characterized in that: The carrier is a three-dimensional, two-dimensional or one-dimensional nanomaterial, preferably one of porous silicon dioxide nanoparticles, porous organic metal frameworks, graphene oxide, carbon nanorods or a mixture of any of them.

3. The structured CO2 alginate-based adsorbent according to claim 1, characterized in that: The organic amine is any one of polyethyleneimine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and triethanolamine, or a mixture of any of the above; Preferably, the organic amine is tetraethylenepentamine.

4. The structured CO2 alginate-based adsorbent according to claim 1, characterized in that: The mass ratio of the sodium alginate, the carrier and the organic amine is 1:1-9:15-35.

5. The structured CO2 alginate-based adsorbent according to claim 4, characterized in that: The mass ratio of the sodium alginate, the carrier and the organic amine is 1:2-8:20-28, and more preferably, the mass ratio of the sodium alginate, the carrier and the organic amine is 1:3-5:23-28.

6. The method for preparing the structured CO2 alginate-based adsorbent according to claim 1, comprising the following steps: The organic amine is loaded on the carrier material by an impregnation method, and sodium alginate is used as a binder. After mixing with water, the mixture is added dropwise into a calcium salt aqueous solution. After washing and freeze-drying, the structured CO2 alginate-based adsorbent is obtained.

7. The preparation method according to claim 6, characterized in that: The preparation method comprises the following specific steps: (1) Weigh sodium alginate and carrier materials, add them into water and stir for 10 to 120 minutes; (2) then adding an organic amine and stirring for 3 to 12 hours to fully mix; (3) The solution in step (2) is then added dropwise to a calcium salt aqueous solution, the resulting pellets are collected and washed with water to remove excess calcium ions, followed by freeze-drying to obtain a structured CO2 alginate-based adsorbent.

8. The preparation method according to claim 7, characterized in that: The temperature used in steps (1) to (3) is 0 to 40°C, more preferably 25°C.

9. The preparation method according to claim 7, characterized in that: The stirring time of step (2) is 3 to 5 hours.

10. The preparation method according to claim 7, characterized in that: In the step (3), the calcium salt aqueous solution is a CaCl2 aqueous solution.