Heterogeneous metal doped iron-based MOF catalyst and preparation method thereof
By using a heterogeneous metal doped iron-based MOF catalyst prepared by multi-stage solvent thermal insulation in the treatment of printing and dyeing wastewater, the Lewis acid level density on the catalyst surface is adjusted, and the problem of difficulty in selective conversion of ROS is solved, and high efficiency is achieved for printing and dyeing wastewater deal with.
Patent Information
- Application Number
- CN202411057261.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
AI Technical Summary
When the existing heterogeneous catalytic ozone oxidation technology treats printing and dyeing wastewater with high salt content and complex water quality, selective conversion of ROS is difficult to achieve, resulting in a reduced treatment efficiency.
By introducing a heterogeneous metal-doped iron-based MOF catalyst, the Lewis acid density on the catalyst surface is regulated, and the selective transduction of·OH or 1O2 is achieved to achieve targeted treatment of specific polluted wastewater. The specific method is to use multi-stage solvent thermal insulation to prepare heterogeneous metal-doped iron-based MOF, and control crystal nucleus growth through oxygen bridge bonding and gradient temperature increase to achieve uniform doping and control of Lewis acid position density.
The Lewis acid density control on the catalyst surface is realized, mediating the selective conversion of ozone to ·OH or 1O2, improving the treatment efficiency of polluted wastewater and providing efficient directional catalytic applications.
Smart Images

Figure CN118925803A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst synthesis, and in particular to a heterogeneous metal-doped iron-based MOF catalyst and a preparation method thereof. Background Art
[0002] In response to the current problem of preventing and controlling polluted wastewater, heterogeneous catalytic ozonation (HCO) technology can not only realize the recovery and reuse of catalysts, but also minimize the secondary pollution caused by residual metal ions. It has outstanding advantages in practical applications and is one of the most promising guarantee measures for deep treatment and resource utilization of wastewater.
[0003] At present, the HCO degradation mechanism recognized by most scholars can be roughly divided into two types: one is to catalyze the decomposition of ozone to produce active oxygen free radicals such as OH, which oxidize organic pollutants adsorbed on the catalyst surface or in the solution, which is called the free radical pathway; the other is the non-free radical pathway, which includes two types: ① catalyzing the ozone reaction chain to produce active oxygen free radicals such as ·OH, which oxidize organic pollutants adsorbed on the catalyst surface or in the solution, which is called the free radical pathway; 1 O2 is the dominant mechanism; ② The catalyst surface chemically adsorbs organic pollutants or ozone to form a catalyst / organic pollutant / ozone surface complex, and the degradation of organic pollutants is achieved through intermolecular electron transfer.
[0004] The ROS generated by the conversion of ozone molecules on the catalyst surface dominate the oxidative degradation process of organic pollutants. From the characteristics of the main reactive oxygen species (ROS), ·OH has a high redox potential (2.8 V vs NHE), but a short lifespan (about 10 -3 μs), no selectivity, poor environmental tolerance; 1 O2 has a moderate redox potential (2.2 V vs NHE), but a long lifetime (2.9-4.6 μs), is selective, and has strong environmental tolerance. Therefore, the two ROS show significant differences in performance in different water quality environments.
[0005] Metal organic framework materials (MOFs) have the characteristics of rich pore structure, unsaturated metal coordination, and modifiable structure design, which can provide a unique solution to the problem of active site exposure and mass transfer enrichment. Among them, the combination of iron-based MOF (Fe-MOFs) materials and HCO technology has shown excellent performance in the deep treatment of printing and dyeing wastewater. In the process of treating polluted wastewater with this combined technology, the dominant ROS are mainly ·OH and / or 1 O2.
[0006] However, printing and dyeing wastewater has the characteristics of high salt content, complex water quality components and variable matrix composition. If the selective conversion of ROS by HCO technology cannot be achieved according to the water quality characteristics, the treatment efficiency of printing and dyeing wastewater will be greatly reduced. Summary of the invention
[0007] The present invention provides a heterogeneous metal doped iron-based MOF catalyst and a preparation method thereof. The present invention explores the mechanism of the influence of doping different heterogeneous metals on the Lewis acid site density on the surface of the iron-based MOF catalyst, and controls the Lewis acid site density by introducing different doping metal types, thereby selectively transducing ·OH or 1 O2, making it possible to treat specific polluted wastewater in a targeted manner.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] The present invention provides a method for preparing a heterogeneous metal-doped iron-based MOF catalyst. The heterogeneous metal-doped iron-based MOF catalyst is obtained by subjecting an N,N-dimethylformamide solution containing a heterogeneous metal source, an iron salt, and terephthalic acid to a solvent thermal reaction and then drying; the heterogeneous metal source is selected from any one of aluminum salts, manganese salts, and magnesium salts; the solvent thermal reaction is: 20 to 30 minutes at 50°C, then 20 to 30 minutes at 100°C, and then 14 to 22 hours at 150°C.
[0010] The present invention provides a method for preparing heterogeneous metal-doped iron-based MOF by multi-stage solvent thermal insulation. The heterogeneous metal atoms and iron atoms are fully combined through oxygen bridge bonds to form more stable crystal nuclei through multi-stage heating. The growth rate of the crystal nuclei can be controlled during the gradient heating process to achieve uniform doping of the heterogeneous metal atoms, thereby achieving regulation of the Lewis acid site density on the surface of the iron-based MOF.
[0011] The three heterogeneous metal atoms selected by the present invention, aluminum, manganese, and magnesium, show different Lewis acid site densities after being doped with iron-based MOF. The applicant conducted DFT calculation simulation on this phenomenon, and the results showed that the oxidizability and electronic structure of the doped heterogeneous metal atoms assisted by multi-stage solvent heat are the key factors for regulating the Lewis acid sites on the surface of iron-based MOF. When the oxidizability is lower than Fe(III), the total acid density of the Lewis acid sites on the surface decreases; when the oxidizability is higher than Fe(III), the total acid density of the Lewis acid sites on the surface increases. The oxidizability of Fe(III) is higher than that of Mn(II) and is much stronger than Al(III). Therefore, aluminum and manganese doping leads to a decrease in the total acid density. Although the oxidizability of Mg(II) is lower than that of Fe(III), the difference in the electronic structure characteristics of Mg(II) and Fe(III) leads to the coordination ability and coordination stability of Mg(II) being weaker than that of Fe(III), and unsaturated metal coordination is easily generated at the doping site, which increases the total acid density of Lewis acid sites on the surface of iron-based MOF.
[0012] Furthermore, the applicant used DFT calculation to simulate the adsorption competition between water molecules and ozone molecules and found that the iron-based MOF material with low Lewis acid site total acid density dominated by ozone molecules tends to catalyze the selective production of ozone. 1 O2, while the high Lewis acid site total acid density iron-based MOF materials with water molecules as the main adsorption tend to catalyze ozone to selectively produce ·OH. Among them, the adsorption energy of aluminum and manganese-doped iron-based MOF catalysts for ozone is greater than that for water, indicating that both are more likely to adsorb ozone molecules in a water environment (dominated by ozone adsorption); while the adsorption energy of magnesium-doped iron-based MOF catalysts for ozone is lower than that for water, indicating that they are more inclined to adsorb water molecules (dominated by water adsorption).
[0013] Furthermore, the applicant correlated the linear relationship between the total acid density of Lewis acid sites on the catalyst surface and the adsorption competition between water molecules and ozone molecules, and found that the Lewis acid sites on the catalyst surface control the adsorption competition between water and ozone molecules, determine the thermodynamic direction of the ozone decomposition reaction, mediate the selective conversion of ozone, and ultimately achieve the OH and 1 Controllable modulation of O2.
[0014] Combining all the above results, it can be seen that magnesium doping leads to an increase in the total acid density of iron-based MOF, which enhances the selective production of ·OH by ozone; while aluminum and manganese doping leads to a decrease in the total acid density of iron-based MOF, mediating the decomposition of ozone to produce ·OH. 1 O2 modulation.
[0015] In summary, the applicants have finally obtained a catalyst with controlled Lewis acid site density by combining multi-stage solvent thermal insulation with heterogeneous metal atoms doped with iron-based MOF. In addition, the applicants have found that heterogeneous metals with different oxidizing properties and electronic structures have different effects on regulating Lewis acid site density on the surface of iron-based MOF under the assistance of multi-stage solvent thermal treatment, thereby making the selective generation of ROS (·OH or 1 O2), which makes the heterogeneous metal atom-doped iron-based MOF catalyst show strong advantages in directional catalysis.
[0016] Preferably, the solvent thermal reaction is: 50°C for 30 min, then 100°C for 30 min, then 150°C for 16 to 20 h.
[0017] Further preferably, the solvent thermal reaction is: 30 min at 50°C, then 30 min at 100°C, then 18 h at 150°C.
[0018] Preferably, the iron salt is selected from any one of ferric nitrate, ferric chloride, ferric sulfate and ammonium ferric citrate.
[0019] Preferably, the aluminum salt is selected from any one of aluminum nitrate, aluminum sulfate and aluminum chloride.
[0020] Preferably, the manganese salt is selected from any one of manganese nitrate, manganese sulfate and manganese chloride.
[0021] Preferably, the magnesium salt is selected from any one of magnesium nitrate, magnesium sulfate and magnesium chloride.
[0022] Preferably, the molar ratio of the heterogeneous metal to iron in the heterogeneous metal source and the iron salt is 1:4.
[0023] Preferably, the ratio between the total molar amount of the heterogeneous metal and iron in the heterogeneous metal source and the iron salt and the molar amount of the terephthalic acid is 1:1.
[0024] Preferably, the drying temperature is 80-120° C., and the drying time is 12-36 hours.
[0025] More preferably, the drying temperature is 100° C. and the drying time is 24 hours.
[0026] The present invention also provides a heterogeneous metal-doped iron-based MOF catalyst prepared by the above preparation method.
[0027] Therefore, the present invention has the following beneficial effects:
[0028] (1) The present invention provides a method for preparing iron-based MOF doped with heterogeneous metal atoms by multi-stage solvent thermal insulation. The heterogeneous metal atoms and iron atoms are fully combined through oxygen bridge bonds to form more stable crystal nuclei by multi-stage heating. The growth rate of the crystal nuclei can be controlled during the gradient heating process to achieve uniform doping of the heterogeneous metal atoms, thereby achieving regulation of the Lewis acid site density on the catalyst surface.
[0029] (2) The present invention doped heterogeneous metal atoms to modify the iron-based MOF catalyst under the assistance of multi-stage solvent thermal treatment. When the saturated coordination number of the heterogeneous metal and iron is the same, the specific metal is selected by selecting the oxidizability between the heterogeneous metal ions and the iron ions and the difference in the electronic structure between the heterogeneous metal ions and the iron ions to achieve the regulation of the Lewis acid sites on the surface of the iron-based MOF, mediate the selective conversion of ozone, and achieve ·OH or 1 Controllable modulation of O2; at the same time, it provides reference and basis for the design and development of other high-efficiency ozone catalysts with adapted Lewis acid site density.
[0030] (3) The heterogeneous metal-doped iron-based MOF catalyst provided by the present invention can mediate the selective conversion of ozone into ·OH or 1 O2, to achieve OH or 1 O2-dominated ozone catalytic system for ·OH or 1 The treatment of highly O2-sensitive polluted wastewater realizes the efficient and directional application of catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 PXRD spectra of undoped and metal-doped MIL-53(Fe)-18H;
[0032] Figure 2 FT-IR spectra of undoped and metal-doped MIL-53(Fe)-18H, where Figure b is an enlarged view of Figure a;
[0033] Figure 3 SEM images of undoped and metal-doped MIL-53(Fe)-18H, where a is MIL-53(Fe)-18H, b is MIL-53(FeMg)-18H, c is MIL-53(FeAl)-18H, and d is MIL-53(FeMn)-18H;
[0034] Figure 4 The BET results of undoped and metal-doped MIL-53(Fe)-18H are shown in Figure 1, where a is the nitrogen adsorption / desorption curve and b is the pore size distribution diagram;
[0035] Figure 5XPS spectra of undoped and metal-doped MIL-53(Fe)-18H, where a is the full spectrum, b is the Mg 1s\Al2p\Mn 2p subdivision spectrum, c is the O1s subdivision spectrum, and d is the Fe 2p subdivision spectrum;
[0036] Figure 6 Py-FTIR spectra of undoped and metal-doped MIL-53(Fe)-18H at different degassing temperatures, where a is MIL-53(Fe)-18H, b is MIL-53(FeMg)-18H, c is MIL-53(FeAl)-18H, and d is MIL-53(FeMn)-18H;
[0037] Figure 7 Solid EPR spectra of undoped and metal-doped MIL-53(Fe)-18H catalytic ozone system, where a is DMPO / ·OH, b is TEMP / 1 O2;
[0038] Figure 8 is the linear relationship between the EPR signal intensity and the total acid density of Lewis acid sites on the surface, where a is ·OH(a) and b is 1 O2;
[0039] Fig. 9 The front and side views of the structures of undoped and metal-doped MIL-53(Fe)-18H catalysts, wherein a is MIL-53(Fe)-18H, b is MIL-53(FeAl)-18H, c is MIL-53(FeMg)-18H, and d is MIL-53(FeMn)-18H;
[0040] Fig.10 The differential charge density diagram of the structures of undoped and metal-doped MIL-53(Fe)-18H catalysts, where a is MIL-53(Fe)-18H, b is MIL-53(FeMg)-18H, c is MIL-53(FeAl)-18H, and d is MIL-53(FeMn)-18H;
[0041] Fig.11 The main view of the undoped and metal-doped MIL-53(Fe)-18H structures adsorbing ozone, E ad s, l O-O , Q e , where a is MIL-53(Fe)-18H, b is MIL-53(FeAl)-18H, c is MIL-53(FeMg)-18H, and d is MIL-53(FeMn)-18H;
[0042] Fig.12The adsorption energies of water and ozone molecules on undoped and metal-doped MIL-53(Fe)-18H structures;
[0043] Fig.13 The main view of the undoped and metal-doped MIL-53(Fe)-18H structures adsorbing water molecules, E ads and the Bader charges of hydrogen atoms at both ends, where a is MIL-53(Fe)-18H, b is MIL-53(FeAl)-18H, c is MIL-53(FeMg)-18H, and d is MIL-53(FeMn)-18H;
[0044] Fig.14 is the total acid density of Lewis acid sites on the surface and the relationship between “AC HQ "The linear relationship;
[0045] Fig.15 is the reaction path and Gibbs free energy of undoped and metal-doped MIL-53(Fe)-18H, where a is the activation ozone production 1 The reaction path and Gibbs free energy of O2, b is the reaction path and Gibbs free energy of HO3;
[0046] Fig.16 is the total acid density of Lewis acid sites on the surface and “S HQ " linear relationship. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0048] [Example]
[0049] Example 1
[0050] Magnesium-doped MIL-53(Fe)-18H was prepared by a solvothermal method. The specific preparation method is as follows: at room temperature, a metal salt mixed with 16mmol FeCl3·6H2O and 4mmol MgCl2·6H2O and 20mmol terephthalic acid (H2BDC) were dissolved in 120mL N,N-dimethylformamide (DMF) to obtain a clear and transparent precursor solution, and then the solution was transferred to a polytetrafluoroethylene reactor and kept at 50℃ for 30min, then heated to 100℃ for another 30min, and finally heated to 150℃ for 18h. After the reaction timer was terminated, the crude catalyst was obtained by centrifugation at 10000rpm for 5min after natural cooling, and then washed at least three times with 50mL DMF and 50mL ethanol respectively to completely remove the residual raw materials and impurities. Finally, the washed solid was placed in a vacuum oven at 100℃ and dried for 24h to obtain a yellow powder catalyst, marked as MIL-53(FeMg)-18H.
[0051] Example 2
[0052] This example is basically the same as Example 1, except that 4 mmol MgCl2·6H2O is replaced by 4 mmol Al(NO3)3·9H2O and is labeled as MIL-53(FeAl)-18H.
[0053] Example 3
[0054] This embodiment is basically the same as embodiment 1, except that 4 mmol MgCl2·6H2O is replaced by 4 mmol MnSO4·H2O and is labeled as MIL-53(FeMn)-18H.
[0055] Comparative Example 1
[0056] This comparative example is basically the same as Example 1, except that the metal salts of 16 mmol FeCl3·6H2O and 4 mmol MgCl2·6H2O are replaced by 20 mmol FeCl3·6H2O, and are labeled as MIL-53(Fe)-18H.
[0057]
Performance test
[0058] 1. Structural characterization
[0059] ①Crystal structure
[0060] In order to explore the structural evolution caused by different metal doping, the catalysts obtained in Examples 1 to 3 and Comparative Example 1 were subjected to PXRD test, and the results are as follows: Figure 1 shown.
[0061] observe Figure 1It can be seen that the characteristic peaks representing MIL-53(Fe) crystals in the range of 2θ from 5° to 25° all appear in the PXRD spectrum of the prepared catalyst material. Compared with MIL-53(Fe)-18H, the characteristic peak position and intensity of metal-doped MIL-53(Fe)-18H crystals change slightly, indicating that heterogeneous metal doping has a certain effect on the crystal structure. Careful observation shows that the doping of magnesium and aluminum heterogeneous metals causes the characteristic peak at 9.4° to weaken and shift to 9.1°, indicating that the (220) and (200) crystal planes have changed, indicating that the microscopic morphology of the two is very likely to change significantly.
[0062] ②Molecular structure
[0063] Furthermore, the molecular structures of the catalysts obtained in Examples 1 to 3 and Comparative Example 1 were characterized by FT-IR spectroscopy. Figure 2 shown.
[0064] observe Figure 2 It can be seen that: located at 700cm -1 To 1700cm -1 The characteristic absorption peaks of the organic linker, the CH bond and C=O bond in the H2BDC molecule, all appeared in the prepared catalyst material. -1 The characteristic absorption peaks at left and right wavenumbers correspond to the OH stretching vibration peaks of water molecules adsorbed on the catalyst surface or bound to the metal sites. In addition, the characteristic absorption peak attributed to the stretching vibration of the Fe-O bond is located at 552 cm -1 Compared with MIL-53(Fe)-18H, the doping of magnesium and manganese causes the stretching vibration peaks of Fe-O bonds to red shift significantly, which are located at 539 cm -1 and 550cm -1 wavenumber, while aluminum doping causes the peak to be significantly blue-shifted to 590 cm -1 wavenumber, this is due to the introduction of heterogeneous metal atoms to form a new Fe-OM (M is Mg, Al or Mn) node structure, indicating the successful preparation of MIL-53(FeMg)-18H, MIL-53(FeAl)-18H and MIL-53(FeMn)-18H catalyst materials.
[0065] ③ Appearance
[0066] In order to further verify the results of PXRD, the catalysts obtained in Examples 1 to 3 and Comparative Example 1 were subjected to SEM test, and the results are as follows: Figure 3 shown.
[0067] observe Figure 3It can be seen that the doping of heterogeneous metals causes a significant change in the crystal morphology of MIL-53(Fe)-18H. The MIL-53(Fe)-18H crystals doped with three heterogeneous metal atoms, magnesium, aluminum, and manganese, have completely different microscopic morphologies. MIL-53(FeMg)-18H presents a regular octahedral structure, and the crystal size is about 200nm, which is much smaller than the MIL-53(Fe)-18H crystal, indicating that magnesium doping accelerates the crystallization nucleation rate. The overall morphology of MIL-53(FeMn)-18H still presents a bipyramidal structure, but a large number of cracks cause the crystal surface to be uneven and fragments to peel off, and some crystals collapse into irregular fragments. Aluminum doping is completely different from magnesium and manganese doping. It no longer retains the original morphology of MIL-53(Fe), but presents an unexpected sea urchin shape, with slender needle-like structures evenly distributed on the surface, and the crystal size is 3-4μm.
[0068] ④Aperture
[0069] The porous structures of the catalysts obtained in Examples 1 to 3 and Comparative Example 1 were evaluated using the BET technique under the following test conditions: degassing temperature of 100°C. Figure 4 And as shown in Table 1.
[0070] like Figure 4 As shown in a, the nitrogen adsorption / desorption curves of the four prepared catalytic materials all have typical type IV isotherms and H3 type hysteresis loops, indicating that they are all mesoporous materials. From the pore size distribution diagram ( Figure 4 b) It can be seen that the pore size range of magnesium and manganese doped MIL-53(Fe)-18H materials is mainly distributed in the range of 2.0-3.0nm, and the distribution of small pore structure is much more than that of MIL-53(FeAl)-18H and MIL-53(Fe)-18H materials (the pore size range is mainly distributed in the range of 2.0-10.0nm), indicating that magnesium and manganese doped MIL-53(Fe)-18H materials have larger pore volume and specific surface area.
[0071] At the same time, it can be seen from Table 1 that among the four prepared catalytic materials, MIL-53(FeMg)-18H does have the largest specific surface area (467.56 m 2 g -1 ) and pore volume (0.308cm 3 g -1 ), and the smallest average pore size (2.63nm). Compared with undoped MIL-53(Fe)-18H, the specific surface area and pore volume of the metal-doped MIL-53(Fe)-18H material prepared by heterogeneous metal doping are improved, and the average pore size is reduced. From the perspective of heterogeneous catalytic mechanism, the optimization of pore structure is conducive to enhancing mass transfer enrichment, increasing active site exposure, and may cause confinement effect, significantly improving the catalytic performance of the material.
[0072] Table 1 Pore structure information of undoped and metal-doped MIL-53(Fe)-18H
[0073]
[0074] ⑤Element composition and chemical state
[0075] In order to analyze the surface structural element composition and chemical state of undoped and metal-doped MIL-53(Fe)-18H catalysts, the prepared catalysts were characterized by XPS technology. The results are shown in Figure 2. Figure 5 shown.
[0076] Figure 5 a is the XPS full spectrum of metal-doped MIL-53(Fe)-18H, showing that new peaks of Mg, Al and Mn elements appear in MIL-53(FeMg)-18H, MIL-53(FeAl)-18H and MIL-53(FeMn)-18H catalysts, respectively, confirming the successful preparation of metal-doped MIL-53(Fe)-18H catalysts.
[0077] Depend on Figure 5 b It can be seen that the Mg1s characteristic peak of MIL-53(FeMg)-18H is located near the binding energy of 1304 eV; the Al 2p characteristic peak of MIL-53(FeAl)-18H is located near the binding energy of 74 eV; the Mn 2p characteristic peak of MIL-53(FeMn)-18H is located near the binding energy of 74 eV. 3 / 2 and Mn 2p 1 / 2 The characteristic peaks are located near the binding energy of 641eV and 654eV respectively. In addition, from the high-resolution O1s XPS spectrum ( Figure 5 c) shows that due to the different types of heterogeneous metal atoms doped, O ads and O latt There are significant differences in the characteristic absorption peak area ratios of the undoped and magnesium, aluminum and manganese doped MIL-53(Fe)-18H, which are 5.56, 25.0, 4.35 and 3.85, respectively, indicating that magnesium doping leads to an increase in the oxygen vacancy content in the MIL-53(Fe)-18H catalyst structure, while aluminum and manganese doping leads to a decrease in the oxygen vacancy content in the MIL-53(Fe)-18H catalyst structure.
[0078] Figure 5 d is the Fe 2p XPS spectra of undoped and metal-doped MIL-53(Fe)-18H. It can be found that magnesium, aluminum, and manganese doping all lead to the Fe 2p of Fe(III). 1 / 2 and Fe 2p 3 / 2The characteristic peak binding energy shifts to a lower level, which is due to the weakening of the anchoring effect of Fe(III) on the outermost electrons, indicating that the Fe(III) site in Mg-, Al-, and Mn-doped MIL-53(Fe)-18H gains electrons, and its electron density increases compared with MIL-53(Fe)-18H.
[0079] ⑥Lewis acid site density
[0080] The present application uses Py-FTIR technology to measure the types and densities of acid sites on the catalyst surfaces obtained in Examples 1 to 3 and Comparative Example 1. The results are as follows: Figure 6 shown.
[0081] observe Figure 6 It can be seen that the four prepared catalytic materials all show the typical Py-FTIR absorption characteristic peak of MIL-53(Fe). According to different degassing temperatures (50℃, 150℃), the Py-FTIR spectrum is roughly located at 1070cm -1 The Lewis acid site composition and density on the surface of metal-doped MIL-53(Fe)-18H catalyst were calculated by using the characteristic peak area of wave number. The results are shown in Table 2.
[0082] From Table 2, it can be found that magnesium doping enhances the total acid density of MIL-53(Fe)-18H from 2.08 mmol g -1 Increased to 2.83 mmol g -1 , while Al and Mn doping weakened the total acid density of MIL-53(Fe)-18H, decreasing to 1.66 mmol g -1 and 1.10mmol g -1 Based on the calculation results of Lewis acid sites on the surface, it is speculated that MIL-53(FeMg)-18H may selectively produce ·OH efficiency when ozone is enhanced, while MIL-53(FeAl)-18H and MIL-53(FeMn)-18H may selectively produce 1 O2 efficiency, and the latter is stronger than the former.
[0083] Table 2 Surface Lewis acid site density of undoped and metal-doped MIL-53(Fe)-18H
[0084]
[0085] 2. ROS analysis of metal-doped MIL-53(Fe)-18H catalytic ozone system
[0086] The experimental conditions and procedures of this part are as follows:
[0087] ①ROS determination
[0088] EPR technology, free radical quenching experiment and free radical probe method were used to analyze the ROS generated by ozone decomposition during catalytic ozone decomposition. In the EPR technology, DMPO was used as ·OH and O2 ·- Signal capture agent, in which water is used as solvent for the capture of OH, O2 ·- Methanol was used as the solvent for the capture; TEMP was used as 1 The O2 signal capture agent, the solvent is water. The EPR spectrum of ROS generated by ozone decomposition and transformation was tested using the A300 electron spin resonance spectrometer of Bruker Company, USA. In the free radical quenching experiment, TBA and methanol were used as ·OH quenchers, and carbon tetrachloride and p-BQ were used as O2 ·- Quenchers, FFA and L-his as 1 O2 quencher, comparative quencher (2 g L -1 )’s inhibition degree on the catalytic degradation system is used to identify the contribution of ROS to the degradation of organic pollutants.
[0089] In the free radical probe method, coumarin (10 mM) was used as the ·OH probe to measure the cumulative concentration of ·OH in the system. 1 O2 probe, measuring system 1 O2 steady-state concentration, MDE and ozone, ·OH, 1 O2, O2 ·- The second-order reaction rate constants are k 1O2,MDE =1.5×10 8 M -1 s -1 , k ·OH,MDE =6×10 9 M -1 s -1 , k O3,MDE <1M -1 s -1 , k O2·-,MDE =0M -1 s -1 It can be seen that in the catalytic ozone system, MDE is mainly 1 O2 and ·OH oxidative degradation, so 20 mg L -1 The solvent composition was replaced by 50% water and 50% methanol to eliminate the reaction between OH and MDE, so that the concentration of MDE changed from 1 O2 dominated, and other reaction conditions were consistent with the catalytic ozone oxidation degradation experiment. 1 The steady-state concentration of O2 is determined by MDE and the relationship between ozone, OH, 1 O2, O2 ·- The second-order reaction rate constant is calculated by the following formula: 1Take O2 as an example:
[0090] MDE+ 1 O2→Substrate (1)
[0091]
[0092] ②DFT calculation parameters and models
[0093] Vienna Abinitio Simulation Package (VASP) was used for DFT calculations. The generalized gradient approximation proposed by Perdew-Burke-Ernzerhof (PBE) was used to describe the exchange-correlation energy. The plane wave cutoff energy was set to 480 eV. In the iterative solution of the Kohn-Sham equation, the energy convergence criterion was set to 10 -5 eV. All structures in the model are relaxed until the residual forces on the atoms drop to less than To avoid interlayer interaction, the layers are kept The vertical vacuum distance. The adsorption energy Eads is expressed as:
[0094] ΔE ads =E A+B -E A -E B (5)
[0095] Where E A+B is the total energy of the adsorption of molecule B by model A, E A is the energy of model A, E B is the energy of molecule B.
[0096] (1) OH and 1 EPR signal of O2
[0097] In order to verify the speculation about ROS modulation in "1. Structural Characterization - ⑥Lewis Acid Site Density", this section uses EPR technology to analyze the ·OH and 1 The production of O2, the results are as follows Figure 7 shown.
[0098] like Figure 7As shown in Figure a, when DMPO is used as an efficient ·OH scavenger, obvious quadruple characteristic peaks belonging to DMPO-·OH adducts are detected in the EPR spectra of the ozone systems catalyzed by the four catalysts, with a signal intensity ratio of 1:2:2:1. However, there are significant differences in the intensity of the ·OH signal peaks, and the order of intensity is magnesium-doped > undoped > aluminum-doped > manganese-doped, indicating that the efficiency of MIL-53(Fe)-18H prepared by different heterogeneous metal doping in catalyzing ozone to produce ·OH is different.
[0099] In addition, from Figure 7 b It can be found that when TEMP is 1 In the case of O2 efficient capture agent, each system showed typical TEMP- 1 The triple characteristic peaks of O2 adducts have a signal intensity ratio of 1:1:1, but 1 The peak intensity of O2 signal also showed significant differences, and the order of intensity was just opposite to that of ·OH signal peak intensity, which was Mn-doped > Al-doped > Undoped > Mg-doped. It can be seen that the occurrence of ·OH and ·OH in the ozone system catalyzed by the four catalysts was significantly different. 1 The modulation between O2 follows the modulation rule that one decreases while the other increases, indicating that MIL-53(Fe)-18H prepared by doping with different heterogeneous metals can catalyze the selective conversion of ozone, realize the modulation of ROS types, and break through the technical difficulties that complex wastewater quality places high demands on ROS generation and utilization. At the same time, it confirms the speculation in "1. Structural Characterization-⑥Lewis Acid Site Density" that magnesium doping enhances the efficiency of MIL-53(Fe)-18H catalyzing ozone selective production of ·OH, while aluminum doping and manganese doping both enhance the selective production of ozone by MIL-53(Fe)-18H. 1 O2 efficiency.
[0100] (2) OH and 1 Relationship between the EPR signal intensity of O2 and the surface Lewis acid site density
[0101] We obtain (1) ·OH and 1 After further investigation of the EPR signal of O2, OH and 1 The relationship between the EPR signal intensity of O2 and the surface Lewis acid site density is shown in the following figure: Figure 8 shown.
[0102] like Figure 8 As shown in the figure, the total acid density of Lewis acid sites on the catalyst surface is taken as the horizontal axis, ·OH and 1 The EPR signal intensity of O2 was used as the ordinate to draw a scatter plot and perform linear fitting. The results showed that the total acid density of Lewis acid sites on the catalyst surface showed an excellent positive linear correlation with the EPR signal intensity of ·OH. 2is 0.87; 1 The EPR signal intensity of O2 showed a good negative correlation linear relationship, Adj.R 2 The value of surface Lewis acid sites as key structures in regulating the selective conversion of ozone is further confirmed, indicating that the selective conversion of ozone can be mediated by constructing different surface Lewis acid site total acid densities by changing the type of heterogeneous metal doping, which provides a new idea for the development and design of ozone catalytic materials with high matching surface Lewis acid site density.
[0103] (3) Surface Lewis acid sites mediate the mechanism of ozone selective conversion
[0104] ①Electron distribution of metal active centers in metal-doped MIL-53(Fe)-18H
[0105] In order to explore the key factors and action rules of heterogeneous metal atomic properties affecting the Lewis acid sites on the surface of MIL-53(Fe)-18H, this application further uses DFT calculation methodology to explore the changes in the electronic distribution of MIL-53(Fe)-18H metal active sites after magnesium, aluminum, and manganese doping. The results are as follows Fig. 9 shown.
[0106] Fig. 9 The optimized models of the crystal plane structure of the undoped and metal-doped MIL-53(Fe)-18H catalytic material (100) are shown. The changes in the electron distribution of metal atoms and nearby oxygen atoms can be observed intuitively by calculating the Barde charge (number of valence electrons) of the surface atoms of the model structure. Fig. 9 It can be seen that the number of valence electrons of Fe atoms on the surface of undoped MIL-53(Fe)-18H is 6.396, and the number of valence electrons of Fe atoms near the doped area after magnesium, aluminum, and manganese doping is 6.411, 6.401, and 6.429, respectively, indicating that the introduction of three heterogeneous metal atoms, Mg, Al, and Mn, leads to an increase in the number of valence electrons of adjacent Fe atoms, that is, an increase in electron density, which is consistent with the Fe2p XPS characterization results. This may be due to the fact that the oxidizability of Fe(III) is higher than that of Mn(II), and much stronger than Al(III) and Mg(II). Therefore, Fe(III) has a strong electron-withdrawing ability and is easy to obtain electrons, which leads to an increase in its own electron density. The electron density of the Fe active center is closely related to its Lewis acid characteristics. Generally, an increase in electron density indicates that its ability to accept lone pairs of ligands is weakened, that is, the Lewis acid site density is reduced.
[0107] However, from the test results of the total acid density of Lewis acid sites on the surface of metal-doped MIL-53(Fe)-18H in "1. Structural Characterization - ⑥ Lewis Acid Site Density", the total acid density of aluminum- and manganese-doped MIL-53(Fe)-18H is indeed reduced compared to undoped MIL-53(Fe)-18H, while the total acid density of magnesium-doped MIL-53(Fe)-18H is increased. According to coordination theory, Mg(II) is a main group metal element in the third period, and its electronic configuration is 1s 2 2s 2 2p 6 , there is no d orbital, so the coordination ability and coordination stability of Mg(II) are weaker than those with 1s 2 2s 2 2p 6 3s 2 3p 6 3d 5 Fe(III) makes it difficult to form Mg-O coordination in the Fe-O-Mg structure or the σ covalent bond is easily broken, resulting in unsaturated metal coordination. All these factors lead to an increase in the total acid density of Lewis acid sites on the surface of MIL-53(FeMg)-18H.
[0108] Furthermore, the differential charge diagrams of undoped and Mg, Al, and Mn-doped catalysts were simulated. Fig.10 It can be seen that Fe atoms show different degrees of electron loss due to the differences in the types of heterogeneous metal doping. Magnesium, aluminum, and manganese doping all lead to a decrease in the degree of electron loss at the Fe site, indicating that the Fe site gains electrons and the electron density increases, which is consistent with the above-mentioned Bader charge calculation results.
[0109] Therefore, the above results indicate that the oxidizability and electronic structure of the doped heterogeneous metal atoms under multi-stage solvothermal assistance are key factors in regulating the Lewis acid sites on the surface of MIL-53(Fe)-18H. According to the coordination theory and metal activity, it can be inferred that among common metals, and under the premise of the same saturated coordination number, the change in the total acid density of Lewis acid sites on the surface of general metal-doped MIL-53(Fe)-18H is directly reflected by the oxidizability of the doped metal atoms, that is, if the oxidizability is lower than Fe(III), the total acid density of Lewis acid sites on the surface decreases, and if the oxidizability is higher than Fe(III), the total acid density of Lewis acid sites on the surface increases. At the same time, the electronic structure of the doped metal atoms should also be considered comprehensively. For example, in the case of Mg(II)-doped MIL-53(Fe)-18H, although the oxidizability of Mg(II) is lower than that of Fe(III), the difference in the electronic structure characteristics between the two leads to the coordination ability and coordination stability of Mg(II) being weaker than that of Fe(III). Unsaturated metal coordination is easily generated at the doping site, and the total acid density of Lewis acid sites on the surface of MIL-53(Fe)-18H is increased instead.
[0110] According to the valence bond theory in the coordination chemical bond theory, the empty d orbital of the Fe(III) center hybridizes with the s and p orbitals to form six hybrid orbitals, which accept the lone pair of electrons provided by the ligand O atom to form a σ coordination covalent bond. Therefore, the bridging O atom in the Fe-O-Fe node structure simultaneously provides a pair of lone electrons to the empty orbitals of the Fe atoms at both ends to form a stable coordination bond. According to the principle of electrical neutrality, since the electronegativity of the O atom is relatively large (3.44), the bonding electron pair is not shared by the bonding atoms, but is biased towards the ligand O atom. Fig. 9 It can be found that the number of valence electrons of the bridging O atoms in the Fe-O-Fe node structure changes significantly due to the doping of heterogeneous metal atoms. Magnesium and aluminum doping leads to a significant increase in the number of valence electrons of the adjacent bridging O atoms at the doped position, while manganese doping is just the opposite, which reduces the number of valence electrons of the adjacent bridging O atoms. This may be because the doping of heterogeneous metals constitutes an Fe-OM asymmetric structure, reconstructs the metal-oxygen coordination environment, and breaks the balance of electronic distribution at the metal node. Due to the difference in the ability of Fe and M atoms to attract electrons, the willingness of the ligand O atom to provide lone pairs of electrons to both ends is tilted, and the bias of the bonding electron pairs is also disturbed, so its Bader charge changes significantly. In the Fe-O-Mn structure, Fe(III) has a stronger electron-withdrawing ability than Mn(II). Therefore, the balance of lone pairs of electrons in O atoms tilts toward Fe atoms, and the bias of shared electron pairs of Fe-O σ bonds toward O atoms is slightly weakened, which, on the one hand, increases the electron density of Fe atoms and makes Fe-O coordination bonding more stable; on the other hand, Mn(II) is also very willing to coordinate with O and is unwilling to give up the lone pairs from O, which leads to a decrease in the electron density of O. In the Fe-O-Mg and Fe-O-Al structures, the electron-withdrawing ability of Mg(II) and Al(III) is much lower than that of Fe(III), which also tilts the balance of lone pairs of electrons in O atoms toward Fe atoms. However, since the attraction of lone pairs of electrons of ligands is greatly weakened by the doping of Mg(II) and Al(III), the shared electron pairs of σ bonds of Mg-O and Al-O are more biased toward O atoms, which leads to an increase in the electron density of bridging O atoms.
[0111] ② Water molecules and ozone molecules compete for adsorption
[0112] Analysis of the above results revealed that the total acid density of Lewis acid sites on the surface of MIL-53(Fe)-18H and the electron density of Fe sites changed due to heterogeneous metal doping.
[0113] Then the adsorption capacity of metal-doped MIL-53(Fe)-18H catalytic material for Lewis base molecules (water and ozone molecules) may also be significantly different compared with undoped MIL-53(Fe)-18H.
[0114] To this end, DFT methodology was used to calculate the adsorption of water and ozone molecules on the optimized crystal surface structure of the prepared catalytic material (100). Since Fe is the main metal active site and its coordination environment and electronic structure are affected by heterogeneous metal doping, the Fe atoms in the doped area are preferentially selected as the adsorption sites of water and ozone molecules in this application, and the adsorption energy (E ads ), ozone terminal oxygen and intermediate oxygen OO bond length (l O-O ), the charge transfer amount between the catalyst surface and ozone (Q e ), the Bader charge of the adsorbed water molecule, the calculation results are shown in Figures 11 to 13 middle.
[0115] Depend on Fig.11 and Fig.13 It can be seen that the terminal oxygen of ozone with high electron density and the intermediate oxygen of water are adsorbed on the Fe site of the doped region through electrostatic attraction and Lewis acid-base interaction. Due to the differences in the coordination environment and electronic structure of the Fe site, the adsorption energies of the four catalysts for water and ozone molecules vary. Fig.12 It can be found that the adsorption energies of aluminum- and manganese-doped catalysts for ozone are greater than those for water, indicating that both are easier to adsorb ozone molecules in a water environment (dominated by ozone adsorption), or when water molecules occupy the active sites first, water molecules are outcompeted by ozone molecules for adsorption and are easier to desorb from the active sites; while the adsorption energies of magnesium-doped and undoped catalysts for ozone are lower than those for water, indicating that they are more inclined to adsorb water molecules (dominated by water adsorption), or when water molecules occupy the active sites first, water molecules are outcompeted by ozone molecules for adsorption and are more difficult to desorb from the active sites.
[0116] Compared with free ozone molecules, the activation ability of the catalyst active sites makes the OO bond length of the terminal oxygen and the intermediate oxygen of ozone from Extend to ( Fig.11 ), indicating that the interaction between ozone and the active sites leads to the formation of ozone by OO bond cleavage and 1 O2 and *O ads In order to explore the interaction between ozone and the active sites of the four catalysts, the differential charge diagram of the adsorption model was drawn, and the amount of electron transfer between ozone and the catalyst was quantitatively calculated using the Bader charge. Fig.11 As shown in the figure, it can be found that ozone in the four models obtains electrons from the catalyst surface, among which ozone obtains the most electrons from the manganese-doped model, indicating that the interaction between the two is very strong and catalytic activation reaction is easy to occur. 1 The formation path of O2, the calculation results predict in advance that ozone-dominated adsorption and 1 The important relationship between O2 production.
[0117] From the formation path of ·OH during ozone activation, the Fe site of the Fe-MOFs catalyst adsorbs water molecules to form M-OH (M is Mg, Al or Mn), which combines with ozone molecules through electrostatic attraction and hydrogen bonding, and then transforms into ·OH. The key to the electrostatic attraction and hydrogen bonding lies in the charge density of hydrogen atoms at both ends of the adsorbed water molecules. Low charge density indicates that hydrogen bonds are easily formed, and the electrostatic attraction between hydrogen and the terminal oxygen with high electron density in the ozone molecule structure is strong, and vice versa.
[0118] Therefore, the experiment used DFT to continue calculating the Bader charges of the hydrogen atoms at both ends of the water molecule in the four catalyst Fe site adsorption water molecule models. The results are shown in Fig.13 In. Fig.13 As shown in the figure, the total Bader charge of the hydrogen atoms at both ends of the adsorbed water molecules is used as an index to represent the ability of the four adsorption models to continue to combine with the terminal oxygen atoms of ozone through electrostatic attraction and hydrogen bonding. The larger the value, the weaker the ability. As a result, the order of the index values of the four models is: MIL-53(FeMn)-18H(0.682)>MIL-53(FeAl)-18H(0.667)>MIL-53(Fe)-18H(0.650)>MIL-53(FeMg)-18H(0.645), indicating that the order of the ability to continue to bind to ozone is MIL-53(FeMg)-18H>MIL-53(Fe)-18H>MIL-53(FeAl)-18H>MIL-53(FeMn)-18H. This is consistent with the order of catalytic ozone → ·OH selectivity, indicating the important role of adsorbed water molecules in the generation of ·OH. It also verifies the traditional catalytic theory based on metal-based adsorbed water molecules forming M-OH (M is Mg, Al or Mn) and activating ozone conversion to form ·OH as the main active site.
[0119] In order to further explore the essential relationship between the total acid density of Lewis acid sites on the surface of MIL-53(Fe)-18H and the adsorption competition between water and ozone molecules, the definition of “AC HQ =E ads (O3)-E ads (H2O)" is used as a key indicator of the adsorption competition between water and ozone molecules, indicating the dominant role of water or ozone in the adsorption of active sites. The linear relationship between the total acid density of Lewis acid sites on the surface and the key indicators is explored. The results are as follows Fig.14 shown.
[0120] observe Fig.14 It can be seen that, except for magnesium doping, the total acid density of Lewis acid sites on the surface shows a strong linear relationship with key indicators, Adj R 2>0.99, indicating that the adsorption competition between water and ozone molecules is the potential mechanism of Lewis acid sites mediating the selective conversion of ozone. From the calculation results of the significant increase in the electron density of O atoms in the magnesium-doped Fe-O-Mg structure ( Fig. 9 c), when water molecules are adsorbed on the Fe site in the doped region, the hydrogen bonding effect between H atoms and O atoms in the Fe-O-Mg structure cannot be ignored. However, in order to simplify the model, the hydrogen bonding effect was ignored in the calculation process, resulting in a low adsorption energy of water by magnesium doping, which caused the magnesium doping to deviate from the linear fitting curve, further illustrating the important role of water molecule adsorption and desorption in the ozone activation process.
[0121] Therefore, according to the DFT calculation results of the adsorption energy, Bader charge, and differential charge density of water and ozone molecules, it is basically determined that the adsorption competition between water and ozone molecules is an important factor in the dominant Lewis acid site-mediated ozone selective conversion. Fe-MOFs materials with low Lewis acid site total acid density dominated by ozone molecules tend to catalyze the selective production of ozone. 1 O2, while Fe-MOFs materials with high Lewis acid site total acid density dominated by water molecules tend to catalyze ozone to selectively produce ·OH.
[0122] ③ Gibbs free energy of ozone decomposition pathway
[0123] Based on the intrinsic relationship between the adsorption competition between water and ozone molecules and the total acid density of Lewis acid sites on the surface, and the modulation of the total acid density of Lewis acid sites on the surface, OH and 1 The regulation of O2 generation is combined with the traditional theory of ozone decomposition and transformation to form ·OH and 1 In order to find the key evidence of water molecule adsorption and desorption involved in ozone activation, and to reveal the Lewis acid site-mediated selective ozone conversion mechanism dominated by water and ozone molecule adsorption competition at the molecular level, this application adopts DFT methodology to refer to the ozone decomposition to produce ·OH and 1 The O2 pathways were calculated for the Fe sites in the undoped, Al-doped, and Mn-doped catalysts. 1 The Gibbs free energy of the O2 process is as follows Fig.15 shown.
[0124] First, the thermodynamic process of ozone activation mechanism is discussed. Fig.15 It can be seen that ozone approaches the active center of the catalyst metal through electrostatic attraction and is adsorbed on the surface active site by Lewis acid-base interaction. The interaction between the active site and ozone drives electron migration, thereby activating ozone, causing the terminal oxygen and the intermediate oxygen OO bond to stretch and break, decomposing and transforming to form 1 O2 and *O ads . 1The formation of O2 is spontaneous and exothermic in all three catalyst models, that is, the energy level difference between the final state and the initial state is less than zero, but the process energy barrier of generating the transition state TS (Fe--O3) in the path increases, indicating that the thermodynamic reaction is an endothermic, uphill process, which is the rate-determining step (PDS) of the overall reaction. The Gibbs free energy change of this step is △G PDS >0. From Fig.15 bIt can be seen that 1 The generation path of O2 is different. The water molecules adsorbed on the active sites first do not desorb, and combine with the oxygen atoms at both ends of ozone through electrostatic attraction and hydrogen bonding to form an unstable six-membered ring, which then breaks to produce surface hydroxyl groups (*OH ads ) and ·HO3, ·HO3 further decomposes to form ·OH and O2. The formation of ·HO3 is also exothermic and spontaneous on the three catalyst models, but the process energy barrier for the generation of transition state TS (Fe-H2O--O3) in the path increases, which is the PDS of the overall reaction, △G PDS >0.
[0125] “② Competition between water molecules and ozone molecules for adsorption” confirms that the competition between water and ozone molecules for adsorption plays a key role in determining the selective conversion of ozone. The adsorbed water molecules change the ozone decomposition pathway by desorption or participation in the activation process, regulating the ·OH or 1 O2 is formed, therefore, OH and 1 The generation of O2 in different catalyst systems should consider the above two pathways comprehensively. 3) The energy barrier of TS (Fe-H2O--O3) determines the direction of the reaction thermodynamically. HQ =△G PDS (TS(Fe--O3))-△G PDS (TS(Fe-H2O--O3))" is a key indicator of the ozone selective conversion pathway, indicating that the catalytic ozone decomposition is formed. 1 The thermodynamic direction of the reaction of O2 or ·OH is as follows: the values of MIL-53(Fe)-18H, MIL-53(FeAl)-18H and MIL-53(FeMn)-18H are 0.37 eV, 0.14 eV and -0.15 eV, respectively, indicating that the three activate ozone → 1 The order of ability to react with O2 is: MIL-53(FeMn)-18H>MIL-53(FeAl)-18H>MIL-53(Fe)-18H, while the order of ability to activate ozone→·OH reaction is exactly the opposite.
[0126] In order to further correlate this index with the key structure of Fe-MOFs and explore the mechanism of surface Lewis acid sites mediating the selective conversion of ozone, the linear relationship between the two was experimentally studied. Fig.16 As shown, the Lewis acid sites on the surface are HQ There is a very good linear relationship between the indicators, Adj R 2 >0.99, indicating that the Lewis acid sites on the surface control the adsorption competition between water and ozone molecules, determine the thermodynamic direction of the ozone decomposition reaction, mediate the selective conversion of ozone, and ultimately achieve ·OH and 1 Controllable modulation of O2.
Claims
1. A method for preparing a heterogeneous metal-doped iron-based MOF catalyst, characterized in that: The heterogeneous metal-doped iron-based MOF catalyst is obtained by solvent thermal reaction of an N,N-dimethylformamide solution containing a heterogeneous metal source, an iron salt, and terephthalic acid, followed by drying; the heterogeneous metal source is selected from any one of aluminum salt, manganese salt, and magnesium salt; the solvent thermal reaction is: 20 to 30 minutes at 50°C, then 20 to 30 minutes at 100°C, and then 14 to 22 hours at 150°C.
2. The preparation method according to claim 1, characterized in that The iron salt is selected from any one of ferric nitrate, ferric chloride, ferric sulfate and ammonium ferric citrate.
3. The preparation method according to claim 1, characterized in that: The aluminum salt is selected from any one of aluminum nitrate, aluminum sulfate and aluminum chloride.
4. The preparation method according to claim 1, characterized in that: The manganese salt is selected from any one of manganese nitrate, manganese sulfate and manganese chloride.
5. The preparation method according to claim 1, characterized in that: The magnesium salt is selected from any one of magnesium nitrate, magnesium sulfate and magnesium chloride.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The molar ratio of the heterogeneous metal to iron in the heterogeneous metal source and the iron salt is 1:
4.
7. The preparation method according to any one of claims 1 to 5, characterized in that: The ratio between the total molar amount of the heterogeneous metal and iron in the heterogeneous metal source and the iron salt and the molar amount of the terephthalic acid is 1:
1.
8. The preparation method according to claim 1, characterized in that: The drying temperature is 80 to 120° C., and the drying time is 12 to 36 hours.
9. A heterogeneous metal-doped iron-based MOF catalyst prepared by the preparation method according to any one of claims 1 to 8.