Manufacturing method of omega-shaped process cover plate
Through the Ω-shaped cover plate manufacturing method, the quality problem of Ω-shaped foam reinforcement rib molding in composite material components is solved, the quality improvement of the appearance surface and stress uniformity are achieved, and the product quality and production efficiency are improved.
Patent Information
- Application Number
- CN202410976374.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-20
AI Technical Summary
The existing technology cover plate cannot effectively solve the molding quality problems of Ω foam reinforcement ribs in composite components, resulting in problems such as pits, poor skin surface quality, and unqualified thickness after curing, affecting product quality and production efficiency. .
A Ω-shaped process cover plate manufacturing method is adopted, through the steps of tool preparation, material preparation, process cover plate laying, curing and forming, demolding and trimming, combined with laser projection assisted manual laying and automatic discharge machine CNC cutting, Ensure the surface quality and stress uniformity of the cover plate, avoid pores and layered defects, and allow multiple reuse.
The surface quality of the Ω foam reinforcement ribs has been improved, which avoids internal defects at the R angle, eliminates stress concentration, ensures the overall uniform pressure effect, and improves the stability of the process cover plate and the feasibility of multiple uses. sex.
Smart Images

Figure CN118927665A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material component manufacturing technology, and in particular to a method for manufacturing an Ω-shaped process cover plate. Background Art
[0002] Composite materials are widely used in modern aviation, aerospace and other fields due to their advantages such as light weight, high strength, good corrosion resistance, good fatigue resistance, shock absorption, good fracture safety and good high temperature resistance. Process cover is a common auxiliary forming tool in the manufacture of composite components. Its main function is to improve the pressure distribution in the R corner area.
[0003] The Ω-shaped foam reinforcement ribs support the ball skin, and their molding quality affects the product quality, and is also a control difficulty in the manufacture of composite ball frames. If a process cover is not used, the cured reinforcement ribs are prone to pits, poor surface quality of the skin, unqualified thickness, and other problems, which seriously affect product quality and reduce production efficiency. The existing process cover cannot meet the manufacturing requirements of this component. Therefore, the present invention specifically designs a new Ω-shaped process cover plate with the function of reducing concentrated stress. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for manufacturing an Ω-shaped process cover plate. The Ω-shaped process cover plate obtained by the manufacturing method of the present invention can ensure that the surface quality of the Ω-shaped foam reinforcement rib is good, and avoid internal defects such as pores and delamination caused by the mismatch of the profile at the R corner; at the same time, the problem of stress concentration is effectively eliminated, and each matching area is effectively compressed, and the overall uniform pressure effect is good. In addition, the process cover plate in the present invention can be reused many times and has good stability.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for manufacturing an Ω-shaped cover plate, which is suitable for forming foam reinforcement ribs of composite material components, comprises the following steps:
[0007] Step S1: tooling preparation: manufacturing and receiving tooling, cleaning tooling and applying release agent;
[0008] Step S2: Material preparation: Take the carbon fiber prepreg and warm it up, then use the automatic unloading machine to numerically control the unloading;
[0009] Step S3: Laying up the process cover: Receive the material package and check the integrity of the cut pieces in the material package according to the layup table; stick a sealing strip on the edge of the tooling, do not remove the backing, and the sealing strip cannot be attached to the release agent or label; when there is a hole on the edge of the tooling, the hole should be outside the bag making range when making bags;
[0010] Step S4: Process cover plate curing and molding: loading the cover plate into the autoclave and testing for leaks, and curing according to curing parameter requirements;
[0011] Step S5: Demolding the cover: remove the vacuum bag, breathable felt, and isolation film, and slowly pry the edge of the cover with a wedge to demold the cover. The cover or the tooling must not be damaged during demolding.
[0012] Step S6: trimming the cover: trim the shape along the cover step with a tolerance of ±2mm; trim the edges to make the edges transition smoothly; remove 5-10mm from the rounded edges of the cover as required; use compressed air to remove surface dust from the processed cover, and after completion, use a wiper dipped in acetone solvent to clean the inner and outer surfaces of the cover.
[0013] Furthermore, step S1 includes mold tooling manufacturing:
[0014] A stacking mold for manufacturing a ribbed cover is used. The digital mold shape surface of the foam core of the mold stacking surface is extracted and manufactured. A laser projection target point is set on the mold to realize the laser projection-assisted manual stacking operation. The shape cutting of the blank is completed based on the theoretical outer contour cutting line of the ribbed cover projected by the laser projector.
[0015] Furthermore, step S3 further includes the following steps:
[0016] Step S31: Lay the whole AIRPAD; control the AIRPAD to cover the net size line of the tooling, and cut the openings at both ends, and then butt joint after opening, and control the butt joint gap to be less than 1.5mm; after the paving is completed, seal the temporary vacuum bag, vacuum at least -0.08Mpa and compact for at least 15min;
[0017] Step S32: laying carbon fiber prepreg, cutting at both ends, butting after the opening, and controlling the butt gap to be less than 1.5mm; after the laying is completed, sealing a temporary vacuum bag, vacuuming to at least -0.08Mpa and compacting for at least 15min;
[0018] Step S33: laying out locally reinforced carbon fiber prepreg, and controlling the prepreg to cover the R corner; laying out two layers of prepreg in the concave area of the Ω-shaped process cover plate, and laying out one layer of prepreg in the edge areas at both ends; after the laying is completed, sealing a temporary vacuum bag, evacuating to at least -0.08Mpa and compacting for at least 15 minutes;
[0019] Step S34: laying carbon fiber prepreg, cutting at both ends, butting after the opening, and controlling the butt gap to be less than 1.5mm; after the laying is completed, sealing a temporary vacuum bag, vacuuming to at least -0.08Mpa and compacting for at least 15min;
[0020] Step S35: Lay the whole AIRPAD, control the AIRPAD to cover the net size line of the tooling, and cut the openings at both ends, and butt joint after opening, and control the butt joint gap to be less than 1.5mm; after the paving is completed, seal the temporary vacuum bag, evacuate to at least -0.08Mpa and compact for at least 15 minutes.
[0021] Further, in step S4, the curing parameters are:
[0022] After the vacuum reaches -80KPa, pressurization begins. When the pressure reaches 140KPa, the vacuum is closed and vented to the atmosphere. After the pressure reaches 610KPa, the temperature is increased to 180±6℃ at a heating rate of 1.5℃ / min and kept warm for 90 minutes. Finally, the temperature is reduced to 50℃ at 2℃ / min and the pressure is released.
[0023] The Ω-shaped process cover plate manufacturing method of the present invention can ensure that the surface quality of the Ω-shaped foam reinforcement rib is good, and avoid internal defects such as pores and delamination caused by the mismatch of the profile at the R corner; at the same time, the problem of stress concentration is effectively eliminated, and each matching area is effectively compressed, and the overall uniform pressure effect is good. In addition, the process cover plate of the present invention can be reused many times and has good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of a lay-up mold of an Ω-shaped cover plate of the present invention;
[0025] Figure 2 This is a schematic diagram of the Ω-shaped cover plate structure of the present invention;
[0026] Figure 3 This is a schematic diagram of laying carbon fiber prepreg for local reinforcement of the Ω-shaped cover plate of the present invention;
[0027] Figure 4 It is a schematic diagram of the Ω-shaped cover plate trimming process of the present invention. DETAILED DESCRIPTION
[0028] In order to make the technical solution and advantages of the present invention clearer, the technical solution of the present invention will be further described in detail in detail with reference to the accompanying drawings. It can be understood that the specific embodiments described here are only partial embodiments of the present invention, which are only used to explain the present invention, not to limit the present invention. It should be noted that, for the convenience of description, only the parts / structures related to the present invention are shown in the accompanying drawings, and other related parts can refer to the general design. In the absence of conflict, the embodiments of the present invention and the technical features in the embodiments can be combined with each other to obtain new embodiments.
[0029] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In addition, unless otherwise defined, the technical terms or scientific terms used in the description of the present invention should be the common meanings understood by ordinary technicians in the field to which the present invention belongs.
[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0031] like Figure 1-4 As shown, a method for manufacturing an Ω-shaped process cover plate, which is suitable for forming foam reinforcement ribs of composite material components, comprises the following steps:
[0032] Step S1: tooling preparation: manufacturing and receiving tooling, cleaning tooling and applying release agent;
[0033] Step S2: Material preparation: Take the carbon fiber prepreg and warm it up, then use the automatic unloading machine to numerically control the unloading;
[0034] Step S3: Laying up the process cover: Receive the material package and check the integrity of the cut pieces in the material package according to the layup table; stick a sealing strip on the edge of the tooling, do not remove the backing, and the sealing strip cannot be attached to the release agent or label; when there is a hole on the edge of the tooling, the hole should be outside the bag making range when making bags;
[0035] Step S4: Process cover plate curing and molding: loading the cover plate into the autoclave and testing for leaks, and curing according to curing parameter requirements;
[0036] Step S5: Demolding the cover: remove the vacuum bag, breathable felt, and isolation film, and slowly pry the edge of the cover with a wedge to demold the cover. The cover or the tooling must not be damaged during demolding.
[0037] Step S6: trimming the cover plate: trim the shape along the cover plate step with a tolerance of ±2mm; trim the edges to make the edges transition smoothly; remove 5-10mm (such as Figure 4 The surface dust of the processed cover plate shall be removed by compressed air, and after completion, the inner and outer surfaces of the cover plate shall be cleaned with a wiper dipped in acetone solvent.
[0038] Among them, step S1 includes mold tooling manufacturing:
[0039] A stacking mold for manufacturing a ribbed cover is used. The digital mold shape surface of the foam core of the mold stacking surface is extracted and manufactured. A laser projection target point is set on the mold to realize the laser projection-assisted manual stacking operation. The shape cutting of the blank is completed based on the theoretical outer contour cutting line of the ribbed cover projected by the laser projector.
[0040] Wherein, step S3 also includes the following steps:
[0041] Step S31: Lay the whole AIRPAD; control the AIRPAD to cover the net size line of the tooling, and cut the openings at both ends, and then butt joint after opening, and control the butt joint gap to be less than 1.5mm; after the paving is completed, seal the temporary vacuum bag, vacuum at least -0.08Mpa and compact for at least 15min;
[0042] Step S32: laying carbon fiber prepreg, cutting at both ends, butting after the opening, and controlling the butt gap to be less than 1.5mm; after the laying is completed, sealing a temporary vacuum bag, vacuuming to at least -0.08Mpa and compacting for at least 15min;
[0043] Step S33: Lay the locally reinforced carbon fiber prepreg, and control the prepreg to cover the R angle; the concave area of the Ω-shaped process cover plate ( Figure 3 Two layers of prepreg are laid on the black area in the figure, and one layer of prepreg is laid on the edge areas at both ends (grid areas); after laying, a temporary vacuum bag is sealed, vacuumed to at least -0.08Mpa and compacted for at least 15 minutes;
[0044] Step S34: laying carbon fiber prepreg, cutting at both ends, butting after the opening, and controlling the butt gap to be less than 1.5mm; after the laying is completed, sealing a temporary vacuum bag, vacuuming to at least -0.08Mpa and compacting for at least 15min;
[0045] Step S35: Lay the whole AIRPAD, control the AIRPAD to cover the net size line of the tooling, and cut the openings at both ends, and butt joint after opening, and control the butt joint gap to be less than 1.5mm; after the paving is completed, seal the temporary vacuum bag, evacuate to at least -0.08Mpa and compact for at least 15 minutes.
[0046] Among them, in step S4, the curing parameters are:
[0047] After the vacuum reaches -80KPa, pressurization begins. When the pressure reaches 140KPa, the vacuum is closed and vented to the atmosphere. After the pressure reaches 610KPa, the temperature is increased to 180±6℃ at a heating rate of 1.5℃ / min and kept warm for 90 minutes. Finally, the temperature is reduced to 50℃ at 2℃ / min and the pressure is released.
[0048] The Ω-shaped process cover plate manufacturing method of the present invention can ensure that the surface quality of the Ω-shaped foam reinforcement rib is good, and avoid internal defects such as pores and delamination caused by the mismatch of the profile at the R corner; at the same time, the problem of stress concentration is effectively eliminated, and each matching area is effectively compressed, and the overall uniform pressure effect is good. In addition, the process cover plate of the present invention can be reused many times and has good stability.
[0049] The above-mentioned implementation modes are for explanation of the present invention rather than limitation of the present invention. It can be understood that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principle and spirit of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for manufacturing an Ω-shaped cover plate, which is suitable for forming foam reinforcement ribs of composite material components, comprising the following steps: Step S1: tooling preparation: manufacturing and receiving tooling, cleaning tooling and applying release agent; Step S2: Material preparation: Take the carbon fiber prepreg and warm it up, then use the automatic unloading machine to numerically control the unloading; Step S3: Process cover plate stacking: receive the material package and check the integrity of the cut pieces in the material package according to the stacking table; Stick a piece of sealing tape on the edge of the tooling, do not remove the backing, and the sealing tape cannot be attached to the release agent or label; when there are holes on the edge of the tooling, the holes should be outside the bag making range when making bags; Step S4: Process cover plate curing and molding: loading the cover plate into the autoclave and testing for leaks, and curing according to curing parameter requirements; Step S5: Demolding the cover: remove the vacuum bag, breathable felt, and isolation film, and slowly pry the edge of the cover with a wedge to demold the cover. The cover or the tooling must not be damaged during demolding. Step S6: trimming the cover plate: trimming the shape along the cover plate step with a tolerance of ±2mm; And trim the edges to make the transition smooth; remove 5-10mm from the rounded edges of the cover as required; use compressed air to remove surface dust from the processed cover, and after completion, use a wiper dipped in acetone solvent to clean the inner and outer surfaces of the cover.
2. The method for manufacturing an Ω-shaped cover plate according to claim 1, characterized in that: in, Step S1 includes mold tooling manufacturing: A stacking mold for manufacturing a ribbed cover is used. The digital mold shape surface of the foam core of the mold stacking surface is extracted and manufactured. A laser projection target point is set on the mold to realize the laser projection-assisted manual stacking operation. The shape cutting of the blank is completed based on the theoretical outer contour cutting line of the ribbed cover projected by the laser projector.
3. The method for manufacturing an Ω-shaped cover plate according to claim 2, characterized in that: in, Step S3 further includes the following steps: Step S31: Lay the whole AIRPAD; control the AIRPAD to cover the net size line of the tooling, and cut the openings at both ends, and then butt joint after opening, and control the butt joint gap to be less than 1.5mm; after the paving is completed, seal the temporary vacuum bag, vacuum at least -0.08Mpa and compact for at least 15min; Step S32: laying carbon fiber prepreg, cutting at both ends, butting after the opening, and controlling the butt gap to be less than 1.5mm; after the laying is completed, sealing a temporary vacuum bag, vacuuming to at least -0.08Mpa and compacting for at least 15min; Step S33: laying out locally reinforced carbon fiber prepreg, and controlling the prepreg to cover the R corner; laying out two layers of prepreg in the concave area of the Ω-shaped process cover plate, and laying out one layer of prepreg in the edge areas at both ends; after the laying is completed, sealing a temporary vacuum bag, evacuating to at least -0.08Mpa and compacting for at least 15 minutes; Step S34: laying carbon fiber prepreg, cutting at both ends, butting after the opening, and controlling the butt gap to be less than 1.5mm; after the laying is completed, sealing a temporary vacuum bag, vacuuming to at least -0.08Mpa and compacting for at least 15min; Step S35: Lay the whole AIRPAD, control the AIRPAD to cover the net size line of the tooling, and cut the openings at both ends, and butt joint after opening, and control the butt joint gap to be less than 1.5mm; after the paving is completed, seal the temporary vacuum bag, evacuate to at least -0.08Mpa and compact for at least 15 minutes.
4. The method for manufacturing an Ω-shaped cover plate according to claim 3, characterized in that: in, In step S4, the curing parameters are: After the vacuum reaches -80KPa, pressurization begins. When the pressure reaches 140KPa, the vacuum is closed and vented to the atmosphere. After the pressure reaches 610KPa, the temperature is increased to 180±6℃ at a heating rate of 1.5℃ / min and kept warm for 90 minutes. Finally, the temperature is reduced to 50℃ at 2℃ / min and the pressure is released.
Citation Information
Patent Citations
Technology method for forming composite material omega-shaped curvature stringer
CN110271205A
Manufacturing method of combined type uniform-pressure cover plate applied to Omega stringer ribbed composite material wallboard
CN111267370A
Novel structure cover plate and preparation method and use method thereof
CN115892509A
Method of manufacturing a z-section component from composite material