Method for preparing lithium iron manganese phosphate material from zinc anode slime and lithium iron phosphate waste material
Through the comprehensive recycling method of zinc anode sludge and lithium iron phosphate waste, high-purity lithium manganese phosphate materials are prepared, which solves the waste of manganese, lead and silver resources and meets the market's demand for lithium manganese phosphate materials. It realizes efficient utilization of resources and environmental protection.
Patent Information
- Application Number
- CN202410944993.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-12
AI Technical Summary
The existing technology is difficult to effectively recover manganese, lead and silver resources in zinc anode mud, and the lithium iron phosphate positive electrode material of lithium ion battery waste is high in regeneration costs and poor electrochemical performance, which cannot meet the market demand for lithium manganese iron phosphate materials. .
The method of combining zinc anode sludge with lithium iron phosphate waste is used to prepare lithium manganese iron phosphate materials through ball milling, leaching, oxidation and roasting and high-temperature sintering. The slurry dezincification, separation and other agents are used for dilute sulfuric acid, starch and activated carbon. Remove impurities, achieve efficient recovery of manganese, lithium, Fe and P, and prepare high-purity lithium manganese iron phosphate positive electrode material.
The comprehensive recycling of zinc anode mud and lithium iron phosphate waste has been achieved, with a manganese recovery rate of 98%, and a Li, Fe and P recovery rate of more than 98.5%. The prepared lithium iron phosphate material has excellent physical and chemical properties and is suitable for large-scale Large-scale industrial production reduces resource waste and environmental pollution.
Smart Images

Figure CN118929606A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive waste recovery, and in particular to a method for preparing lithium iron manganese phosphate material by utilizing zinc anode mud and lithium iron phosphate waste. Background Art
[0002] Manganese ions play an important role in the production of zinc electrolysis. 2+ Oxidized to form solid MnO2 (also known as zinc anode mud) attached to the lead-silver anode plate to protect the anode and extend the service life of the anode plate. 2+ When the content of Mn in zinc electrolyte is too low, the life of anode plate is shortened and the quality of zinc precipitation is affected. 2 + If it continues to rise, the power consumption in the zinc electrolysis process will increase, and the viscosity of the electrolyte will increase. Therefore, the Mn content in the zinc electrolyte should be properly controlled. 2+ Under normal circumstances, 50-60 kg of anode mud can be produced for every ton of electrolytic zinc. Zinc anode mud generally contains valuable metals such as manganese, lead, zinc and silver, with contents of 30-40%, 10-15%, 2% and about 500g / ton respectively, which is of great recycling value.
[0003] Manganese in zinc anode mud mainly exists in the form of manganese dioxide, which has certain oxidizing properties. Therefore, most manufacturers directly return it to zinc leaching as an oxidant and to supplement the manganese ions in zinc sulfate. Since manganese dioxide in zinc anode mud is generally insoluble in acid and alkali, and lead and silver are eventually transferred to acid leaching residue, and the silver recovery rate of acid leaching residue using silver flotation process is less than 60%, therefore, returning zinc anode mud for use will result in a waste of manganese, lead and silver resources.
[0004] Some manufacturers directly process zinc anode mud through a lead metallurgical furnace to recover the lead and silver in the anode mud. Although this treatment method can recover lead and silver very well, the large amount of zinc anode mud and high manganese content will increase the cost of lead and silver recovery. In addition, the manganese, sulfuric acid and zinc in the anode mud cannot be effectively recycled, which also causes a serious waste of resources. At the same time, this process has a greater impact on the environment and a low metal recovery rate.
[0005] A few manufacturers pile up zinc anode mud, which leads to insufficient resource utilization, serious pollution to public health and the environment, and other serious problems. Some scientific and technological workers use physical separation to separate manganese from lead and silver in zinc anode mud, that is, flotation-gravity separation-magnetic separation or flotation-magnetic separation. However, due to the serious dispersion of silver in concentrate and tailings, it is impossible to achieve efficient recovery of lead, silver, zinc and manganese in zinc anode mud.
[0006] Lithium iron phosphate, a positive electrode material for lithium-ion batteries, has a theoretical specific capacity of 170 mAh g-1 , the actual specific capacity exceeds 140mAh g -1 (0.2C, 25℃), with the advantages of low price, good thermal stability, environmental protection, high safety and excellent cycle performance. In 2022, the global total shipment of lithium-ion batteries was 957.7GWh, just one step away from TWh, a year-on-year increase of 70.3%; China's lithium-ion battery shipments reached 660.8GWh, a year-on-year increase of 97.7%, accounting for 69.0% of the global total shipments of lithium-ion batteries. China's lithium iron phosphate battery installations accounted for more than 62% of the total installations, while the share of ternary batteries dropped to less than 38%.
[0007] The life cycle of lithium-ion power batteries is generally 5-8 years, and some are even shorter. With the widespread application of LiFePO4 positive electrode materials and the passage of time, a large number of waste lithium-ion power batteries will be generated. The recycling of waste lithium iron phosphate battery positive electrode materials has become an important task. The prior art mentions the use of waste lithium iron phosphate batteries to regenerate lithium iron phosphate positive electrode materials or lithium iron manganese phosphate positive electrode materials through precise separation and a series of means, but their electrochemical performance is not as good as that of the original lithium iron phosphate positive electrode materials or lithium iron manganese phosphate positive electrode materials. There are also reports on the use of acid hydrolysis to re-synthesize lithium iron phosphate positive electrode materials or lithium iron manganese phosphate positive electrode materials. The lithium iron phosphate positive electrode materials or lithium iron manganese phosphate positive electrode materials synthesized by this method are basically consistent with the original performance, but the currently reported preparation methods of lithium iron manganese phosphate basically use high-purity chemical reagents for synthesis, and their costs are relatively high.
[0008] Mn 3+ / Mn 2+ Relative to Li + / Li has a higher potential, which makes LiFeMnPO4 / C composite material have the advantage of relatively high energy density, and people are paying more and more attention to lithium manganese iron phosphate materials. 1-x Mn x Compared with LiFePO4, PO4 has weaker cycle stability, but its advantages are higher operating voltage (3.8V) and lower self-discharge rate. The general electrolyte on the market can remain stable and not decompose within the voltage range of 4.0V, and will not reduce the specific energy due to too low voltage, so it is inevitable that lithium manganese iron phosphate will be widely used.
[0009] Therefore, if zinc anode mud and lithium iron phosphate waste can be used to prepare lithium iron manganese phosphate materials, it will not only make comprehensive utilization of waste resources from two different industries and save resources, but also meet the current market's growing demand for lithium iron manganese phosphate positive electrode materials, and has very broad application prospects. Summary of the invention
[0010] The purpose of the present invention is to provide a method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste, which can not only use manganese in zinc anode mud and lithium, iron and phosphorus in lithium iron phosphate waste as raw materials to prepare high-quality and high-purity lithium iron manganese phosphate positive electrode material, so that the manganese recovery rate is as high as 98%, and the recovery rates of Li, Fe and P are all over 98.5%, but also can separate and recover valuable metals such as zinc, copper, lead and silver from zinc anode mud.
[0011] In order to solve the above technical problems, the present invention provides a method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste, comprising the following steps:
[0012] Add zinc anode mud and dilute sulfuric acid into a ball mill for slurry dezincification, and filter to obtain slurry dezincification slag and zinc sulfate solution;
[0013] The pulped dezincification slag and starch are added to a phosphoric acid solution for leaching, and when the pH value of the leaching end point is 0.5 to 2.0, a manganese dihydrogen phosphate leaching solution and lead-silver slag are obtained by filtering;
[0014] Iron powder is added to the manganese dihydrogen phosphate leaching solution to remove impurities, and activated carbon is added for adsorption before filtering, and then filtered to obtain iron powder impurity removal liquid and iron powder impurity removal residue;
[0015] The lithium iron phosphate waste is oxidized and roasted in an air atmosphere to obtain roasted sand composed of lithium iron phosphate and iron oxide;
[0016] Adding roasted sand and lithium source, iron source, manganese source and carbon source into the iron powder impurity removal liquid for batching, and then subjecting the batching to two-stage ball milling and spray drying for activation to obtain lithium manganese iron phosphate precursor;
[0017] The lithium iron manganese phosphate material is obtained by solid phase synthesis by sintering the lithium iron manganese phosphate precursor at high temperature in an inert atmosphere.
[0018] Furthermore, the mass ratio of the zinc anode mud to the dilute sulfuric acid is 1:3-1:6, the concentration of the dilute sulfuric acid is 30-50 g / L, the slurry dezincification temperature is 55-65° C., and the time is 1.0-1.5 h.
[0019] Furthermore, the amount of starch used is such that the Mn content of the pulped dezincified slag is 4+ Reduction to Mn 2+ The molar amount of phosphoric acid in the phosphoric acid solution is 1.05 to 1.30 times the theoretical amount, and the molar amount of phosphoric acid in the phosphoric acid solution is 2.15 to 2.30 times the molar amount of manganese in the slurry dezincification slag.
[0020] Furthermore, the liquid-solid mass ratio of the phosphoric acid solution to the slurry dezincification slag and starch is 4:1-6:1, the leaching temperature is 70-85° C., and the leaching time is 3-5 hours.
[0021] Furthermore, the iron powder is reduced iron powder, the amount of iron powder added is 3-5g of iron powder per liter of manganese dihydrogen phosphate leaching solution, the iron powder impurity removal temperature is 70-85°C, the impurity removal time is 1-2 hours, and the activated carbon is added 20-30 minutes before filtration, and the amount of activated carbon added is 3-5g of activated carbon per liter of manganese dihydrogen phosphate leaching solution.
[0022] Furthermore, the oxidation roasting temperature of the lithium iron phosphate waste is 420-475° C., and the time is 7-9 hours. The mass percentages of F and C in the roasted sand obtained after the oxidation roasting of the lithium iron phosphate waste are less than 0.02% and 0.008%, respectively.
[0023] Furthermore, the iron powder impurity removal liquid and roasted sand are added with lithium source, iron source, manganese source and carbon source for batching after element detection, and the molar ratio of lithium, iron, manganese and phosphorus in the batching is Li:(Fe+Mn):P=(1.01-1.05):(0.96-0.99):1, and Li:Fe:P=(1.01-1.05):(0.6-0.9):1, Li:Mn:P=(1.01-1.05):(0.1-0.4):1, and the amount of carbon source added is 9%-11% of the total mass of the batching.
[0024] Furthermore, the lithium source is one of lithium carbonate, lithium oxalate and lithium hydroxide; the iron source is one of iron oxide, iron hydroxide and ferrous oxide; the manganese source is one of manganese hydroxide, manganese acetate, manganese dioxide and manganese carbonate; the carbon source is one or more of glucose, starch and sucrose.
[0025] Furthermore, the high temperature sintering solid phase synthesis of the lithium manganese iron phosphate precursor includes
[0026] First, sinter and synthesize at a temperature of 425-445°C for 9-11 hours, then heat to 600-650°C for sintering and curing for 3-5 hours, then heat to 700-750°C for sintering and purification for 16-18 hours, and finally cool to 500-550°C for sintering and activation for 6-10 hours.
[0027] Furthermore, during the high-temperature sintering solid-phase synthesis process of the lithium manganese iron phosphate precursor, the heating rate is 1.2-1.8°C / min, the cooling rate is 3-4°C / min, the furnace temperature is 90-105°C, the inert gas of the inert atmosphere is one or more of nitrogen, helium and argon, the furnace pressure during the high-temperature sintering solid-phase synthesis process is 5-10Pa, and the oxygen concentration is 5-15ppm.
[0028] The present invention provides a method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste, which makes full use of the properties of various valuable metals in the zinc anode mud, separates and enriches them to the maximum extent, and removes various harmful impurities such as zinc, lead, silver, etc. in the zinc anode mud that have an impact on the lithium iron manganese phosphate positive electrode material to be prepared in the processes of slurry dezincification, leaching separation and iron powder impurity removal, thereby ensuring the physical and chemical properties of the final lithium iron manganese phosphate material product from the source.
[0029] In addition, the present invention uses starch as a reducing agent, which has a reliable source, fast reaction, low cost, and no need for aging. It can make the manganese leaching rate in the zinc anode mud exceed 99.5%, and the manganese recovery rate in the zinc anode mud can be as high as 98%. At the same time, the iron powder impurity removal liquid does not need to be prepared into manganese phosphate but can directly prepare manganese iron phosphate lithium positive electrode material.
[0030] Moreover, the present invention adopts an acidic reduction system of phosphoric acid + reducing agent starch, and by strictly controlling the pH value of the acidic reduction leaching system to 0.5-2.0, it can not only effectively separate impurity lead and a small amount of residual zinc without introducing other impurities, but also use a small amount of acid, and have a high leaching rate of manganese, and can effectively complete the enrichment of valuable metals lead and silver and eliminate the heavy metal problem of wastewater, and can also effectively activate the lithium iron manganese phosphate precursor because starch is used as a reducing agent, thereby ensuring the quality of the lithium iron manganese phosphate material product.
[0031] At the same time, the present invention realizes the simultaneous recovery of valuable components in zinc anode mud and lithium iron phosphate waste, completes the comprehensive treatment of wastes from two different industries, the leaching reagents used in the process are common and used in small amounts, no new impurities are introduced into the lithium manganese iron phosphate, the recovery cost is low, no wastewater is generated, the prepared lithium manganese iron phosphate positive electrode material is high in quality, the contents of impurities such as copper, lead, zinc and fluorine meet the requirements of lithium manganese iron phosphate positive electrode materials, and is suitable for large-scale industrial production of lithium manganese iron phosphate.
[0032] In addition, the present invention has the advantages of reasonable process, low production cost, green environmental protection, non-toxicity, etc., which complies with the national dual carbon policy, is easy to realize industrialization, and has a very broad application prospect. At the same time, the manganese recovery rate in zinc anode mud reaches 98%, and all components of Li, Fe and P in lithium iron phosphate waste are recovered, and their recovery rates also exceed 98.5%. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 A flow chart of a method for preparing lithium iron manganese phosphate material using zinc anode mud and lithium iron phosphate waste provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0034] See also Figure 1 The present invention provides a method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste, comprising the following steps:
[0035] Step 1) Slurry dezincification: zinc anode mud and dilute sulfuric acid are added to a ball mill for slurry dezincification, and slurry dezincification slag and zinc sulfate solution are obtained by filtering.
[0036] Since zinc anode mud usually contains valuable metals such as manganese dioxide, zinc, lead and silver, among which manganese dioxide is generally insoluble in acid and alkali, lead and silver are generally insoluble in acid due to their stable chemical properties, and zinc is relatively active in chemical properties and can react with acid. Therefore, adding a certain amount of dilute sulfuric acid to zinc anode mud can dissolve and remove zinc therein, so that after the reaction is completed, slurry dezincification slag and zinc sulfate solution containing manganese dioxide, lead and silver are obtained by filtration. The zinc sulfate solution returns to the zinc system to recover zinc, and valuable substances such as manganese dioxide, lead and silver are further enriched in the slurry dezincification slag.
[0037] Among them, in order to make the zinc in the zinc anode mud completely react and dissolve, and at the same time fully enrich the manganese dioxide, lead and silver, the mass ratio of zinc anode mud to dilute sulfuric acid is controlled to be 1:3~1:6, and the concentration of dilute sulfuric acid is 30~50g / L.
[0038] In addition, in order to speed up the reaction and improve the efficiency of slurry dezincification, the zinc anode mud and dilute sulfuric acid will be slurried and dezincified during the ball milling process in the ball mill, the temperature is 55-65°C, and the time is 1.0-1.5h.
[0039] Step 2) leaching separation: adding the slurry dezincification slag and starch into a reaction tank whose reaction system is a phosphoric acid solution for acid leaching separation, and filtering to obtain dihydrogen manganese phosphate leaching solution and lead-silver slag when the leaching end point pH is 0.5-2.0.
[0040] The present invention uses starch as a reducing agent, and promotes starch fermentation under the acidic condition of phosphoric acid solution. During starch fermentation, redox reaction occurs with manganese dioxide in pulped dezincification slag, and tetravalent manganese in manganese dioxide is reduced to divalent manganese, while carbon in starch is oxidized to tetravalent manganese to generate carbon dioxide and water. At the same time, in the acidic reaction system of phosphoric acid solution, divalent manganese generated by reduction combines with phosphoric acid to form dihydrogen manganese phosphate, thereby forming dihydrogen manganese phosphate leaching solution. The undissolved lead and silver in pulped dezincification slag remain in the leaching solution after the reaction, and lead and silver enriched slag is obtained by filtration.
[0041] The invention uses starch as a reducing agent, and the source of starch is reliable and the price is low, which not only reduces the process cost and has high economic benefits, but also the starch as a reducing agent does not need to be cooked, has a fast reaction speed and high process efficiency.
[0042] In order to ensure that the reaction is complete, the amount of starch used is such that the starch can reduce the Mn content of the slurry dezincification slag to 4+ All reduced to Mn 2+The molar amount of phosphoric acid in the phosphoric acid solution is 1.05 to 1.30 times of the theoretical amount, and the molar amount of phosphoric acid in the phosphoric acid solution is 2.15 to 2.30 times of the molar amount of manganese in the slurry dezincification slag, and the liquid-solid mass ratio of the phosphoric acid solution to the slurry dezincification slag and starch is 4:1 to 6:1.
[0043] Furthermore, in order to ensure the smooth progress of the reaction, fast reaction speed and high process efficiency, the acid leaching temperature is controlled at 70-85° C. and the leaching time is 3-5 hours.
[0044] At the same time, the present invention controls the pH of the leaching end point solution to be between 0.5 and 2.0, which can not only ensure that phosphoric acid ferments starch and reacts with manganese dioxide under acidic conditions, so that tetravalent manganese is reduced to divalent manganese and generates dihydrogen manganese phosphate with phosphoric acid, but also control the dosage range of phosphoric acid to ensure that the sufficient leaching rate of manganese dioxide in the anode mud exceeds 99.5%. At the same time, the pH of the solution is between 0.5 and 2.0 under the weak acid condition, which is conducive to inhibiting the dissolution of impurities such as copper and entering the leaching solution, which can not only reduce the influence of these harmful impurities on the finally prepared lithium manganese iron phosphate positive electrode material, but also ensure the physical and chemical properties of the finally prepared lithium manganese iron phosphate material product from the source, and also facilitate subsequent purification.
[0045] Step 3) iron powder impurity removal: iron powder is added to the manganese dihydrogen phosphate leaching solution to remove impurities, and activated carbon is added for adsorption before filtering, and then filtered to obtain iron powder impurity removal liquid and iron powder impurity removal residue.
[0046] Because in the manganese dihydrogen phosphate leachate, there is phosphoric acid in addition to manganese dihydrogen phosphate, and the leachate also has ions such as copper ions and ferric iron ions. Because impurities such as less active copper are important impurities that affect the quality of the final lithium iron manganese phosphate product, the content of copper must be reduced to a relatively low level, and ferric iron is a magnetic substance, which can also affect the quality of the final lithium iron manganese phosphate product, and the ferric iron in the leachate must also be removed. Therefore, the present invention adds iron powder to the manganese dihydrogen phosphate leachate, and the iron powder can not only reduce the copper ions in the manganese dihydrogen phosphate leachate to elemental copper and precipitate out, but also react with the excess phosphoric acid in the leachate to generate ferrous phosphate, and the iron powder can also reduce a small amount of ferric iron in the leachate to ferrous iron. After the reaction is completed, in order to facilitate the small amount of copper and residual iron that are reduced in the leachate to be more easily precipitated from the leachate, activated carbon is added to the solution before filtering the reacted solution to adsorb a small amount of copper and iron in the solution, accelerating the precipitation of copper and iron. Finally, the solution is filtered to obtain an iron powder impurity removal liquid containing manganese dihydrogen phosphate and ferrous phosphate, and an iron powder impurity removal slag containing copper, iron and activated carbon.
[0047] Among them, in order to improve the reaction ability of the iron powder, the iron powder is reduced iron powder, and in order to thoroughly remove impurities from the iron powder, the amount of iron powder added is 3 to 5 g of iron powder per liter of dihydrogen manganese phosphate leaching solution. At the same time, in order to speed up the reaction speed, shorten the process time, and improve the process efficiency, when removing impurities from the iron powder, the temperature is controlled at 70 to 85° C., and the impurity removal time is 1 to 2 hours.
[0048] In addition, in order to make the activated carbon adsorb more fully, the activated carbon is added 20 to 30 minutes before filtration, and the amount of activated carbon added is 3 to 5 g per liter of dihydrogen manganese phosphate leaching solution.
[0049] Step 4) Oxidation roasting: The lithium iron phosphate waste is oxidized and roasted in an air atmosphere to obtain roasted sand composed of lithium iron phosphate and iron oxide.
[0050] The effective component of lithium iron phosphate waste is lithium iron phosphate. The lithium iron phosphate waste is calcined in an air atmosphere, and the lithium iron phosphate in the lithium iron phosphate waste reacts with oxygen in the air to generate lithium iron phosphate with positive trivalent iron and iron oxide, and the carbon and / or carbon-containing organic matter in the lithium iron phosphate waste is burned to form carbon dioxide, and F in the organic matter can be removed at the same time. In addition, the lithium iron phosphate waste with differentiated structures and the lithium iron phosphate waste with different failure mechanisms are homogenized to generate positive trivalent lithium iron phosphate and iron oxide with completely consistent structures, solving the problem of poor product consistency caused by the differentiation of raw materials, and laying a foundation for the consistency problem of the subsequent preparation of lithium iron manganese phosphate products.
[0051] In order to make the oxidation roasting more complete and thorough, the temperature of the oxidation roasting of the lithium iron phosphate waste is controlled at 420-475°C, and the roasting time is 7-9 hours. In addition, the mass percentages of F and C in the roasted sand obtained after the oxidation roasting of the lithium iron phosphate waste are less than 0.02% and 0.008% respectively.
[0052] Step 5) batching and activation: adding roasted sand and lithium source, iron source, manganese source and carbon source to the iron powder impurity removal liquid for batching, and then the batching is activated by two-stage ball milling and spray drying to obtain lithium manganese iron phosphate precursor.
[0053] Among them, in order to understand the element content in the iron powder impurity removal liquid and roasted sand in detail, so as to calculate the molar ratio of the iron powder impurity removal liquid, roasted sand, lithium source, iron source, manganese source and carbon source during batching, the iron powder impurity removal liquid and roasted sand were respectively tested for elements before batching.
[0054] When preparing the ingredients, the molar ratio of lithium, iron, manganese and phosphorus in the ingredients satisfies Li:(Fe+Mn):P=(1.01-1.05):(0.96-0.99):1, and at the same time satisfies Li:Fe:P=(1.01-1.05):(0.6-0.9):1, Li:Mn:P=(1.01-1.05):(0.1-0.4):1. In addition, the amount of carbon source added is 9%-11% of the total weight of the ingredients.
[0055] The reason why the molar ratio of lithium, iron, manganese and phosphorus in the ingredients is set to the above ratio is to better solve the chemical properties and physical properties such as the charge and discharge voltage platform and rate performance of the lithium iron manganese phosphate battery. The molar ratio of lithium, iron, manganese and phosphorus in the ingredients is controlled in order to generate a single lithium iron manganese phosphate substance. There is an appropriate surplus of lithium in the ingredients to satisfy the migration of lithium during the conduction process without failure; the molar ratio of manganese is less than that of iron in order to ensure that the prepared lithium iron manganese phosphate material has more discharge per unit lithium iron manganese phosphate after being prepared into a battery.
[0056] Among them, the lithium source is one of lithium carbonate, lithium oxalate and lithium hydroxide; the iron source is one of iron oxide, iron hydroxide and ferrous oxide; the manganese source is one of manganese hydroxide, manganese acetate, manganese dioxide and manganese carbonate; the carbon source is one or more of glucose, starch and sucrose.
[0057] Step 6) Synthesis: The lithium iron manganese phosphate precursor is sintered at high temperature in an inert atmosphere to obtain a lithium iron manganese phosphate material.
[0058] Among them, the high temperature sintering solid phase synthesis of lithium manganese iron phosphate precursor is carried out according to the following process:
[0059] First, sinter and synthesize at a temperature of 425-445°C for 9-11 hours, then heat to 600-650°C for sintering and curing for 3-5 hours, then heat to 700-750°C for sintering and purification for 16-18 hours, and finally cool to 500-550°C for sintering and activation for 6-10 hours.
[0060] Among them, during the high-temperature sintering solid-phase synthesis process of the lithium manganese iron phosphate precursor, the heating rate is 1.2-1.8°C / min, the cooling rate is 3-4°C / min, the furnace temperature is 90-105°C, the inert gas of the inert atmosphere is one or more of nitrogen, helium and argon, the furnace pressure during the high-temperature sintering solid-phase synthesis process is 5-10Pa, and the oxygen concentration is 5-15ppm.
[0061] The present invention provides a method for preparing lithium iron manganese phosphate material by utilizing zinc anode mud and lithium iron phosphate waste. Through the above process steps, efficient recovery of valuable metals such as lead, silver, zinc, and manganese in the zinc anode mud and recovery of all components of lithium iron phosphate waste can be achieved, and finally the lithium iron manganese phosphate material can be prepared through recycling, thereby realizing the comprehensive utilization of waste materials from two different industries.
[0062] The following is a specific description of a method for preparing lithium iron manganese phosphate material using zinc anode mud and lithium iron phosphate waste provided by the present invention through examples.
[0063] Example 1
[0064] Lithium iron manganese phosphate material is prepared using zinc anode mud with components of Zn 2.68wt%, Mn 35.85wt%, Pb15.31wt%, Ag0.0570wt% and lithium iron phosphate waste, and the remaining valuable metals in the zinc anode mud are comprehensively recovered.
[0065] 1. Slurry dezincification: zinc anode mud and dilute sulfuric acid with a titer of 30g / L are added into a ball mill at a mass ratio of 1:6, and then ball milled for slurry dezincification. The slurrying temperature is 55°C and the slurrying time is 1.5h. After filtering, slurry dezincification slag and zinc sulfate solution are obtained;
[0066] 2. Leaching separation: the obtained slurry dezincification slag and 1.05 times the theoretical amount of starch are added into a reaction tank with phosphoric acid as the reaction system for acid leaching separation, the amount of phosphoric acid used is 2.15 times the molar amount of manganese, the liquid-solid weight ratio is 6:1, the leaching separation temperature is 85°C, the time is 3 hours, the leaching end point pH is 2.0, and the dihydrogen manganese phosphate solution and lead-silver slag are obtained by filtration;
[0067] 3. Iron powder impurity removal: Add reduced iron powder to the obtained manganese dihydrogen phosphate leaching solution for impurity removal, with an addition amount of 3g / L, a temperature of 70°C, and a time of 2 hours. 20 minutes before filtration, add 5g of activated carbon per liter of solution for adsorption, and separate the liquid and solid to obtain iron powder impurity removal liquid and iron powder impurity removal slag;
[0068] 4. Oxidation roasting: roast the lithium iron phosphate waste in an air atmosphere at a temperature of 475°C for 7 hours, and obtain roasted sand composed of lithium iron phosphate (III) and iron oxide after cooling;
[0069] 5. Batching and activation: Add the obtained roasted sand, lithium carbonate, iron oxide, manganese carbonate and glucose to the iron powder impurity removal liquid after element detection for batching, wherein the amount of glucose added is 11% of the batching mass, wherein the molar ratio of lithium, iron, manganese and phosphorus is Li:(Fe+Mn):P=1.01:0.99:1, Li:Fe:P=1.01:0.9:1, Li:Mn:P=1.01:0.1:1, and perform two-stage ball milling and spray drying activation to obtain a lithium manganese iron phosphate precursor;
[0070] 6. Synthesis: The obtained lithium iron manganese phosphate precursor was sintered under nitrogen protection, maintaining the furnace pressure at 5Pa, the oxygen concentration at 15ppm, the heating rate at 1.2℃ / min, the sintering synthesis temperature at 445℃, the synthesis time at 9h, the sintering and curing temperature at 600℃, the curing time at 5h, the sintering and purification temperature at 750℃, the purification time at 16h, the cooling rate at 3℃ / min, the sintering activation temperature at 500℃, and the activation time at 10h to perform high-temperature solid phase synthesis of lithium iron manganese phosphate positive electrode material.
[0071] Through the comprehensive recovery of zinc anode mud and lithium iron phosphate waste, the manganese recovery rate in zinc anode mud reached 98.6%, lead and silver were enriched in lead-silver slag, and all components of Li, Fe and P in manganese lithium iron phosphate waste were recovered with a recovery rate of 98.8%; the impurity content of Pb, Zn, Ca, Mg and other impurities in the prepared manganese lithium iron phosphate positive electrode material was at the ppm level, and it also had excellent physical and chemical properties, with a discharge capacity of 1C of 151.38mAh / g.
[0072] Example 2
[0073] Lithium iron manganese phosphate material is prepared using zinc anode mud with components of Zn 2.68wt%, Mn 35.85wt%, Pb15.31wt%, Ag0.0570wt% and lithium iron phosphate waste, and the remaining valuable metals in the zinc anode mud are comprehensively recovered.
[0074] 1. Slurry dezincification: zinc anode mud and dilute sulfuric acid with a titer of 40g / L are added into a ball mill at a mass ratio of 1:4, and then ball milled for slurry dezincification. The slurrying temperature is 60°C and the slurrying time is 1.2h. After filtering, slurry dezincification slag and zinc sulfate solution are obtained;
[0075] 2. Leaching separation: the obtained slurry dezincification slag and 1.15 times the theoretical amount of starch are added into a reaction tank with phosphoric acid as the reaction system for acid leaching separation, the amount of phosphoric acid used is 2.25 times the molar amount of manganese, the liquid-solid weight ratio is 5:1, the leaching separation temperature is 80°C, the time is 4 hours, the leaching end point pH is 1.0, and the manganese dihydrogen phosphate solution and lead-silver slag are obtained by filtration;
[0076] 3. Iron powder impurity removal: Add reduced iron powder to the obtained manganese dihydrogen phosphate leaching solution for impurity removal, the addition amount is 4g / L, the temperature is 80℃, the time is 1.5 hours, 25min before filtration, 4g of activated carbon is added per liter of solution for adsorption, and the iron powder impurity removal liquid and iron powder impurity removal slag are obtained by liquid-solid separation;
[0077] 4. Oxidation roasting: roast the lithium iron phosphate waste in an air atmosphere at a temperature of 450°C for 8 hours, and obtain roasted sand composed of lithium iron phosphate (III) and iron oxide after cooling;
[0078] 5. Batching and activation: Add the obtained roasted sand, lithium oxalate, iron hydroxide, manganese hydroxide and starch to the iron powder impurity removal liquid after element detection for batching, wherein the amount of starch added is 10% of the batching mass, wherein the molar ratio of lithium, iron, manganese and phosphorus is Li:(Fe+Mn):P=1.03:0.97:1, Li:Fe:P=1.03:0.7:1, Li:Mn:P=1.03:0.27:1, and perform two-stage ball milling and spray drying activation to obtain a lithium manganese iron phosphate precursor;
[0079] 6. Synthesis: The obtained lithium iron manganese phosphate precursor was sintered under helium protection, maintaining the furnace pressure at 8Pa, the oxygen concentration at 5ppm, the heating rate at 1.5℃ / min, the sintering synthesis temperature at 435℃, the synthesis time at 10h, the sintering curing temperature at 630℃, the curing time at 4h, the sintering purification temperature at 720℃, the purification time at 17h, the cooling rate at 3.5℃ / min, the sintering activation temperature at 520℃, and the activation time at 8h to carry out high-temperature solid phase synthesis of lithium iron manganese phosphate positive electrode material.
[0080] Through the comprehensive recovery of zinc anode mud and lithium iron phosphate waste, the manganese recovery rate in zinc anode mud reached 98.9%, lead and silver were enriched in lead-silver slag, and all components of Li, Fe and P in manganese lithium iron phosphate waste were recovered with a recovery rate of 99.2%; the impurity content of Pb, Zn, Ca, Mg and so on in the prepared manganese lithium iron phosphate positive electrode material was at the ppm level, and it also had excellent physical and chemical properties, with a discharge capacity of 1C of 150.86mAh / g.
[0081] Example 3
[0082] Lithium iron manganese phosphate material is prepared using zinc anode mud with components of Zn 2.68wt%, Mn 35.85wt%, Pb15.31wt%, Ag0.0570wt% and lithium iron phosphate waste, and the remaining valuable metals in the zinc anode mud are comprehensively recovered.
[0083] 1. Slurry dezincification: zinc anode mud and dilute sulfuric acid with a titer of 50g / L are added into a ball mill at a mass ratio of 1:3, and then ball milled for slurry dezincification. The slurrying temperature is 65°C and the slurrying time is 1.0h. After filtering, slurry dezincification slag and zinc sulfate solution are obtained;
[0084] 2. Leaching separation: the obtained slurry dezincification slag and 1.30 times the theoretical amount of starch are added into a reaction tank with phosphoric acid as the reaction system for acid leaching separation, the amount of phosphoric acid used is 2.30 times the molar amount of manganese, the liquid-solid weight ratio is 4:1, the leaching separation temperature is 70°C, the time is 5 hours, the leaching end point pH is 0.5, and the dihydrogen manganese phosphate solution and lead-silver slag are obtained by filtration;
[0085] 3. Iron powder impurity removal: Add reduced iron powder to the obtained manganese dihydrogen phosphate leaching solution for impurity removal, the addition amount is 5g / L, the temperature is 85°C, the time is 1 hour, 30 minutes before filtration, 3g of activated carbon is added per liter of solution for adsorption, and liquid-solid separation is performed to obtain iron powder impurity removal liquid and iron powder impurity removal slag;
[0086] 4. Oxidation roasting: roast the lithium iron phosphate waste in an air atmosphere at a temperature of 420°C for 9 hours, and obtain roasted sand composed of lithium iron phosphate (III) and iron oxide after cooling;
[0087] 5. Batching and activation: adding the obtained roasted sand, lithium hydroxide, ferrous oxide, manganese dioxide and starch + sucrose to the iron powder impurity removal liquid after element detection for batching, wherein the amount of starch + sucrose added is 9% of the batching mass, wherein the molar ratio of lithium, iron, manganese and phosphorus is Li: (Fe + Mn): P = 1.05: 0.96: 1, Li: Fe: P = 1.05: 0.6: 1, Li: Mn: P = 1.05: 0.4: 1, and performing two-stage ball milling and spray drying activation to obtain a lithium manganese iron phosphate precursor;
[0088] 6. Synthesis: The lithium iron manganese phosphate precursor obtained in step E was sintered under argon protection, maintaining a furnace pressure of 10 Pa, an oxygen concentration of 5 ppm, a heating rate of 1.8 ° C / min, a sintering synthesis temperature of 425 ° C, a synthesis time of 11 h, a sintering curing temperature of 650 ° C, a curing time of 3 h, a sintering purification temperature of 700 ° C, a purification time of 18 h, a cooling rate of 4 ° C / min, a sintering activation temperature of 550 ° C, and an activation time of 6 h to perform high-temperature solid phase synthesis of lithium iron manganese phosphate positive electrode material.
[0089] Through the comprehensive recovery of zinc anode mud and lithium iron phosphate waste, the manganese recovery rate in zinc anode mud reached 98.6%, lead and silver were enriched in lead-silver slag, and all components of Li, Fe and P in manganese lithium iron phosphate waste were recovered, and their recovery rates exceeded 99.1%; the impurity contents of Pb, Zn, Ca, Mg and other impurities in the prepared manganese lithium iron phosphate positive electrode material were at the ppm level, and it also had excellent physical and chemical properties, with a discharge capacity of 1C of 152.15mAh / g.
[0090] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing lithium iron manganese phosphate material using zinc anode mud and lithium iron phosphate waste, It is characterized in that The steps include: Add zinc anode mud and dilute sulfuric acid into a ball mill for slurry dezincification, and filter to obtain slurry dezincification slag and zinc sulfate solution; The pulped dezincification slag and starch are added to a phosphoric acid solution for leaching, and when the pH value of the leaching end point is 0.5 to 2.0, a manganese dihydrogen phosphate leaching solution and lead-silver slag are obtained by filtering; Iron powder is added to the manganese dihydrogen phosphate leaching solution to remove impurities, and activated carbon is added for adsorption before filtering, and then filtered to obtain iron powder impurity removal liquid and iron powder impurity removal residue; The lithium iron phosphate waste is oxidized and roasted in an air atmosphere to obtain roasted sand composed of lithium iron phosphate and iron oxide; Adding roasted sand and lithium source, iron source, manganese source and carbon source into the iron powder impurity removal liquid for batching, and then subjecting the batching to two-stage ball milling and spray drying for activation to obtain lithium manganese iron phosphate precursor; The lithium iron manganese phosphate material is obtained by solid phase synthesis by sintering the lithium iron manganese phosphate precursor at high temperature in an inert atmosphere.
2. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 1, Features: The mass ratio of the zinc anode mud to the dilute sulfuric acid is 1:3-1:6, the concentration of the dilute sulfuric acid is 30-50 g / L, the slurry dezincification temperature is 55-65° C., and the time is 1.0-1.5 h.
3. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 1, Features: The amount of starch used is to reduce the Mn content of the slurry dezincification slag to 4+ Reduction to Mn 2+ The molar amount of phosphoric acid in the phosphoric acid solution is 1.05 to 1.30 times the theoretical amount, and the molar amount of phosphoric acid in the phosphoric acid solution is 2.15 to 2.30 times the molar amount of manganese in the slurry dezincification slag.
4. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 3, Features: The liquid-solid mass ratio of the phosphoric acid solution to the slurry dezincification slag and starch is 4:1-6:1, the leaching temperature is 70-85° C., and the leaching time is 3-5 hours.
5. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 1, Features: The iron powder is reduced iron powder, and the amount of iron powder added is 3-5g per liter of manganese dihydrogen phosphate leaching solution. The iron powder impurity removal temperature is 70-85° C., and the impurity removal time is 1-2 hours. The activated carbon is added 20-30 minutes before filtration, and the amount of activated carbon added is 3-5g per liter of manganese dihydrogen phosphate leaching solution.
6. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 1, Features: The oxidation roasting temperature of the lithium iron phosphate waste is 420-475° C., and the time is 7-9 hours. The mass percentages of F and C in the roasted sand obtained after the oxidation roasting of the lithium iron phosphate waste are less than 0.02% and 0.008% respectively.
7. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 1, Features: The iron powder impurity removal liquid and roasted sand are added with lithium source, iron source, manganese source and carbon source for batching after element detection. The molar ratio of lithium, iron, manganese and phosphorus in the batch is Li:(Fe+Mn):P=(1.01-1.05):(0.96-0.99):1, and Li:Fe:P=(1.01-1.05):(0.6-0.9):1, Li:Mn:P=(1.01-1.05):(0.1-0.4):1, and the amount of carbon source added is 9%-11% of the total mass of the batch.
8. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 7, Features: The lithium source is one of lithium carbonate, lithium oxalate and lithium hydroxide; the iron source is one of ferric oxide, ferric hydroxide and ferrous oxide; the manganese source is one of manganese hydroxide, manganese acetate, manganese dioxide and manganese carbonate; the carbon source is one or more of glucose, starch and sucrose.
9. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 1, It is characterized in that The high temperature sintering solid phase synthesis of the lithium manganese iron phosphate precursor comprises: First, sinter and synthesize at a temperature of 425-445°C for 9-11 hours, then heat to 600-650°C for sintering and curing for 3-5 hours, then heat to 700-750°C for sintering and purification for 16-18 hours, and finally cool to 500-550°C for sintering and activation for 6-10 hours.
10. The method for preparing lithium iron manganese phosphate material by using zinc anode mud and lithium iron phosphate waste according to claim 9, Features: During the high-temperature sintering solid-phase synthesis process of the lithium manganese iron phosphate precursor, the heating rate is 1.2-1.8°C / min, the cooling rate is 3-4°C / min, the furnace temperature is 90-105°C, the inert gas of the inert atmosphere is one or more of nitrogen, helium and argon, the furnace pressure during the high-temperature sintering solid-phase synthesis process is 5-10Pa, and the oxygen concentration is 5-15ppm.
Citation Information
Patent Citations
Method for recovering valued metals from zinc anode sludge
CN102586599A
Method of recycling zinc, manganese, lead and silver from zinc electrowinning anode mud
CN102912138A
Method for recycling and preparing lithium iron manganese phosphate from positive electrode materials of waste lithium iron phosphate batteries
CN104609385A
Method of recycling waste lithium iron phosphate battery and lithium manganate battery
CN106997975A
Method for repairing and regenerating lithium iron manganese phosphate by using lithium iron phosphate waste powder and lithium iron manganese phosphate waste powder
CN116621146A