Low-temperature-resistant sponge sealing strip and preparation method thereof

By improving the compatibility of modified EPDM and EPDM rubber, combined with the synergistic effect of composite flame retardant, the problem of degradation of sealing strips in low temperature environments is solved, and the low-temperature resistant sponge sealing strips are realized Excellent mechanical properties and long service life, suitable for multi-field applications.

CN118956065APending Publication Date: 2024-11-15NINGBO NEWANTON SEAL & INSULATION SYST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411299478.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing EPDM seal strips become brittle and deformed in low temperature environments, resulting in a degradation of sealing performance and inability to return to their original state, limiting their application range.

Method used

Modified EPDM rubber and EPDM rubber are adopted by modifying EPDM rubber, zinc oxide, stearic acid, reinforcement, composite flame retardant, plasticizer, anti-aging agent and sulfur. The compatibility of the graphene oxide modified melamine polyphosphate and silane coupling agent modified nanoantimon trioxide improves the low temperature resistance, flame retardant and mechanical properties of the material.

Benefits of technology

It achieves good mechanical properties, long service life, excellent low temperature resistance and excellent flame retardant properties of low temperature sponge sealing strips, and is suitable for applications in many fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047188030000091
    Figure BDA0005047188030000091
Patent Text Reader

Abstract

The invention relates to the technical field of sealing strips, in particular to a low-temperature-resistant sponge sealing strip and a preparation method thereof. The low-temperature-resistant sponge sealing strip is prepared from the following raw materials in parts by mass: 20 to 25 parts of modified ethylene propylene diene monomer, 60 to 65 parts of ethylene propylene diene monomer, 4 to 5 parts of zinc oxide, 0.5 to 0.8 part of stearic acid, 50 to 55 parts of reinforcing agent, 3 to 4 parts of composite flame retardant, 10 to 12 parts of plasticizer, 3 to 4 parts of anti-aging agent, 1.0 to 1.5 parts of sulfur and 1 to 3 parts of accelerant, the composite flame retardant is prepared from graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide. According to the low-temperature-resistant sponge sealing strip, due to the innovative material combination and preparation process, excellent flame retardance, low-temperature resistance and mechanical property are achieved, the service life is prolonged, meanwhile, production simplicity and economical efficiency are kept, and the requirements of modern industry for high-performance sealing materials are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of sealing strips, and in particular to a low-temperature resistant sponge sealing strip and a preparation method thereof. Background Art

[0002] Ethylene propylene diene monomer (EPDM) is a terpolymer made of ethylene, propylene and an unsaturated third monomer (non-conjugated diene). The third monomer of EPDM mainly includes ENB (5-ethylidene-2-norbornene), DCPD (dicyclopentadiene), HD (1,4-hexadiene) and VNB (5-vinyl-2-norbornene). The molecular structure of EPDM determines that it has excellent aging resistance, chemical resistance, and excellent electrical insulation properties. It is currently widely used in rubber products such as automotive parts, waterproof materials for construction, wires and cables, hoses, tapes, and automotive seals. Although EPDM has the above-mentioned excellent properties, it also has certain disadvantages, which limit its promotion and application in some special fields. For example, the low-temperature performance is average. When the vinyl content in the EPDM molecular chain is high, it has a certain crystallinity, which reduces its elasticity at low temperatures, and even makes it hard and brittle, losing its practical use value.

[0003] Currently, sealing strips are usually made of ethylene propylene diene monomer (EPDM), which may become brittle and deformed in low temperature environments, causing the seal to become hard and its resilience to weaken, and it may not be able to return to its original state, making it difficult to seal and open and close the door. Summary of the invention

[0004] The purpose of this application is to provide a low-temperature resistant sponge sealing strip and a preparation method thereof in response to the deficiencies of current technology. The low-temperature resistant sponge sealing strip of the present application has a simple preparation process and is easy to prepare on a large scale; the product has the advantages of good mechanical properties, long service life, good low-temperature resistance and excellent flame retardant properties.

[0005] In the first aspect, the present application provides a low temperature resistant sponge sealing strip, which adopts the following technical solution: A low-temperature resistant sponge sealing strip comprises the following raw materials in parts by mass: 20-25 parts of modified EPDM rubber, 60-65 parts of EPDM rubber, 4-5 parts of zinc oxide, 0.5-0.8 parts of stearic acid, 50-55 parts of reinforcing agent, 3-4 parts of composite flame retardant, 10-12 parts of plasticizer, 3-4 parts of antioxidant, 1.0-1.5 parts of sulfur and 1-3 parts of accelerator, wherein the composite flame retardant is composed of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide.

[0006] By adopting the above technical scheme, the modified EPDM rubber is modified by methyl hydrogen silicone oil, and this modification significantly improves the cold resistance of the material. At the same time, due to its good compatibility with unmodified EPDM rubber, it helps to improve the mechanical properties and service life of the overall material. EPDM rubber is used as the main substrate, and EPDM rubber provides good elasticity and weather resistance. Its high filling capacity allows a large amount of reinforcing agents and other functional additives to be added without damaging its basic physical properties. Zinc oxide is used as a vulcanization catalyst. During the rubber vulcanization process, zinc oxide can accelerate the vulcanization process and improve the vulcanization efficiency, thereby improving the physical properties of the finished product. Stearic acid is used as a processing aid. Stearic acid plays a softening and plasticizing role in the rubber mixing process and improves the processability of the rubber. The reinforcing agent is usually carbon black or wollastonite, which can significantly improve the mechanical strength and wear resistance of the rubber. The composite flame retardant is composed of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide. This composite flame retardant can release flame retardant gases such as phosphoric acid when burning, forming a protective layer, slowing down the burning speed and preventing the spread of flames. In addition, these two modifiers improve the compatibility of the flame retardant with EPDM rubber, promote its uniform dispersion in the material, and thus improve the flame retardant and mechanical properties. Plasticizers are used to increase the flexibility and processability of rubber mixtures, reduce the hardness of materials, and make products softer and more elastic. Anti-aging agents are used to delay the aging of rubber due to oxidation, heat, light and other factors, and extend the service life of products. Sulfur is an indispensable cross-linking agent in the vulcanization process of rubber, which improves the physical properties of rubber by forming a cross-linked network structure. Accelerators accelerate the vulcanization process, make the vulcanization reaction more complete, and further improve the physical and chemical properties of rubber products. In summary, these components contribute to the excellent performance of low-temperature resistant sponge sealing strips through their respective specific functions and the synergistic effects between them in this application, including good mechanical properties, long service life, excellent low-temperature resistance and outstanding flame retardant properties.

[0007] Preferably, the mass ratio of the graphene oxide modified melamine polyphosphate to the silane coupling agent modified nano antimony trioxide is 4:2-3.

[0008] By adopting the above technical scheme, graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide are used as key components of the composite flame retardant, and the mass ratio between them is 4:2-3. This ratio is adjusted to maximize their respective performance advantages and achieve synergistic effects, thereby significantly improving the flame retardant effect of low-temperature resistant sponge sealing strips. During the combustion process of graphene oxide modified melamine polyphosphate, the modified melamine polyphosphate can release flame retardant gases such as phosphoric acid, which can form a protective layer to effectively slow down the combustion rate and prevent the spread of flames. Through the modification of γ-aminopropyltrimethoxysilane and graphene oxide, the compatibility of melamine polyphosphate with EPDM rubber is improved, which is conducive to improving its dispersibility in the sealing strip, thereby improving the uniformity and overall performance of the material. As a synergistic flame retardant, the good compatibility of silane coupling agent modified nano antimony trioxide with EPDM rubber helps to improve its dispersibility in the sealing strip, thereby improving the flame retardant performance. Nano antimony trioxide can form a stable protective layer when burning, and work together with the flame-retardant gas released by graphene oxide modified melamine polyphosphate to form a more effective barrier layer, further preventing oxygen from reaching the combustion area and delaying the combustion of the material. The combination of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide realizes the combination of gas phase and condensed phase flame retardant mechanisms, providing more comprehensive flame retardant protection. The synergistic effect of these two flame retardants not only improves the flame retardant effect, but also improves production efficiency and product performance consistency due to better dispersibility and compatibility. By adjusting the ratio of these two components, flame retardant properties and other physical properties, such as mechanical properties and low temperature resistance, can be optimized for different application requirements. In summary, the mass fraction ratio of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide is 4:2-3. In this application, through their synergistic effect, not only the flame retardant effect of the low temperature resistant sponge sealing strip is significantly improved, but also the overall performance of the material is enhanced by improving dispersibility and compatibility.

[0009] Preferably, the method for preparing the graphene oxide modified melamine polyphosphate comprises the following steps: S31, preparing an aqueous suspension by mixing 30 parts of hydrotalcite and 40 parts of water in parts by mass; S32, dispersing 250 parts of melamine polyphosphate and 10 parts of graphene oxide in a solution consisting of 10 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 30 parts of water according to mass fractions to obtain a mixed solution; S33, slowly adding the water suspension to the mixed solution, heating to 46°C, stirring at a rate of 500 rpm, reacting for 50-60 minutes, filtering, and vacuum drying at 80°C for 24 hours, grinding and sieving to obtain graphene oxide modified melamine polyphosphate with a particle size of 5-10 μm.

[0010] By adopting the above technical scheme, the preparation method of graphene oxide modified melamine polyphosphate involves multiple key steps, which ensure the effective combination of the modifier and melamine polyphosphate, thereby improving its application performance in low-temperature resistant sponge sealing strips. S31. Preparation of an aqueous suspension. First, 30 parts of hydrotalcite and 40 parts of water are mixed to prepare an aqueous suspension. As a layered material, hydrotalcite can provide a large amount of surface area, which is conducive to the subsequent reaction. S32. Preparation of a mixed solution. 250 parts of melamine polyphosphate and 10 parts of graphene oxide are dispersed in a solution consisting of 10 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 30 parts of water. This step is critical because graphene oxide has excellent physical properties and chemical stability, and γ-aminopropyltrimethoxysilane, as a coupling agent, can promote the combination of graphene oxide and melamine polyphosphate. S33. Reaction and post-treatment, slowly add the water suspension to the mixed solution, heat to 46 ° C, and react for 50-60 minutes at a stirring rate of 500 rpm. These conditions ensure that the reaction is fully carried out. After the reaction is completed, filter and vacuum dry at 80 ° C for 24 hours, then grind and sieve to obtain graphene oxide modified melamine polyphosphate with a particle size of 5-10 μm. The modified melamine polyphosphate can release flame-retardant gases such as phosphoric acid during combustion to form a protective layer, effectively slowing down the combustion rate and preventing the spread of flames. Through the modification of γ-aminopropyltrimethoxysilane, the compatibility of melamine polyphosphate with EPDM rubber is improved, which is conducive to improving its dispersibility in the sealing strip, thereby improving the uniformity and overall performance of the material. The addition of graphene oxide not only improves the flame retardant efficiency of melamine polyphosphate, but also may enhance the mechanical properties of the sealing strip through its excellent physical properties and extend the service life. In summary, the preparation method of this modified melamine polyphosphate provides a good basis for its application in low-temperature resistant sponge sealing strips, and achieves multi-faceted improvements in product performance by improving flame retardant properties, enhancing compatibility and dispersibility, and utilizing the physical properties of graphene oxide.

[0011] Preferably, the preparation method of the silane coupling agent modified nano antimony trioxide is as follows: according to the mass fraction, 10 parts of nano antimony trioxide with a particle size of 20 nm are dispersed in a solution consisting of 0.15 parts of γ-aminopropyltrimethoxysilane, 20 parts of ethanol and 3 parts of water to obtain a mixed solution; the heating temperature is 42°C, the stirring rate is 200rpm, the reaction is carried out for 40-50min, and then the mixture is filtered and vacuum dried at 82°C for 20-24h to obtain the silane coupling agent modified nano antimony trioxide.

[0012] By adopting the above technical scheme, the prepared modified nano antimony trioxide can form a stable protective layer during the combustion process, and work together with the flame-retardant gas released by graphene oxide modified melamine polyphosphate to form a more effective barrier layer, further preventing oxygen from reaching the combustion area and delaying the combustion of the material. Through the modification of silane coupling agent, the compatibility of nano antimony trioxide with EPDM rubber is improved, which is conducive to improving its dispersibility in the sealing strip, thereby improving the uniformity and overall performance of the material. The combination of silane coupling agent modified nano antimony trioxide and graphene oxide modified melamine polyphosphate realizes the combination of gas phase and condensed phase flame retardant mechanisms, provides more comprehensive flame retardant protection, and may enhance the mechanical properties and durability of the sealing strip by improving dispersibility and compatibility. In summary, the preparation method of this modified nano antimony trioxide provides a good foundation for its application in low-temperature resistant sponge sealing strips, and achieves multi-faceted improvement of product performance by improving flame retardant properties, enhancing compatibility and dispersibility, and utilizing the characteristics of silane coupling agents.

[0013] Preferably, the preparation method of the modified EPDM rubber is as follows: according to the mass parts, 100 parts of EPDM rubber and 20 parts of methyl hydrogen silicone oil are dissolved in 200 parts of toluene, 0.5 parts of platinum catalyst are added, and after reacting at 160°C for 70 minutes, the solvent is removed by reduced pressure distillation at 0.1 MPa and 65°C for 70 minutes, and then vacuum drying is carried out at 60°C for 24 hours to obtain the modified EPDM rubber.

[0014] By adopting the above technical scheme, the key steps involved in the preparation method of modified EPDM rubber ensure the effective combination of this rubber and methyl hydrogen silicone oil, thereby improving its application performance in low-temperature resistant sponge sealing strips. First, 100 parts of EPDM rubber and 20 parts of methyl hydrogen silicone oil are dissolved in 200 parts of toluene. Toluene, as a solvent, helps to mix the components evenly. Subsequently, 0.5 parts of platinum catalyst are added. The platinum catalyst plays a key catalytic role here to promote subsequent chemical reactions. React at 160°C for 70 minutes. This combination of temperature and time is to allow EPDM rubber and methyl hydrogen silicone oil to fully react and form a stable chemical structure. After the reaction is completed, the solvent is removed by reduced pressure distillation at 0.1MPa and 65°C for 70 minutes. Reduced pressure distillation helps to effectively remove toluene at a lower temperature to prevent the adverse effects of high temperature on product performance. Finally, vacuum drying is performed at 60°C for 24 hours to ensure that all residual solvents are completely removed to obtain the final modified EPDM rubber. The modified EPDM rubber has significantly improved its cold resistance by modification with methyl hydrogen silicone oil. This is because methyl hydrogen silicone oil itself has excellent low temperature resistance, and the silicon-oxygen bonds in its structure provide the material with good flexibility and cold resistance. The modified EPDM rubber has good compatibility with the unmodified EPDM rubber, which helps to maintain the uniformity and overall mechanical properties of the material. At the same time, the addition of methyl hydrogen silicone oil may also improve the flexibility and ductility of the material, thereby extending the service life of the sealing strip. The excellent cold resistance of the modified EPDM rubber combined with the flame retardant properties of other components such as composite flame retardants enables the final low-temperature resistant sponge sealing strip to maintain good performance in extreme low temperature environments and have excellent flame retardant properties. In summary, the preparation method of this modified EPDM rubber provides a good foundation for its application in low-temperature resistant sponge sealing strips, and achieves multi-faceted improvements in product performance by improving cold resistance, maintaining mechanical properties and compatibility, and achieving synergistic effects with other components.

[0015] Preferably, the ethylene content of the EPDM rubber is 48% by weight, the third monomer content of ENB is 5% by weight, and the effective substance platinum content of the platinum catalyst is 6wt%.

[0016] Preferably, the reinforcing agent is composed of N550 carbon black, N330 carbon black and N762 carbon black in a mass ratio of 5:3:3.

[0017] Preferably, the plasticizer is EPDM rubber grafted with maleic anhydride, wherein the mass content of maleic anhydride is 2%.

[0018] Preferably, the accelerator is at least one of accelerator ZDTP50, accelerator CLD80 and accelerator ZBEC7; and the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.

[0019] In a second aspect, the present application provides a method for preparing a low-temperature resistant sponge sealing strip, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned low-temperature resistant sponge sealing strip, comprising the following steps: S101, respectively adding modified EPDM rubber and EPDM rubber to a rubber mixing device according to their weight fractions and stirring them evenly, then adding zinc oxide, stearic acid, a reinforcing agent and a composite flame retardant for mixing, then adding a plasticizer, an antioxidant and an accelerator, mixing evenly and adding sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 170-180°C and the vulcanization pressure is 180-200kg / cm 2 The vulcanization time is 8-12 minutes, and finally it is extruded by an extruder to form a low-temperature resistant sponge sealing strip.

[0020] By adopting the above technical scheme, the preparation method of a low-temperature resistant sponge sealing strip of the present application is simple, the operation and control are convenient, the produced product is of high quality, the cost is low, and it is conducive to industrial production.

[0021] In summary, the beneficial technical effects of this application are: 1. Excellent flame retardant properties By using graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide as composite flame retardants, the sponge sealing strip of the present application can release flame retardant gas during combustion to form a protective layer, effectively slowing down the combustion speed and preventing the spread of flames. The synergistic effect of these two flame retardants significantly improves the flame retardant ability of the material, thereby providing higher safety.

[0022] 2. Good low temperature resistance Modified EPDM rubber is modified with methyl hydrogen silicone oil, which significantly improves the cold resistance of the material. This modification enables the sealing strip to maintain its physical properties at extremely low temperatures without hardening or embrittlement, ensuring its reliability and long-term effectiveness in cold environments.

[0023] 3. Good mechanical properties and service life The good compatibility of modified EPDM and EPDM, combined with the use of reinforcing agents, gives the sealing strip excellent mechanical properties. This composite material not only has high strength and good elasticity, but also can withstand long-term use and environmental impact, thus extending the service life of the product.

[0024] 4. Simple preparation process and large-scale production The sponge sealing strip of the present application has a simple preparation process, and the raw materials are easily available, which is suitable for large-scale production. This simple process reduces production costs and improves production efficiency, so that the sealing strip can be widely used in many fields such as construction, automobiles, and aerospace. DETAILED DESCRIPTION

[0025] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0026] In the following preparation examples and embodiments, 1 part means 0.1 kg.

[0027] Preparation Example 1 Preparation of modified EPDM rubber The preparation method of the modified EPDM rubber is as follows: according to the mass parts, 100 parts of EPDM rubber and 20 parts of methyl hydrogen silicone oil are dissolved in 200 parts of toluene, 0.5 parts of platinum catalyst are added, and the reaction is carried out at 160°C for 70 minutes, and the solvent is removed by reduced pressure distillation at 0.1MPa and 65°C for 70 minutes, and then vacuum drying is carried out at 60°C for 24 hours to obtain the modified EPDM rubber, wherein the ethylene mass content of the EPDM rubber is 48%, the mass content of the ENB third monomer is 5%, and the content of platinum, an effective substance, in the platinum catalyst is 6wt%.

[0028] Preparation Example 2 Preparation of graphene oxide modified melamine polyphosphate The preparation method of graphene oxide modified melamine polyphosphate comprises the following steps: S31, preparing an aqueous suspension by mixing 30 parts of hydrotalcite and 40 parts of water in parts by mass; S32, dispersing 250 parts of melamine polyphosphate and 10 parts of graphene oxide in a solution consisting of 10 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 30 parts of water according to mass fractions to obtain a mixed solution; S33, slowly adding the water suspension to the mixed solution, heating to 46°C, stirring at a rate of 500 rpm, reacting for 55 minutes, filtering, and vacuum drying at 80°C for 24 hours, grinding and sieving to obtain graphene oxide modified melamine polyphosphate with a particle size of 5-10 μm.

[0029] Preparation Example 3 Preparation of Silane Coupling Agent Modified Nano Antimony Trioxide The preparation method of silane coupling agent modified nano antimony trioxide is as follows: according to mass proportions, 10 parts of nano antimony trioxide with a particle size of 20 nm are dispersed in a solution consisting of 0.15 parts of γ-aminopropyltrimethoxysilane, 20 parts of ethanol and 3 parts of water to obtain a mixed solution; the heating temperature is 42°C, the stirring rate is 200 rpm, after reacting for 45 minutes, filtering, and vacuum drying at 82°C for 22 hours to obtain silane coupling agent modified nano antimony trioxide.

[0030] Example 1 A low-temperature resistant sponge sealing strip comprises the following raw materials in parts by mass: 20 parts of modified EPDM rubber, 60 parts of EPDM rubber, 4 parts of zinc oxide, 0.5 parts of stearic acid, 50 parts of reinforcing agent, 3 parts of composite flame retardant, 10 parts of plasticizer, 3 parts of antioxidant, 1.0 part of sulfur, and 1 part of accelerator ZDTP50, wherein the composite flame retardant is composed of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide in a mass ratio of 4:2, the reinforcing agent is composed of N550 carbon black, N330 carbon black and N762 carbon black in a mass ratio of 5:3:3, the plasticizer is EPDM rubber grafted maleic anhydride, wherein the mass content of maleic anhydride is 2%, and the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.

[0031] The method for preparing the above-mentioned low-temperature resistant sponge sealing strip comprises the following steps: S101, respectively adding modified EPDM rubber and EPDM rubber to a rubber mixing device according to their weight fractions and stirring them evenly, then adding zinc oxide, stearic acid, a reinforcing agent and a composite flame retardant for mixing, then adding a plasticizer, an antioxidant and an accelerator ZDTP50, mixing evenly and adding sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 170°C and the vulcanization pressure is 200kg / cm 2 The vulcanization time is 12 minutes, and finally it is extruded by an extruder to form a low-temperature resistant sponge sealing strip.

[0032] Example 2 A low-temperature resistant sponge sealing strip comprises the following raw materials in parts by mass: 25 parts of modified EPDM rubber, 65 parts of EPDM rubber, 5 parts of zinc oxide, 0.8 parts of stearic acid, 55 parts of reinforcing agent, 4 parts of composite flame retardant, 12 parts of plasticizer, 4 parts of antioxidant, 1.5 parts of sulfur, and 3 parts of accelerator CLD80, wherein the composite flame retardant is composed of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide in a mass ratio of 4:3, the reinforcing agent is composed of N550 carbon black, N330 carbon black and N762 carbon black in a mass ratio of 5:3:3, the plasticizer is EPDM rubber grafted maleic anhydride, wherein the mass content of maleic anhydride is 2%, and the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.

[0033] The method for preparing the above-mentioned low-temperature resistant sponge sealing strip comprises the following steps: S101, respectively adding modified EPDM rubber and EPDM rubber to a rubber mixing device according to their mass fractions and stirring them evenly, then adding zinc oxide, stearic acid, a reinforcing agent and a composite flame retardant for mixing, then adding a plasticizer, an antioxidant and an accelerator CLD80, mixing evenly and then adding sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 180°C and the vulcanization pressure is 180kg / cm 2 The vulcanization time is 8 minutes, and finally it is extruded by an extruder to form a low-temperature resistant sponge sealing strip.

[0034] Example 3 A low-temperature resistant sponge sealing strip comprises the following raw materials in parts by mass: 23 parts of modified EPDM rubber, 63 parts of EPDM rubber, 4.5 parts of zinc oxide, 0.7 parts of stearic acid, 54 parts of reinforcing agent, 3.5 parts of composite flame retardant, 11 parts of plasticizer, 3.5 parts of antioxidant, 1.2 parts of sulfur, and 2 parts of accelerator ZBEC7, wherein the composite flame retardant is composed of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide in a mass ratio of 4:2.5, the reinforcing agent is composed of N550 carbon black, N330 carbon black and N762 carbon black in a mass ratio of 5:3:3, the plasticizer is EPDM rubber grafted maleic anhydride, wherein the mass content of maleic anhydride is 2%, and the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.

[0035] The method for preparing the above-mentioned low-temperature resistant sponge sealing strip comprises the following steps: S101, respectively adding modified EPDM rubber and EPDM rubber to a rubber mixing device according to their mass fractions and stirring them evenly, then adding zinc oxide, stearic acid, a reinforcing agent and a composite flame retardant for mixing, then adding a plasticizer, an antioxidant and an accelerator ZBEC7, mixing evenly and adding sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 178°C and the vulcanization pressure is 190kg / cm 2 The vulcanization time is 11 minutes, and finally it is extruded by an extruder to form a low-temperature resistant sponge sealing strip.

[0036] Comparative Example 1 The same as Example 3, except that an equal amount of EPDM rubber is used instead of modified EPDM rubber.

[0037] Comparative Example 2 The same as Example 3, except that the composite flame retardant is graphene oxide modified melamine polyphosphate.

[0038] Comparative Example 3 The same as Example 3, except that the composite flame retardant is nano antimony trioxide modified by a silane coupling agent.

[0039] Comparative Example 4 The same as Example 3, except that an equal amount of melamine polyphosphate is used instead of the composite flame retardant.

[0040] Comparative Example 5 The same as Example 3, except that an equal amount of nano antimony trioxide with a particle size of 20 nm is used instead of the composite flame retardant.

[0041] Performance Testing The low temperature resistant sponge sealing strips prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were subjected to performance tests, and the results are shown in Table 1.

[0042] Tensile strength and elongation at break: refer to GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber to test tensile strength and elongation, and the tensile rate is 500mm / min; Flame retardant test: refer to the test method in ANSI / UL-94-1985, vertical burning test according to 94V-0, 94V-1, 94V-2, the test strip thickness is 1mm; Oxygen index: Test the oxygen index of materials according to GB / T 2406-1993; Brittleness temperature: Tested according to ASTM D-746 standard.

[0043] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The low temperature resistant sponge sealing strips prepared in Examples 1 to 3 have the advantages of good mechanical properties, long service life, good low temperature resistance and excellent flame retardant properties. The low temperature resistant sponge sealing strips of the present application have a simple preparation process and are easy to prepare on a large scale.

[0044] 2) The performance comparison analysis of the low-temperature resistant sponge sealing strips prepared in combination with Example 3 and Comparative Example 1 shows that the modified EPDM rubber significantly improves its cold resistance by modification with methyl hydrogen silicone oil. This is because methyl hydrogen silicone oil itself has excellent low-temperature resistance, and the silicon-oxygen bonds in its structure provide the material with good flexibility and cold resistance. The modified EPDM rubber has good compatibility with the unmodified EPDM rubber, which helps to maintain the uniformity and overall mechanical properties of the material. At the same time, the addition of methyl hydrogen silicone oil may also improve the flexibility and ductility of the material, thereby extending the service life of the sealing strip. The excellent cold resistance of the modified EPDM rubber is combined with the flame retardant properties of other components such as the composite flame retardant, so that the final low-temperature resistant sponge sealing strip can still maintain good performance in an extremely low temperature environment, while having excellent flame retardant properties. The modified EPDM rubber achieves a multi-faceted improvement in product performance by improving cold resistance, maintaining mechanical properties and compatibility, and achieving synergistic effects with other components.

[0045] 3) The performance comparison analysis of the low temperature resistant sponge sealing strip prepared in combination with Example 3 and Comparative Examples 2-3 shows that the composite flame retardant is composed of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide in a mass ratio of 4:2.5. The adjustment of this ratio is to maximize their respective performance advantages and achieve synergistic effects, thereby significantly improving the flame retardant effect of the low temperature resistant sponge sealing strip. During the combustion process of graphene oxide modified melamine polyphosphate, the modified melamine polyphosphate can release flame retardant gases such as phosphoric acid, which can form a protective layer, effectively slow down the combustion speed, and prevent the spread of flames. Through the modification of γ-aminopropyltrimethoxysilane and graphene oxide, the compatibility of melamine polyphosphate with EPDM rubber is improved, which is conducive to improving its dispersibility in the sealing strip, thereby improving the uniformity and overall performance of the material. As a synergistic flame retardant, the good compatibility of nano antimony trioxide modified by silane coupling agent with EPDM rubber helps to improve its dispersibility in the sealing strip, thereby improving the flame retardant performance. Nano antimony trioxide can form a stable protective layer when burning, and work together with the flame-flammable gas released by graphene oxide modified melamine polyphosphate to form a more effective barrier layer, further preventing oxygen from reaching the combustion area and delaying the combustion of the material. The synergistic effect of these two flame retardants not only improves the flame retardant effect, but also improves production efficiency and product performance consistency due to better dispersibility and compatibility. Through their synergistic effect, graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide not only significantly improve the flame retardant effect of low-temperature resistant sponge sealing strips, but also enhance the overall performance of the material by improving dispersibility and compatibility.

[0046] 4) The performance comparison analysis of the low-temperature resistant sponge sealing strips prepared in combination with Example 3 and Comparative Example 4 shows that the modified melamine polyphosphate can release flame-retardant gases such as phosphoric acid during combustion to form a protective layer, effectively slowing down the combustion rate and preventing the spread of flames. Through the modification of γ-aminopropyltrimethoxysilane, the compatibility of melamine polyphosphate with EPDM rubber is improved, which is conducive to improving its dispersibility in the sealing strip, thereby improving the uniformity and overall performance of the material. The addition of graphene oxide not only improves the flame retardant efficiency of melamine polyphosphate, but also may enhance the mechanical properties of the sealing strip through its excellent physical properties and extend the service life. In summary, the modified melamine polyphosphate achieves a multi-faceted improvement in product performance by improving flame retardancy, enhancing compatibility and dispersibility, and utilizing the physical properties of graphene oxide.

[0047] 5) The performance comparison analysis of the low-temperature resistant sponge sealing strips prepared in combination with Example 3 and Comparative Example 5 shows that the modified nano antimony trioxide prepared by the present application can form a stable protective layer during the combustion process, and work together with the flame-retardant gas released by the graphene oxide modified melamine polyphosphate to form a more effective barrier layer, further preventing oxygen from reaching the combustion area and delaying the combustion of the material. Through the modification of the silane coupling agent, the compatibility of nano antimony trioxide with EPDM rubber is improved, which is conducive to improving its dispersibility in the sealing strip, thereby improving the uniformity and overall performance of the material.

[0048] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A low temperature resistant sponge sealing strip, characterized in that: The invention comprises the following raw materials in parts by weight: 20-25 parts of modified EPDM rubber, 60-65 parts of EPDM rubber, 4-5 parts of zinc oxide, 0.5-0.8 parts of stearic acid, 50-55 parts of reinforcing agent, 3-4 parts of composite flame retardant, 10-12 parts of plasticizer, 3-4 parts of antioxidant, 1.0-1.5 parts of sulfur and 1-3 parts of accelerator, wherein the composite flame retardant is composed of graphene oxide modified melamine polyphosphate and silane coupling agent modified nano antimony trioxide.

2. The low temperature resistant sponge sealing strip according to claim 1, characterized in that: The mass ratio of the graphene oxide modified melamine polyphosphate to the silane coupling agent modified nano antimony trioxide is 4:2-3.

3. The low temperature resistant sponge sealing strip according to claim 1, characterized in that: The preparation method of the graphene oxide modified melamine polyphosphate comprises the following steps: S31, preparing an aqueous suspension by mixing 30 parts of hydrotalcite and 40 parts of water in parts by mass; S32, dispersing 250 parts of melamine polyphosphate and 10 parts of graphene oxide in a solution consisting of 10 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 30 parts of water according to mass fractions to obtain a mixed solution; S33, slowly adding the water suspension to the mixed solution, heating to 46°C, stirring at a rate of 500 rpm, reacting for 50-60 minutes, filtering, and vacuum drying at 80°C for 24 hours, grinding and sieving to obtain graphene oxide modified melamine polyphosphate with a particle size of 5-10 μm.

4. The low temperature resistant sponge sealing strip according to claim 1, characterized in that: The preparation method of the silane coupling agent modified nano antimony trioxide is as follows: according to mass fractions, 10 parts of nano antimony trioxide with a particle size of 20 nm are dispersed in a solution consisting of 0.15 parts of γ-aminopropyltrimethoxysilane, 20 parts of ethanol and 3 parts of water to obtain a mixed solution; heating the mixture to 42° C., stirring at a rate of 200 rpm, reacting for 40-50 minutes, filtering, and vacuum drying at 82° C. for 20-24 hours to obtain the silane coupling agent modified nano antimony trioxide.

5. The low temperature resistant sponge sealing strip according to claim 1, characterized in that: The preparation method of the modified EPDM rubber is as follows: according to the mass fractions, 100 parts of EPDM rubber and 20 parts of methyl hydrogen silicone oil are dissolved in 200 parts of toluene, 0.5 parts of platinum catalyst are added, reacted at 160° C. for 70 minutes, and then the solvent is removed by reduced pressure distillation at 0.1 MPa and 65° C. for 70 minutes, and then vacuum dried at 60° C. for 24 hours to obtain the modified EPDM rubber.

6. A low temperature resistant sponge sealing strip according to claim 5, characterized in that: The ethylene content of the EPDM rubber is 48% by weight, the third monomer content of ENB is 5% by weight, and the effective substance platinum content of the platinum catalyst is 6wt%.

7. The low temperature resistant sponge sealing strip according to claim 1, characterized in that: The reinforcing agent is composed of N550 carbon black, N330 carbon black and N762 carbon black in a mass ratio of 5:3:

3.

8. The low temperature resistant sponge sealing strip according to claim 1, characterized in that: The plasticizer is EPDM rubber grafted with maleic anhydride, wherein the mass content of maleic anhydride is 2%.

9. The low temperature resistant sponge sealing strip according to claim 1, characterized in that: The accelerator is at least one of accelerator ZDTP50, accelerator CLD80 and accelerator ZBEC7; the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:

2.

10. A method for preparing a low-temperature resistant sponge sealing strip according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101, respectively adding modified EPDM rubber and EPDM rubber to a rubber mixing device according to their weight fractions and stirring them evenly, then adding zinc oxide, stearic acid, a reinforcing agent and a composite flame retardant for mixing, then adding a plasticizer, an antioxidant and an accelerator, mixing evenly and adding sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 170-180°C and the vulcanization pressure is 180-200kg / cm 2 The vulcanization time is 8-12 minutes, and finally it is extruded by an extruder to form a low-temperature resistant sponge sealing strip.