Carbon aerogel as well as preparation method and application thereof

By using formaldehyde and resorcinol as precursors, combining specific catalysts and oxidative pore-forming agents, the problem that carbon aerogels in the prior art are difficult to have both low density and high specific surface area, and high specific surface area is achieved and low-density carbon aerogel preparation, suitable for thermal insulation, catalytic, adsorption and electrode materials.

CN118929619APending Publication Date: 2024-11-12IBIH ADVANCED MATERIALS CO LTD

Patent Information

Application Number
CN202310529955.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult to obtain carbon aerogels with both low density and high specific surface area in the prior art, especially the vacancy left during drying, resulting in relatively small specific surface area.

Method used

By using formaldehyde and resorcinol as precursors, combined with specific catalysts and oxidative pore-forming agents, pre-reduction is carried out to form a micro-crystalline dispersion. The subsequent hydrogel is replaced by solvent and supercritical drying, and is further annealed and carbonized to form a combination of both Carbon aerogel with low density and high specific surface area.

Benefits of technology

It achieves both low density and high specific surface area of ​​carbon aerogel, can absorb organic oil far exceed its own mass, and has high mechanical strength and porosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929619A_ABST
    Figure CN118929619A_ABST
Patent Text Reader

Abstract

The invention relates to the field of aerogel preparation, and discloses carbon aerogel as well as a preparation method and application thereof. The preparation method comprises the following steps: heating a mixed solution containing formaldehyde, resorcinol, a catalyst and an oxidation pore-forming agent for pre-reduction to obtain a micro-minced dispersion liquid with the viscosity of 300-520Pa. S at 25 DEG C; wherein the catalyst is one or more of sodium carbonate, hydrazine hydrate, sodium bicarbonate and sodium borohydride; the oxidation pore-forming agent is one or more of polyethylene glycol, polyvinyl alcohol, ammonium bicarbonate and formamide; the micro-minced dispersion liquid is heated for reduction, and hydrogel is obtained; carrying out solvent replacement on the obtained hydrogel, and then carrying out supercritical drying on the obtained product to obtain aerogel; wherein a solvent used for solvent replacement is an organic solvent; and carrying out annealing carbonization on the aerogel to obtain the carbon aerogel. The carbon aerogel provided by the invention has low density and high specific surface area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aerogel preparation, and in particular to carbon aerogel and a preparation method and application thereof. Background Art

[0002] Aerogel is a material with a three-dimensional porous structure formed by dispersing air in a solid medium. Carbon aerogel is a three-dimensional material obtained by using a carbon reagent as a precursor. Carbon aerogel has the characteristics of both aerogel and carbon materials, that is, it has good conductivity while maintaining low density and high specific surface area.

[0003] By using hydrophilic carbon source chemicals as precursors, the sol-gel method is used to self-assemble them into three-dimensional hydrogels. The aerogels obtained after subsequent treatment with special drying methods have a huge specific surface area and low density due to their complex internal pore structure, and can absorb organic oils far exceeding their own mass. Aerogels are mostly made using organic matter or ice as templates. Compared with organic matter as templates, the raw material ice of the ice template method is cheap, but ice crystals grow into nuclei and dry, leaving large vacancies, which makes it have a lower specific surface area, making it difficult to obtain low-density, high-specific surface area carbon aerogels.

[0004] CN109850870A discloses a high-strength carbon aerogel and its preparation method and application, which uses industrial phenolic resin as raw material, hexamethylenetetramine as curing agent, ethylene glycol and water as solvent, and performs sol-gel reaction at a certain temperature after mixing, obtains phenolic aerogel after normal pressure drying, and carbonizes at high temperature to obtain carbon aerogel. Although the microstructure of the carbon aerogel is a three-dimensional network structure in which particles are interconnected, since the phenolic resin itself has a high molecular weight, the cross-linked phenolic aerogel has a small specific surface area, which in turn leads to a small specific surface area of ​​the carbon aerogel.

[0005] CN102092708A discloses a method for preparing phenol-formaldehyde carbon aerogel under low alkali conditions, wherein phenol and formaldehyde are used as reaction monomers, resorcinol is used as a co-monomer and nucleating agent, a strong base is used as a catalyst, and water is used as a solvent. The gel is heated at 70°C to 100°C and then aged to obtain an organic wet gel; the organic wet gel is replaced with an organic solvent so that the organic solvent fills the gel; the replaced organic wet gel is supercritically dried to obtain an organic aerogel; and the organic aerogel is carbonized in an inert atmosphere to obtain the desired carbon aerogel. The carbon aerogel contains a large number of mesopores, micropores, and some macropores, and the BET specific surface area is 680m 2 / g, pore volume is 1.042cm 3 g -1 , and the raw material cost is low, and the gel can be obtained by reaction under low base catalytic concentration, but it only retains the specific surface area of ​​the carbon aerogel itself, and the specific surface area is still small. Summary of the invention

[0006] The purpose of the present invention is to overcome the problem that it is difficult to obtain carbon aerogels with low density and high specific surface area in the prior art.

[0007] In order to achieve the above object, the present invention provides a method for preparing carbon aerogel in a first aspect, the preparation method comprising:

[0008] (1) heating a mixed solution containing formaldehyde, resorcinol, a catalyst and an oxidative pore-forming agent for pre-reduction to obtain a micro-crushed dispersion; wherein:

[0009] The viscosity of the micro-crushed dispersion at 25°C is 300-520 Pa·s;

[0010] The catalyst is selected from one or more of sodium carbonate, hydrazine hydrate, sodium bicarbonate and sodium borohydride;

[0011] The oxidative pore-forming agent is selected from one or more of polyethylene glycol, polyvinyl alcohol, ammonium bicarbonate and formamide;

[0012] (2) heating the micro-dispersion liquid to reduce the micro-dispersion liquid to obtain a hydrogel;

[0013] (3) subjecting the hydrogel to solvent replacement, and then subjecting the obtained product to supercritical drying to obtain an aerogel; wherein the solvent used in the solvent replacement is an organic solvent;

[0014] (4) Annealing and carbonizing the aerogel to obtain carbon aerogel.

[0015] The second aspect of the present invention provides a carbon aerogel prepared by the preparation method described in the first aspect, wherein the density of the carbon aerogel is 0.01-0.05 g / cm 3 ; BET specific surface area is 900-1500m 2 / g.

[0016] The third aspect of the present invention provides the use of the carbon aerogel as described in the second aspect in one or more of thermal insulation materials, catalytic materials, adsorption materials and electrode materials.

[0017] Through the above technical scheme, the preparation method provided by the present invention uses formaldehyde and resorcinol as precursors, and combines the use of a specific catalyst and a specific oxidation pore-forming agent, preferably, the use of an activator, and pre-reduces by heating a mixed solution containing the above substances to accelerate the aldol condensation, and pre-reduces at a certain time to form a micro-mash-like dispersion (phenolic sol) with a specific viscosity. During the pre-reduction process, the hydroxyl group and the aldehyde group condense under the initiation of the catalyst, and the obtained phenolic sol is further heated for reduction, gradually forming a precursor hydrogel of a body structure, and the oxidation pore-forming agent is retained. The subsequent hydrogel is subjected to solvent replacement and supercritical fluid drying treatment to remove the solvent in the hydrogel, and further annealing and carbonization treatment decomposes the oxidation pore-forming agent in the aerogel to form vacancies, and finally a carbon aerogel with both low density and high specific surface area can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a macroscopic appearance diagram of the carbon aerogel prepared in Example 1 of the present invention;

[0019] Figure 2 is a schematic diagram of the oil absorption performance of the carbon aerogel prepared in Example 1 of the present invention;

[0020] Figure 3 is a schematic diagram of the weight of the carbon aerogel prepared in Example 1 of the present invention;

[0021] Figure 4 is a schematic diagram of the mechanical properties of the carbon aerogel prepared in Example 1 of the present invention;

[0022] Figure 5 yes Figure 4 Schematic diagram of the weight of the heavy object on the carbon aerogel. DETAILED DESCRIPTION

[0023] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0024] As mentioned above, the first aspect of the present invention provides a method for preparing carbon aerogel, the preparation method comprising:

[0025] (1) heating a mixed solution containing formaldehyde, resorcinol, a catalyst and an oxidative pore-forming agent for pre-reduction to obtain a micro-crushed dispersion; wherein:

[0026] The viscosity of the micro-crushed dispersion at 25°C is 300-520 Pa·s;

[0027] The catalyst is selected from one or more of sodium carbonate, hydrazine hydrate, sodium bicarbonate and sodium borohydride;

[0028] The oxidative pore-forming agent is selected from one or more of polyethylene glycol, polyvinyl alcohol, ammonium bicarbonate and formamide;

[0029] (2) heating the micro-dispersion liquid to reduce the micro-dispersion liquid to obtain a hydrogel;

[0030] (3) subjecting the hydrogel to solvent replacement, and then subjecting the obtained product to supercritical drying to obtain an aerogel; wherein the solvent used in the solvent replacement is an organic solvent;

[0031] (4) Annealing and carbonizing the aerogel to obtain carbon aerogel.

[0032] Although the existing carbon aerogel has a high density, the vacancies left in the drying process are large, so that its specific surface area is relatively small, and it is difficult to have both low density and high specific surface area. The inventors of the present invention have found in the research process that by using formaldehyde and resorcinol as precursors, and combining the use of specific catalysts and specific oxidative pore-forming agents, preferably, there is also the use of activators, by heating the mixed solution containing the above substances for pre-reduction, accelerating the aldol condensation, and pre-reducing in a certain time to form a micro-mash-like dispersion (phenolic sol) with a specific viscosity. During the pre-reduction process, the hydroxyl group and the aldehyde group condense under the initiation of the catalyst, and the obtained phenolic sol continues to be heated for reduction, gradually forming a precursor hydrogel of a body structure, and the oxidative pore-forming agent is retained. The subsequent hydrogel is subjected to solvent replacement and supercritical fluid drying to remove the solvent in the hydrogel, and further annealing and carbonization treatment decomposes the oxidative pore-forming agent in the aerogel to form vacancies, and finally a carbon aerogel with both low density and high specific surface area can be obtained.

[0033] According to some embodiments of the present invention, in step (1), the mixed solution containing formaldehyde, resorcinol, a catalyst and an oxidative pore-forming agent is heated for pre-reduction to obtain a micro-crushed dispersion; wherein the viscosity of the micro-crushed dispersion at 25° C. is 300-520 Pa·s. In the above process, resorcinol reacts with the formaldehyde under the action of the catalyst to form resorcinol-formaldehyde colloidal clusters, i.e., micro-crushed prepolymers.

[0034] According to some embodiments of the present invention, preferably, in step (1), the formaldehyde is provided in the form of a formaldehyde dispersion; the mass fraction of the formaldehyde dispersion may be 20-40%.

[0035] According to some embodiments of the present invention, in step (1), there is no particular limitation on the method for preparing the mixed solution, as long as a mixed solution containing formaldehyde, resorcinol, a catalyst and an oxidative pore-forming agent can be obtained, the purpose of the present invention can be achieved to a certain extent. Preferably, the step of preparing the mixed solution comprises: adding resorcinol, a catalyst, an activator and an oxidative pore-forming agent to a formaldehyde dispersion, and performing dispersion mixing; preferably, the temperature of the dispersion mixing is 15-30°C.

[0036] According to some embodiments of the present invention, preferably, in step (1), the weight ratio of the formaldehyde to the resorcinol is 2-10: 1. The above preferred embodiment is conducive to further promoting the reaction between formaldehyde and resorcinol, and is more conducive to obtaining a micro-crushed dispersion with a viscosity that meets the above requirements.

[0037] According to some embodiments of the present invention, preferably, in step (1), the catalyst is sodium carbonate.

[0038] According to some embodiments of the present invention, preferably, in step (1), the weight ratio of the catalyst to the resorcinol is 0.02-0.2: 1. The above preferred embodiment is beneficial to further promote the reaction between formaldehyde and resorcinol.

[0039] According to some embodiments of the present invention, in step (1), the oxidative pore former is selected from one or more of polyethylene glycol, polyvinyl alcohol, ammonium bicarbonate and formamide. In the oxidative pore former, the polymer with hydroxyl groups will be well mixed and combined with the system through hydrogen bonds due to the presence of hydroxyl groups, and will occupy certain vacancies during the reaction. At the same time, through subsequent annealing and carbonization, the oxidative pore former can be etched and burned, leaving vacancies; small molecule inorganic compounds with high temperature decomposition gas properties will decompose and produce gas after the reaction process reaches a certain temperature, and will also produce certain vacancies, increasing the specific surface area of ​​the gel, and subsequently through supercritical fluid treatment, ignoring the surface tension capillary effect during the liquid volatilization process, the vacancies are retained. The above-mentioned specific oxidative pore former is conducive to obtaining carbon aerogels with both low density and high specific surface area.

[0040] According to some embodiments of the present invention, preferably, in step (1), the oxidative pore-forming agent is polyvinyl alcohol and / or ammonium bicarbonate, preferably a combination of polyvinyl alcohol and ammonium bicarbonate, and more preferably, in the combination, the weight ratio of polyvinyl alcohol to ammonium bicarbonate is 0.2-2: 1. The use of the above preferred embodiment is conducive to further reducing the density of the carbon aerogel and increasing the specific surface area of ​​the carbon aerogel.

[0041] According to some embodiments of the present invention, preferably, in step (1), the weight ratio of the oxidative pore former to the resorcinol is 0.02-0.2: 1. The above preferred embodiment is conducive to further reducing the density of the carbon aerogel and increasing the specific surface area of ​​the carbon aerogel.

[0042] According to some embodiments of the present invention, preferably, in step (1), the mixed solution further contains an activator, and the activator is selected from one or more of zinc oxide, ferrous chloride and calcium oxide, preferably zinc oxide. The above preferred embodiment is conducive to further reducing the density of the carbon aerogel and increasing the specific surface area of ​​the carbon aerogel.

[0043] According to some embodiments of the present invention, preferably, in step (1), the weight ratio of the activator to the resorcinol is 0.01-0.02:1.

[0044] According to some embodiments of the present invention, preferably, in step (1), the pre-reduction conditions include: temperature of 25-45° C., and time of 20-50 min.

[0045] According to some embodiments of the present invention, in step (2), the micro-crushed dispersion is heated for reduction to obtain a hydrogel. In the above process, the micro-crushed prepolymer (mainly resorcinol-formaldehyde colloid clusters) is further heated for reduction, and the surface hydroxymethyl groups in the clusters are cross-linked to form a macroscopic bulk hydrogel with a stable structure.

[0046] According to some embodiments of the present invention, preferably, in step (2), the reduction conditions include: temperature of 30-65° C. and time of 10-100 h.

[0047] According to some embodiments of the present invention, in step (3), the hydrogel is subjected to solvent replacement, and the obtained product is then subjected to supercritical drying to obtain an aerogel. Wherein, the solvent used in the solvent replacement is an organic solvent. In the above process, since the surface tension of water is large and extraction is relatively difficult, the water in the phenolic hydrogel is first replaced with an organic solvent, and it is ensured that the phenolic hydrogel becomes a phenolic organic solvent gel (such as a phenolic alcohol gel), and the phenolic organic solvent gel is subsequently extracted by supercritical drying, until the organic solvent in the gel is extracted by carbon dioxide, and supercritical carbon dioxide occupies the liquid vacancy in the gel, so that the supercritical carbon dioxide does not undergo liquid-gas conversion, but directly becomes a gaseous state from a supercritical state, and finally retains the mesopores and pores in the phenolic aerogel.

[0048] According to some embodiments of the present invention, preferably, in step (3), the organic solvent is one or more of methanol, ethanol and glycerol. Preferably, the number of times of solvent replacement is 1-5 times.

[0049] According to some embodiments of the present invention, preferably, in step (3), the supercritical drying is supercritical carbon dioxide drying; the conditions of the supercritical drying include: a pressure of 15-30 MPa and a temperature of 50-70°C.

[0050] According to some embodiments of the present invention, in step (4), the aerogel is annealed and carbonized to obtain a carbon aerogel.

[0051] According to some embodiments of the present invention, preferably, in step (4), the annealing and carbonization conditions include: a temperature of 1100-1300° C. and a time of 3-7 hours.

[0052] According to some embodiments of the present invention, preferably, in step (4), the annealing and carbonization is performed under the protection of an inert gas. Preferably, the inert gas is at least one of nitrogen, argon, neon and helium.

[0053] The second aspect of the present invention provides a carbon aerogel prepared by the preparation method described in the first aspect, wherein the density of the carbon aerogel is 0.01-0.05 g / cm 3 , preferably 0.01-0.025 g / cm 3 ; BET specific surface area is 900-1500m 2 / g, preferably 1300-1450m 2 / g, which can have both low density and high specific surface area.

[0054] According to some embodiments of the present invention, preferably, the porosity of the carbon aerogel is 85-95%, preferably 90%-95%.

[0055] According to some embodiments of the present invention, preferably, the proportion of the mesopore volume of the carbon aerogel to the total pore volume is 35%-40%; the proportion of the small pore volume to the total pore volume is 40%-60%.

[0056] Preferably, the carbon aerogel having the above-mentioned specific pore structure has a lower density and a higher specific surface area.

[0057] According to some embodiments of the present invention, the carbon aerogel can bear a weight several hundred times its own mass and has high mechanical strength.

[0058] The third aspect of the present invention provides the use of the carbon aerogel as described in the second aspect in one or more of thermal insulation materials, catalytic materials, adsorption materials and electrode materials.

[0059] The present invention will be described in detail below through examples.

[0060] In the following examples and comparative examples, unless otherwise specified, the raw materials used are commercially available.

[0061] In the following examples and comparative examples, the relevant parameters were measured by the following methods:

[0062] The viscosity of the micro-dispersion was measured by a viscometer at a test temperature of 25°C;

[0063] The density of carbon aerogel was obtained by the weight volume density method;

[0064] The pore structure properties of carbon aerogel were measured by the BET test method. Specifically, the Quantachrome AS-6B analyzer was used for measurement, the specific surface area was obtained by the Brunauer-Emmett-Taller (BET) method, and the pore distribution curve was calculated by the Barrett-Joyner-Halenda (BJH) method for the desorption curve.

[0065] The following examples are used to illustrate the carbon aerogel and the preparation method thereof provided by the present invention.

[0066] Example 1

[0067] (1) heating a mixed solution containing formaldehyde, 10 g of resorcinol, an activator, a catalyst and an oxidative pore-forming agent for pre-reduction to obtain a micro-crushed dispersion; wherein:

[0068] The viscosity of the micro-dispersion at 25°C is 400 Pa·s;

[0069] The catalyst is sodium carbonate; the oxidation pore-forming agent is a combination of polyvinyl alcohol and ammonium bicarbonate, and the weight ratio of polyvinyl alcohol to ammonium bicarbonate is 1:1; the activator is zinc oxide;

[0070] The weight ratio of formaldehyde to resorcinol is 2.5:1; the weight ratio of catalyst to resorcinol is 0.05:1; the weight ratio of oxidation pore former to resorcinol is 0.2:1; the weight ratio of activator to resorcinol is 0.01:1;

[0071] The preparation steps of the mixed solution are as follows: adding resorcinol, a catalyst, an activator and an oxidation pore-forming agent into 100 mL of a formaldehyde dispersion having a mass fraction of 25%, and performing dispersion mixing at a dispersion mixing temperature of 25° C.; the pre-reduction conditions are as follows: a temperature of 45° C. and a time of 30 minutes;

[0072] (2) heating the micro-dispersion liquid for reduction to obtain a hydrogel; wherein:

[0073] The reduction conditions were: temperature 65°C, time 100 h;

[0074] (3) subjecting the hydrogel to solvent replacement, and then subjecting the obtained product to supercritical drying to obtain an aerogel; wherein:

[0075] The solvent used for solvent replacement was ethanol, and the number of solvent replacements was 3 times;

[0076] Supercritical drying is supercritical carbon dioxide drying, and the conditions of supercritical drying are: pressure 15MPa, temperature 70℃;

[0077] (4) annealing and carbonizing the aerogel to obtain a carbon aerogel; wherein:

[0078] The annealing and carbonization conditions are: temperature of 1200° C. and time of 5 hours; the annealing and carbonization is carried out under the protection of nitrogen.

[0079] Example 2

[0080] The method of Example 1 is different from that of Example 1:

[0081] In step (1), the oxidative pore-forming agent is polyethylene glycol;

[0082] In step (2), the reduction conditions are: temperature is 30°C and time is 10h;

[0083] The rest of the process was the same, and carbon aerogel was obtained.

[0084] Example 3

[0085] The method of Example 1 is followed, except that in step (1), the catalyst is hydrazine hydrate, and the rest is the same, to obtain a carbon aerogel.

[0086] Example 4

[0087] The method of Example 1 is followed, except that in step (1), the mixed solution does not contain an activator, and the rest is the same to obtain a carbon aerogel.

[0088] Comparative Example 1

[0089] The method of Example 1 is followed, except that in step (1), the mixed solution does not contain an oxidative pore-forming agent, and the rest is the same to obtain a carbon aerogel.

[0090] The present invention exemplarily provides a macroscopic appearance of the carbon aerogel prepared in Example 1 (see Figure 1 ), schematic diagram of the oil absorption performance of the carbon aerogel (see Figure 2 ), a schematic diagram of the weight of the carbon aerogel (see Figure 3 ), schematic diagram of the mechanical properties of the carbon aerogel (see Figure 4 ), and a schematic diagram of the weight of the weight pressed on the carbon aerogel (see Figure 5 ).in:

[0091] from Figure 2 It can be seen that the carbon aerogel has high oil absorption performance and good affinity to oil;

[0092] from Figure 3-5 It can be seen that the carbon aerogel can withstand a weight hundreds of times its own mass and has high mechanical strength.

[0093] Test Case

[0094] The relevant characteristic parameters of the carbon aerogels prepared in the embodiment and the comparative example were tested respectively, including density, BET specific surface area and porosity. The results are shown in Table 1.

[0095] Table 1

[0096]

[0097]

[0098] It can be seen from the above results that the carbon aerogel provided by the present invention can have both low density and high specific surface area.

[0099] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing carbon aerogel, characterized in that: The preparation method comprises: (1) heating a mixed solution containing formaldehyde, resorcinol, a catalyst and an oxidative pore-forming agent for pre-reduction to obtain a micro-crushed dispersion; wherein: The viscosity of the micro-crushed dispersion at 25°C is 300-520 Pa·s; The catalyst is selected from one or more of sodium carbonate, hydrazine hydrate, sodium bicarbonate and sodium borohydride; The oxidative pore-forming agent is selected from one or more of polyethylene glycol, polyvinyl alcohol, ammonium bicarbonate and formamide; (2) heating the micro-dispersion liquid to reduce the micro-dispersion liquid to obtain a hydrogel; (3) subjecting the hydrogel to solvent replacement, and then subjecting the obtained product to supercritical drying to obtain an aerogel; wherein the solvent used in the solvent replacement is an organic solvent; (4) Annealing and carbonizing the aerogel to obtain carbon aerogel.

2. The preparation method according to claim 1, wherein In step (1), the weight ratio of the formaldehyde to the resorcinol is 2-10:

1.

3. The preparation method according to claim 1, wherein In step (1), the catalyst is sodium carbonate; And / or, the weight ratio of the catalyst to the resorcinol is 0.02-0.2:

1.

4. The preparation method according to any one of claims 1 to 3, wherein In step (1), the oxidative pore-forming agent is polyvinyl alcohol and / or ammonium bicarbonate, preferably a combination of polyvinyl alcohol and ammonium bicarbonate, and more preferably, in the combination, the weight ratio of polyvinyl alcohol to ammonium bicarbonate is 0.2-2:1; And / or, the weight ratio of the oxidative pore-forming agent to the resorcinol is 0.02-0.2:

1.

5. The preparation method according to any one of claims 1 to 3, wherein: In step (1), the mixed solution further contains an activator, which is selected from one or more of zinc oxide, ferrous chloride and calcium oxide, preferably zinc oxide; And / or, the weight ratio of the activator to the resorcinol is 0.01-0.02:

1.

6. The preparation method according to any one of claims 1 to 3, wherein: In step (1), the pre-reduction conditions include: temperature of 25-45°C and time of 20-50 min; And / or, in step (2), the reduction conditions include: temperature of 30-65° C. and time of 10-100 h.

7. The preparation method according to any one of claims 1 to 3, wherein: In step (3), the organic solvent is one or more of methanol, ethanol and glycerol; Preferably, in step (3), the supercritical drying is supercritical carbon dioxide drying; the conditions of the supercritical drying include: a pressure of 15-30 MPa and a temperature of 50-70°C.

8. The preparation method according to any one of claims 1 to 3, wherein: In step (4), the annealing and carbonization conditions include: a temperature of 1100-1300° C. and a time of 3-7 hours; And / or, in step (4), the annealing and carbonization is carried out under the protection of an inert gas.

9. A carbon aerogel prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The density of the carbon aerogel is 0.01-0.05 g / cm 3 , preferably 0.01-0.025 g / cm 3 ; BET specific surface area is 900-1500m 2 / g, preferably 1300-1450m 2 / g; Preferably, the carbon aerogel has a porosity of 85-95%, preferably 90%-95%.

10. Use of the carbon aerogel according to claim 9 in one or more of thermal insulation materials, catalytic materials, adsorption materials and electrode materials.

Citation Information

Patent Citations

  • Preparation method of polyethylene glycol modified carbon aerogel / fiber composite material

    CN113526974A

  • Phenolic resin-based carbon aerogel and preparation method thereof

    CN114715878A

  • Porous carbon material as well as preparation method and application thereof

    CN115872403A

  • Carbon aerogels, process for their preparation and their use

    SG163143A1

Cited By

  • Preparation method of aerogel spherical porous carbon, preparation method of aerogel spherical silicon carbon negative electrode material and battery

    CN119735206A