Preparation method of hollow silicon dioxide microspheres

The preparation of hollow silica microspheres by core-shell polymer emulsion method was solved, and the problems of spherical structure incomplete and insufficient dispersion caused by high-temperature calcination and solvent etching in the prior art were solved, thereby achieving a complete and monodispersible hollow Silica microsphere preparation, suitable for catalysis and controlled drug release fields.

CN118929676APending Publication Date: 2024-11-12DONGGUAN CSG SOLAR GLASS +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410932400.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing preparation methods for hollow silica microspheres require cumbersome and energy-consuming processes such as high-temperature calcination or solvent etching, resulting in incomplete spherical structure and insufficient dispersion, limiting their application in the fields of catalysis and controlled drug release.

Method used

The core-shell polymer emulsion method is used to form a seed emulsion by dropping acrylic monomers and acrylate monomers, wrapping the hard organic shell layer, adding ammonia water or ammonia organic alkali for neutralization, forming hollow polymer microspheres , and deposit a silica shell on its surface to avoid high temperature treatment.

Benefits of technology

The preparation of complete and monodispersible hollow silica microspheres is achieved, avoiding the adverse effects of high-temperature calcination and solvent etching, and improving the integrity and dispersion of the spherical structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929676A_ABST
    Figure CN118929676A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of hollow silicon dioxide microspheres. The problems that in the prior art, high-temperature calcination or solvent etching, repeated centrifugal washing and other tedious and energy-consuming processes for removing an internal template are needed for preparing the hollow silicon dioxide microspheres are solved, and adverse effects on the hollow microspheres caused by various possibly-adopted post-treatment means are avoided; in order to solve the problems of insufficient integrity of a hollow spherical structure and insufficient monodispersity of the sphere, the invention synthesizes the complete and monodisperse hollow silicon dioxide microsphere.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and particularly relates to a method for preparing hollow silica microspheres. Background Art

[0002] Nano hollow silica microspheres often exhibit many physical and chemical properties different from solid particles, such as good electrical, magnetic, permeability, mechanical properties, optical properties, etc. They have broad market application prospects in many important fields such as sustained-release capsules, lightweight fillers, selective adsorption, anti-reflection, thermal insulation, active substance encapsulation, catalysis, insulation, etc.

[0003] The hard template method is the most typical and widely used method for preparing hollow spheres. The hard template method generally uses polymer microspheres as templates to deposit and grow silica precursors on the polymer surface, and finally obtains silica composite core-shell microspheres. After the reaction is completed, it is necessary to undergo high-temperature calcination or solvent etching to obtain hollow silica microspheres; this preparation method is costly and brings environmental problems. Removing the core template by high-temperature calcination and chemical etching will also destroy the silica shell. The soft template method usually uses microemulsion droplets as templates, and a large amount of surfactants need to be introduced. The silicon source undergoes hydrolysis, polymerization, sol-gel and other chemical reactions at the interface of the two phases to form a film, and finally separated and dried to obtain porous silica microspheres, but in the end, it is necessary to remove both the soft template and all surfactant molecules in the system. Both methods have problems such as complex preparation process, poor dispersibility and structural integrity, which not only increase the production cost but also affect their application to a certain extent. CN101857234A discloses a monodisperse mesoporous hollow silica nanosphere and a preparation method thereof, wherein, under ultrasonic radiation, an inorganic sodium salt or potassium salt is used as a hydrolysis aid, and Tween is used as a dispersant, to prepare hollow silica nanospheres containing an n-octylamine template in the inner layer, and then the hollow silica nanospheres are placed in a muffle furnace for calcination to remove the organic template and prepare hollow silica microspheres of 40-200 nm, but the hollow spheres prepared by the method have a larger particle size, a wider distribution range, and require high-temperature calcination. CN101214965A discloses a preparation method of macroporous-mesoporous hollow silica microspheres, wherein a block copolymer P123 is used as a template agent, to obtain hollow silica microspheres having two pore structures of macropores and mesopores, but the double emulsion configuration of the template is relatively complicated, and the post-processing process requires high-temperature calcination to remove the surfactant and the organic solvent. CN101121519A also discloses that in an alcohol system, ammonia catalyzes the hydrolysis of silicate and silane coupling agent to obtain hybrid silica submicron spheres, which have a mesoporous structure with an average pore size of 3 to 10 nm. The preparation process is simple, but the process requires an alcohol organic solvent and an ammonia alkaline solution, and uses hydrofluoric acid to corrode the sol of the hybrid silica submicron spheres, which is very dangerous. CN201310754067X discloses a method for preparing hollow silica microspheres. Although this method avoids energy-consuming and cumbersome processes such as high-temperature calcination and solvent etching, it requires repeated extraction, centrifugal washing and other steps to remove the core part template agent to obtain hollow silica microspheres, and the post-processing is cumbersome, which limits its large-scale production.

[0004] At present, the preparation methods of hollow silica microspheres all require the use of high-temperature calcination, chemical corrosion, repeated centrifugal washing and other methods to remove the template agent, which greatly hinders the application of hollow silica nanospheres in catalysis, drug controlled release and other fields. Summary of the invention

[0005] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the present invention provides a method for preparing hollow silica microspheres, which solves the cumbersome and energy-consuming process of removing the internal template by high-temperature calcination or solvent etching, repeated centrifugal washing, etc. in the prior art for preparing hollow silica microspheres, avoids the adverse effects of various possible post-processing methods on the hollow microspheres, such as the integrity of the hollow spherical structure and the lack of monodispersity of the spheres, and synthesizes complete and monodisperse hollow silica microspheres.

[0006] The first aspect of the present invention provides a method for preparing hollow silica microspheres, the preparation method comprising the following steps:

[0007] S1: dropping acrylic acid monomer and acrylate monomer into the initiator solution for mixing reaction to obtain a seed emulsion;

[0008] S2: adding a hard monomer and an initiator solution dropwise to the seed emulsion to react, and keeping the temperature after the addition is completed to obtain a core-shell polymer emulsion;

[0009] S3: adding ammonia water or an ammonia-based organic base to the core-shell polymer emulsion, adjusting the pH, and then dropping silicate. After the addition is completed, aging is performed to obtain the hollow silica microspheres.

[0010] A technical solution in the method for preparing hollow silica microspheres of the present invention has at least the following beneficial effects:

[0011] The preparation method of the present invention comprises the following steps: firstly synthesizing a seed emulsion, wherein the seed emulsion is prepared from an acrylic monomer and an acrylate monomer under the action of an initiator, wherein the acrylic monomer itself contains a carboxyl group, and the prepared seed emulsion is a highly acidic seed emulsion rich in carboxylic acid, and then 1-2 layers of hard organic shell layer emulsion are wrapped on the outside of the seed emulsion to prepare a core-shell structure emulsion. Finally, at the softening point temperature of the organic shell layer polymer, ammonia water or an ammonia organic base is added for neutralization, and the ammonia water enters the interior of the polymer to react with the highly acidic core layer rich in carboxylic acid to generate a hydrophilic polymer rich in carboxylate ions. Since the hydrophilicity of the carboxylate ions is much greater than that of the carboxylate group, the carboxylate-rich chain segments (or molecules) will pull the entire core polymer molecular chain to migrate to the surface of the colloid particles, resulting in the formation of voids inside the colloid particles. Simultaneously, due to the difference in ion concentration, a large amount of water enters the interior of the polymer to swell, forming a hollow polymer microsphere emulsion. Finally, silicate is slowly dripped into the hollow polymer microsphere emulsion. The silicate is hydrolyzed and condensed under the catalysis of ammonium carboxylate and captured by ammonium carboxylate ions, thereby growing a layer of silica shell on the surface of the hollow polymer latex sphere, and finally forming a hollow silica microsphere.

[0012] In the preparation method of the present invention, the preparation of the core-shell structure polymer emulsion is a key step. If the structure design of the core-shell polymer is unreasonable, the hollow microsphere cavity will be too large or too small, or the hollow microsphere structure will be unstable.

[0013] In the preparation method of the present invention, the amount of ammonia water added has an important influence on the morphology and structure of the hollow silica. If the amount of ammonia water added is too little, the hydrophilicity of the highly acidic core molecular chain in the core-shell structure polymer emulsion is insufficient, and the entire core polymer molecular chain cannot be pulled to migrate to the surface of the colloid particle to form a hollow polymer microsphere emulsion, so hollow silica microspheres cannot be formed; if the amount of ammonia water added is too much, the carboxylate-rich polymer will diffuse to the particle surface in large quantities, causing the hollow polymer particles to collapse or part of the carboxylate-rich molecules to completely enter the water phase, thereby reducing the volume increase of the latex particles or even shrinking the volume; at the same time, if the amount of ammonia water is too much, the silicate condensation speed is too fast, and it cannot be deposited on the surface of the hollow polymer microsphere to form a silica shell layer, but self-polymerizes to form solid silica particles.

[0014] The preparation method of the present invention solves the cumbersome and energy-consuming process of preparing hollow silica microspheres in the prior art, which requires high-temperature calcination or solvent etching, repeated centrifugal washing and the like to remove the internal template, and avoids the adverse effects of various possible post-treatment means on the hollow microspheres, such as the integrity of the hollow spherical structure and the lack of monodispersity of the spheres, thereby synthesizing complete and monodisperse hollow silica microspheres.

[0015] According to some embodiments of the present invention, in the acrylic acid monomer and acrylate monomer added dropwise in step S1, the content of the acrylic acid monomer is 5 wt % to 50 wt %.

[0016] According to some embodiments of the present invention, the acrylic monomer includes at least one of acrylic acid and methacrylic acid.

[0017] According to some embodiments of the present invention, the acrylic acid ester monomer includes at least one of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate.

[0018] According to some embodiments of the present invention, in step S1, the temperature of adding acrylic acid monomer and acrylate monomer for mixing reaction is 70°C to 90°C for 30min to 300min. After the addition is completed, the mixture is kept warm for 2h to 4h.

[0019] According to some embodiments of the present invention, in step S1, the amount of the initiator added is 0.1-2% of the total amount of the mixed monomers of the acrylic acid monomer and the acrylate monomer.

[0020] According to some embodiments of the present invention, in step S1, a certain amount of deionized water may be first added to a four-necked flask equipped with a stirrer and a spherical condenser, and then the initiator may be added to the water for mixing.

[0021] According to some embodiments of the present invention, the solid content of the seed emulsion is 10% to 20%.

[0022] According to some embodiments of the present invention, the pH of the seed emulsion is 2-3.

[0023] According to some embodiments of the present invention, the hard monomer includes at least one of styrene, acrylonitrile and divinylbenzene.

[0024] According to some embodiments of the present invention, in step S2, hard monomer and initiator solution are added to the seed emulsion for reaction, the amount of hard monomer added is 1 to 5 times the total amount of acrylic monomer and acrylate monomer mixed monomer, and the amount of initiator solution added is 0.1 to 2% of the amount of hard monomer.

[0025] According to some embodiments of the present invention, in step S2, the hard monomer and initiator solution are added dropwise for a reaction time of 30 to 300 minutes. After the addition is completed, the mixture is kept warm for 2 to 4 hours, cooled to 40 to 50° C., filtered, and discharged to obtain the core-shell polymer emulsion.

[0026] According to some embodiments of the present invention, the solid content of the core-shell polymer emulsion is 25% to 45%.

[0027] According to some embodiments of the present invention, in step S2, the hard monomer and the initiator solution may be slowly added dropwise to a four-necked flask containing the highly acidic seed emulsion under stirring.

[0028] According to some embodiments of the present invention, in step S3, ammonia water or an ammonia-based organic base is added to adjust the pH to 8-13.

[0029] According to some embodiments of the present invention, in step S3, ammonia water or an ammonia-based organic base is added to adjust the pH, and the pH is preferably 11 to 12.8.

[0030] Ammonia-based organic bases include triethylamine.

[0031] According to some embodiments of the present invention, in step S3, the time for adding the silicate dropwise is 30 min to 300 min.

[0032] The amount of silicate added is core-shell polymer emulsion solid content / theoretical silica content=20-50%, wherein the core-shell polymer emulsion solid content is the core-shell polymer emulsion mass×solid content; the theoretical silica content is silicate molar amount×60.

[0033] According to some embodiments of the present invention, in step S3, a certain amount of core-shell polymer emulsion can be added to a four-necked flask containing a certain amount of water, a certain amount of ammonia water is added, the pH value is adjusted to a suitable range, and the silicate is slowly dripped in while stirring at room temperature to 40°C.

[0034] According to some embodiments of the present invention, the silicate includes at least one of ethyl orthosilicate, methyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane and phenyltriethoxysilane.

[0035] According to some embodiments of the present invention, the initiator solution includes at least one of azobisisobutylcyanide solution, azobisisobutylamidine hydrochloride solution, benzoyl peroxide solution, dibenzoyl peroxide solution, tert-butyl benzoyl peroxide solution, methyl ethyl ketone peroxide solution, tert-butyl hydrogen peroxide solution, ammonium or alkali metal salt solution of persulfate, and sodium perborate solution.

[0036] According to some embodiments of the present invention, the initiator solution is an aqueous solution of an initiator. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is the microscopic morphology of the hollow silica microspheres prepared in Example 1. DETAILED DESCRIPTION

[0038] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.

[0039] In a first aspect, some embodiments of the present invention provide a method for preparing hollow silica microspheres, comprising the following steps:

[0040] S1: dropping acrylic acid monomer and acrylate monomer into the initiator solution for mixing reaction to obtain a seed emulsion;

[0041] S2: adding hard monomer and initiator solution dropwise to the seed emulsion to react, and keeping the temperature after the addition is completed to obtain a core-shell polymer emulsion;

[0042] S3: adding ammonia water or an ammonia-based organic base to the core-shell polymer emulsion, adjusting the pH, and then dropping silicate. After the addition is completed, aging is performed to obtain hollow silica microspheres.

[0043] It can be understood that the preparation method of the present invention first synthesizes a seed emulsion, which is made from acrylic monomers and acrylate monomers under the action of an initiator, and is a highly acidic seed emulsion rich in carboxylic acid, and then 1-2 layers of hard organic shell layer emulsion are wrapped on the outside of the seed emulsion to obtain a core-shell structure emulsion. Finally, at the softening point temperature of the organic shell polymer, ammonia water or an ammonia organic base is added for neutralization, and ammonia water enters the interior of the polymer and reacts with the high acid core layer rich in carboxylic acid to produce a hydrophilic polymer rich in carboxylate ions. Since the hydrophilicity of the carboxylate ions is much greater than that of the carboxylate group, the carboxylate-rich chain segments (or molecules) will pull the entire core polymer molecular chain to migrate to the surface of the colloid particles, resulting in a gap formed inside the colloid particles. At the same time, due to the difference in ion concentration, a large amount of water enters the interior of the polymer to swell, forming a hollow polymer microsphere emulsion. Finally, silicate is slowly dripped into the hollow polymer microsphere emulsion. The silicate is hydrolyzed and condensed under the catalysis of ammonium carboxylate and captured by ammonium carboxylate ions, thereby growing a layer of silica shell on the surface of the hollow polymer latex sphere, and finally forming a hollow silica microsphere.

[0044] It should be noted that in the preparation method of the present invention, the preparation of the core-shell structure polymer emulsion is a key step. If the structure design of the core-shell polymer is unreasonable, the hollow microsphere cavity will be too large or too small, or the hollow microsphere structure will be unstable.

[0045] The carboxylic acid content of high-acid seed latex and the particle size of high-acid seed latex affect the size of the cavity of hollow polymer microspheres; when synthesizing high-acid seed latex, the more carboxylic acid content, the stronger the hydrophilicity, the smaller the particle size of the formed high-acid seed latex particles, and the smaller the cavity of the subsequently synthesized hollow polymer microspheres, or even no cavity can be formed; at the same time, the carboxylic acid content affects the hydrophilicity of the core polymer molecular chain after neutralization with ammonia water, thereby affecting the speed and amount of migration of the entire core polymer molecular chain to the surface of the colloid particle. The less the core polymer molecular chain migrates to the surface of the colloid particle, the smaller the cavity formed, and the more the core polymer molecular chain migrates to the surface of the colloid particle, the larger the cavity formed; in addition, the type and amount of hard monomer introduced affect the thickness and hardness of the shell layer of the core-shell polymer latex. When the shell layer is thick or harder, the structure of the hollow microsphere formed is firm.

[0046] It should also be noted that in the preparation method of the present invention, the amount of ammonia added has an important influence on the morphology and structure of the hollow silica. If the amount of ammonia added is too little, the high-acid core molecular chain in the core-shell structure polymer emulsion is not sufficiently hydrophilic, and cannot pull the entire core polymer molecular chain to migrate to the surface of the colloid particles to form a hollow polymer microsphere emulsion, and therefore cannot form hollow silica microspheres; if the amount of ammonia added is too much, the carboxylate-rich polymer will diffuse to the particle surface in large quantities, causing the hollow polymer particles to collapse or some of the carboxylate-rich molecules to completely enter the water phase, thereby reducing the volume increase of the latex particles or even shrinking the volume; at the same time, if the amount of ammonia is too much, the silicate condensation rate is too fast, and it cannot be deposited on the surface of the hollow polymer microspheres to form a silica shell layer, but instead self-polymerizes to form solid silica particles.

[0047] The preparation method of the present invention solves the cumbersome and energy-consuming process of preparing hollow silica microspheres in the prior art, which requires high-temperature calcination or solvent etching, repeated centrifugal washing and the like to remove the internal template, and avoids the adverse effects of various possible post-treatment means on the hollow microspheres, such as the integrity of the hollow spherical structure and the lack of monodispersity of the spheres, thereby synthesizing complete and monodisperse hollow silica microspheres.

[0048] In combination with the first aspect, in some embodiments of the present invention, in the acrylic acid monomer and acrylate monomer added dropwise in step S1, the content of the acrylic acid monomer is 5 wt % to 50 wt %.

[0049] In combination with the first aspect, in some embodiments of the present invention, the acrylic monomer includes at least one of acrylic acid and methacrylic acid.

[0050] In combination with the first aspect, in some embodiments of the present invention, the acrylic acid ester monomer includes at least one of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate.

[0051] In combination with the first aspect, in some embodiments of the present invention, in step S1, the temperature of adding acrylic acid monomer and acrylate monomer for mixing reaction is 70°C to 90°C and the time is 30min to 300min. After the addition is completed, the mixture is kept warm for 2h to 4h.

[0052] In combination with the first aspect, in some embodiments of the present invention, in step S1, the amount of the initiator added is 0.1-2% of the total amount of the mixed monomers of the acrylic acid monomer and the acrylate monomer.

[0053] In combination with the first aspect, in some embodiments of the present invention, in step S1, a certain amount of deionized water can be first added to a four-necked flask equipped with a stirrer and a spherical condenser, and then the initiator can be added to the water for mixing.

[0054] In combination with the first aspect, in some embodiments of the present invention, the solid content of the seed emulsion is 10% to 20%.

[0055] In combination with the first aspect, in some embodiments of the present invention, the pH of the seed emulsion is 2-3.

[0056] In combination with the first aspect, in some embodiments of the present invention, the hard monomer includes at least one of styrene, acrylonitrile, and divinylbenzene.

[0057] In combination with the first aspect, in some embodiments of the present invention, in step S2, hard monomers and initiator solutions are added to the seed emulsion for reaction, the amount of hard monomers added is 1 to 5 times the total amount of the mixed monomers of acrylic monomers and acrylate monomers, and the amount of initiator solution added is 0.1 to 2% of the amount of hard monomers.

[0058] In combination with the first aspect, in some embodiments of the present invention, in step S2, the hard monomer and initiator solution are added dropwise for reaction for 30 min to 300 min. After the addition is completed, the mixture is kept warm for 2 h to 4 h, cooled to 40° C. to 50° C., filtered, and discharged to obtain a core-shell polymer emulsion.

[0059] In combination with the first aspect, in some embodiments of the present invention, the solid content of the core-shell polymer emulsion is 25% to 45%.

[0060] In combination with the first aspect, in some embodiments of the present invention, in step S2, the hard monomer and initiator solution may be slowly added dropwise to a four-necked flask containing the high-acid seed emulsion under stirring.

[0061] In combination with the first aspect, in some embodiments of the present invention, in step S3, ammonia water or an ammonia-based organic base is added to adjust the pH to 8-13.

[0062] In combination with the first aspect, in some embodiments of the present invention, in step S3, ammonia water or an ammonia-based organic base is added to adjust the pH, and the pH is preferably 11 to 12.8.

[0063] In combination with the first aspect, in some embodiments of the present invention, in step S3, the time for adding the silicate dropwise is 30 min to 300 min.

[0064] The amount of silicate added is core-shell polymer emulsion solid content / theoretical silica content=20-50%, wherein the core-shell polymer emulsion solid content is the core-shell polymer emulsion mass×solid content; the theoretical silica content is silicate molar amount×60.

[0065] In combination with the first aspect, in some embodiments of the present invention, in step S3, a certain amount of core-shell structure polymer emulsion can be added to a four-necked flask containing a certain amount of water, a certain amount of ammonia water is added, the pH value is adjusted to a suitable range, and the silicate is slowly dripped in while stirring at room temperature to 40°C.

[0066] In combination with the first aspect, in some embodiments of the present invention, the silicate includes at least one of ethyl orthosilicate, methyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane and phenyltriethoxysilane.

[0067] In combination with the first aspect, in some embodiments of the present invention, the initiator solution includes at least one of azobisisobutylcyanide solution, azobisisobutylamidine hydrochloride solution, benzoyl peroxide solution, dibenzoyl peroxide solution, tert-butyl benzoyl peroxide solution, methyl ethyl ketone peroxide solution, tert-butyl hydrogen peroxide solution, ammonium or alkali metal salt solution of persulfate, and sodium perborate solution.

[0068] In combination with the first aspect, in some embodiments of the present invention, the initiator solution is an aqueous solution of the initiator.

[0069] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0070] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0071] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.

[0072] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.

[0073] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0074] Example 1

[0075] A hollow silica microsphere was prepared, and the specific steps were as follows:

[0076] 1. Seed emulsion synthesis

[0077] In a four-necked flask equipped with a stirrer and a spherical condenser, add 85 g of deionized water, add 0.15 g of ammonium persulfate initiator into the water and mix, control the reaction temperature to 75°C, slowly drop 5 g of methacrylic acid and 10 g of methyl methacrylate to carry out a mixing reaction, the dropwise reaction time is 30 minutes, and after the addition is completed, keep warm for 2 hours to obtain a highly acidic seed emulsion.

[0078] 2. Synthesis of core-shell polymer emulsion:

[0079] Into a four-necked flask containing high-acid seed emulsion, 25 g of styrene and 0.25 g of ammonium persulfate initiator were slowly added dropwise under stirring. The reaction time was 150 minutes. After the addition was completed, the temperature was kept at 75°C for 3 hours, then the temperature was lowered to 45°C, and the material was filtered and discharged to obtain a core-shell structure polymer emulsion.

[0080] 3. Preparation of hollow silica microspheres:

[0081] Take 10g of the core-shell structure polymer emulsion and add it to a four-necked flask containing 20g of deionized water, add 35g of 28% concentrated ammonia water, adjust the pH value to 12.51, and slowly drop 27g of ethyl orthosilicate while stirring at room temperature (25°C) for 150 minutes. After the addition is completed, age at room temperature for 4 days to obtain a hollow silica microsphere emulsion.

[0082] Example 2

[0083] A hollow silica microsphere was prepared, and the specific steps were as follows:

[0084] 1. Synthesis of high acid seed emulsion

[0085] In a four-necked flask equipped with a stirrer and a spherical condenser, 90 g of deionized water was added, 0.10 g of ammonium persulfate initiator was added to the water for mixing, the reaction temperature was controlled to 75°C, 3 g of methacrylic acid and 7 g of methyl methacrylate were slowly added dropwise for mixing reaction, the dropwise reaction time was 30 minutes, and after the addition was completed, the temperature was kept for 2 hours to obtain a high-acid seed emulsion.

[0086] 2. Synthesis of core-shell polymer emulsion:

[0087] Into a four-necked flask containing high-acid seed emulsion, 37.5 g of styrene, 0.5 g of divinylbenzene and 0.38 g of ammonium persulfate initiator were slowly added dropwise under stirring. The reaction time was 180 minutes. After the addition was completed, the temperature was kept at 75°C for 3 hours, then the temperature was lowered to 45°C, and the material was filtered and discharged to obtain a core-shell structure polymer emulsion.

[0088] 3. Preparation of hollow silica microspheres:

[0089] Take 10g of the core-shell structure polymer emulsion and add it to a four-necked flask filled with 40g of deionized water, add 20g of 28% concentrated ammonia water, adjust the pH value to 12.13, and slowly drop 35g of ethyl orthosilicate while stirring at room temperature (25°C) for 150 minutes. After the addition is completed, age at room temperature for 4 days to obtain a hollow silica microsphere emulsion.

[0090] Example 3

[0091] A hollow silica microsphere was prepared, and the specific steps were as follows:

[0092] 1. Synthesis of high acid seed emulsion

[0093] Add 80g of deionized water to a four-necked flask equipped with a stirrer and a spherical condenser, add 0.20g of ammonium persulfate initiator into the water and mix, control the reaction temperature to 75°C, slowly drop 8g of methacrylic acid and 12g of methyl methacrylate to carry out a mixing reaction, the drop reaction time is 30 minutes, and keep warm for 2h after the addition is completed to obtain a high-acid seed emulsion.

[0094] 2. Synthesis of core-shell polymer emulsion:

[0095] Into a four-necked flask containing high-acid seed emulsion, 33 g of styrene, 0.5 g of divinylbenzene and 0.335 g of ammonium persulfate initiator were slowly added dropwise under stirring. The reaction time was 180 minutes. After the addition was completed, the temperature was kept at 75°C for 3 hours, then the temperature was lowered to 45°C, and the material was filtered and discharged to obtain a core-shell structure polymer emulsion.

[0096] 3. Preparation of hollow silica microspheres:

[0097] Take 10g of the core-shell structure polymer emulsion and add it to a four-necked flask filled with 40g of deionized water, add 40g of concentrated ammonia water with a mass fraction of 28%, adjust the pH value to 11.98, and slowly drop 31g of ethyl orthosilicate while stirring at room temperature of 25°C for 150 minutes. After the addition is completed, age at room temperature for 4 days to obtain a hollow silica microsphere emulsion.

[0098] Comparative Example 1

[0099] Taking Example 3 as a reference, a silica microsphere was prepared, which differed from Example 3 in that methacrylic acid was not added. The prepared microsphere was a solid microsphere.

[0100] Comparative Example 2

[0101] Taking Example 3 as a reference, a silicon dioxide was prepared, which differed from Example 3 in that no ammonia water was added. The prepared silicon dioxide was linear silicon dioxide.

[0102] The morphology of the silica microspheres prepared in Example 1 was observed. Figure 1 As shown, it can be seen that it is a hollow microsphere.

[0103] The particle sizes and pore sizes of the silica microspheres and silica materials prepared in the examples and comparative examples were tested, as shown in Table 1.

[0104] Table 1

[0105]

[0106]

[0107] In Table 1, “pore size” refers to the diameter of the cavity of the hollow silica nanoparticles.

[0108] It should be noted that the preparation method of the present invention can prepare hollow silica microspheres without complicated processing steps such as calcination and etching.

[0109] The hollow silica microspheres prepared by the preparation method of the present invention are usually in the form of an emulsion. The microspheres in the form of an emulsion are convenient for use in coatings and other scenarios, and can also be further processed according to specific application scenarios to become solid or other forms.

[0110] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A method for preparing hollow silica microspheres, characterized in that: The preparation method comprises the following steps: S1: dropping acrylic acid monomer and acrylate monomer into the initiator solution for mixing reaction to obtain a seed emulsion; S2: adding a hard monomer and an initiator solution dropwise to the seed emulsion to react, and keeping the temperature after the addition is completed to obtain a core-shell polymer emulsion; S3: adding ammonia water or an ammonia-based organic base to the core-shell polymer emulsion, adjusting the pH, and then dropping silicate. After the addition is completed, aging is performed to obtain the hollow silica microspheres.

2. The preparation method according to claim 1, characterized in that: In the acrylic acid monomer and acrylate monomer added dropwise in step S1, the content of the acrylic acid monomer is 5 wt % to 50 wt %.

3. The preparation method according to claim 1, characterized in that: In step S1, the temperature of adding acrylic acid monomer and acrylic ester monomer for mixed reaction is 70°C to 90°C for 30min to 300min. After the addition is completed, the mixture is kept warm for 2h to 4h.

4. The preparation method according to claim 1, characterized in that: In step S2, the hard monomer and initiator solution are added dropwise for a reaction time of 30 to 300 minutes. After the addition is completed, the temperature is kept for 2 to 4 hours, then the temperature is lowered to 40° C. to 50° C., and the core-shell polymer emulsion is obtained by filtering and discharging.

5. The preparation method according to claim 1, characterized in that: In step S3, ammonia water or an ammonia-based organic base is added to adjust the pH to 8-13.

6. The preparation method according to claim 1, characterized in that: In step S3, the time for dropping the silicate is 30 min to 300 min.

7. The preparation method according to any one of claims 1 to 6, characterized in that The acrylic monomer includes at least one of acrylic acid and methacrylic acid; and / or the acrylate monomer includes at least one of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate.

8. The preparation method according to any one of claims 1 to 6, characterized in that: The hard monomer includes at least one of styrene, acrylonitrile and divinylbenzene.

9. The preparation method according to any one of claims 1 to 6, characterized in that: The solid content of the core-shell polymer emulsion is 25% to 45%.

10. The preparation method according to any one of claims 1 to 6, characterized in that: The initiator solution comprises at least one of azobisisobutylcyanide solution, azobisisobutylamidine hydrochloride solution, benzoyl peroxide solution, dibenzoyl peroxide solution, tert-butyl benzoyl peroxide solution, methyl ethyl ketone peroxide solution, tert-butyl hydrogen peroxide solution, ammonium or alkali metal salt solution of persulfate, and sodium perborate solution.

Citation Information

Patent Citations

  • Preparation method for coating silica by utilizing polymer hollow microspheres

    CN102311555A

  • Amino functionalized hollow multistage mesoporous silica microspheres and preparation method thereof

    CN109399647A

  • Method for preparing silicon dioxide-polymer hollow microspheres by continuous method

    CN118165352A

  • Hollow silica powder, method for producing the same and application thereof

    JP2011042527A

  • Method of producing spherical hollow silica particles

    JP2014125400A