Method for forming scratch channel and separating reinforced display glass

By forming vertical defects on the reinforced display glass and using laser source and cooling injection technology, the problem of blocking cross-channels of the separation line substrate is solved, and the precise segmentation and high-quality edge characteristics of the reinforced display glass are achieved.

CN118930029AInactive Publication Date: 2024-11-12QINGDAO FUSION PHOTOELECTRIC TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410998813.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Prior art When separating the reinforced display glass, the whole body separation of the substrate along the separation line prevents the formation of additional crossing channels on the individual reinforced display glass, resulting in poor edge characteristics and uncontrollable separation.

Method used

By forming vertical defects on the compressed surface of the reinforced display glass, and using laser sources and cooling jet technology, the light beam and cooling points are guided along the desired separation line to form accurate scratch channels, and precise segmentation of the reinforced display glass is achieved.

Benefits of technology

The precise scratching channels are formed on the reinforced display glass, ensuring the neatness and quality of the segmented surfaces, avoiding uncontrollable whole-body separation, and allowing accurate separation and processing during marking and breaking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930029A_ABST
    Figure CN118930029A_ABST
Patent Text Reader

Abstract

The invention provides a method for forming a scratch channel and separating strengthened display glass, which comprises the following steps of: forming a vertical defect by compressing a surface layer, so that the defect deviates from a first edge of the strengthened display glass; the internal tensile stress layer exposed below the compression layer of the glass is beneficial to starting the channel in the laser scratching process; directing a beam spot of the laser source onto the compression layer along the desired separation line, a cooling point produced by the cooling nozzle being directed onto the compression layer such that the cooling point is located near a trailing edge of the beam spot; according to the use method, the strengthened display glass can be separated through the scribing and breaking process, a scribing channel is formed in the surface of the display glass and does not make contact with the edge of the display glass, and the strengthened display glass applied to the scribing channel can be separated by applying force to the scribing channel along the line. And the strengthened display glass can be crossed and scribed by forming crossed scribing channels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of separating strengthened display glass, in particular to a method for forming a scratch channel and separating strengthened display glass. Background Art

[0002] Thin display glass has a variety of applications in consumer electronic devices. For example, display glass can be used as a cover plate for LCD and LED displays in mobile phones, display devices such as televisions and computer monitors, and various other electronic devices. The cover plates used in these devices can be formed by splitting or separating a large display glass into multiple smaller display glasses using various laser cutting techniques. For example, the display glass can be separated by a scribing and breaking technique. However, when a strengthened display glass (such as ion exchange glass) is separated using a scribing and breaking technique, uncontrolled full-body separation may occur instead of the formation of the scribing line. Uncontrolled separation generally results in poor edge characteristics compared to the scribing and breaking process. In addition, the full-body separation of the substrate along the separation line prevents the formation of additional cross-channels on the single strengthened display glass.

[0003] In summary, the present invention provides a method for forming a scratch channel and separating a strengthened display glass to solve the above problems. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for forming a scratch channel and separating a strengthened display glass, so as to solve the problem that the whole body separation of the substrate along the separation line in the prior art prevents the formation of additional cross channels on a single strengthened display glass.

[0005] A method for forming a scratch channel and separating a strengthened display glass, comprising:

[0006] forming a vertical defect by compressing the surface layer such that the defect is offset from the first edge of the strengthened display glass;

[0007] The exposed internal tensile stress layer beneath the compressive layer of glass helps initiate channels during laser scratching;

[0008] directing a beam spot of a laser source onto the compression layer along the desired separation line, and directing a cooling spot generated by a cooling nozzle onto the compression layer such that the cooling spot is located near a trailing edge of the beam spot;

[0009] By translating the laser source and the cooling nozzle, or by translating the strengthened display glass, the cooling point and the beam spot are advanced along the desired separation line until the beam spot is positioned at a termination position deviating from the second edge of the strengthened display glass, thereby forming a channel that partially passes through the thickness of the strengthened glass, and the formed scratch channel extends from the deviated defect to the termination position, thereby achieving precise separation of the strengthened display glass;

[0010] The intersecting score channels are formed by forming a first score channel at a first score speed and forming an intersecting second score channel at a second score speed greater than the first score speed.

[0011] Furthermore, the strengthened display glass can be composed of various glasses, including one or more of borosilicate glass, aluminosilicate glass and aluminoborosilicate glass, and can be firmly held in the system by using a mechanical or vacuum suction cup, which can be achieved by a series of vacuum holes spaced a certain distance apart on a vacuum plate.

[0012] Furthermore, the cooling jet generally includes a pressurized fluid ejected from a nozzle and directed to the surface of the tempered display glass, the cooling jet including one of compressed air, compressed nitrogen, compressed helium or similar compressed gases, or a mixture of liquid and compressed gas, wherein the mixture of liquid and compressed gas is a mist gas mixture of one of compressed deionized water, air and nitrogen.

[0013] Furthermore, by controlling the width and length of the beam spot, the heating effect of the laser beam on the strengthened display glass can be adjusted, thereby controlling the depth and formation process of the channel.

[0014] Further, the defect is mechanically formed by applying a diamond scriber, and the defect depth is not less than the layer depth.

[0015] Furthermore, in order to form the scratch channel on the surface of the strengthened display glass, it is necessary to use a cooling jet emitted from a nozzle to cool or quench the heated surface of the strengthened display glass.

[0016] Furthermore, the strengthened glass includes strengthened display glass made of borosilicate glass, strengthened display glass made of aluminosilicate glass and ion exchange strengthened aluminosilicate glass.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. The method of use of the present invention allows the strengthened display glass to be separated through a scribing and breaking process, wherein a scribing channel is formed on the surface of the display glass, the channel does not contact the edge of the display glass, the strengthened display glass applied to the scribing channel can be separated by applying a force along the scribing channel, and the strengthened display glass can be cross-scored by forming intersecting scribing channels.

[0019] 2. The present invention generates tensile stress below the glass surface along the desired separation line through the heat energy generated by the laser source and the quenching effect of the cooling jet. The tensile stress causes a channel to form and propagate inside the strengthened display glass. By precisely controlling the position of laser heating, the position of the cooling jet and the relative speed of the two, a precise scratch channel can be formed on the strengthened display glass for subsequent segmentation and processing.

[0020] 3. The present invention can ensure that the scratch channel is formed only between the defect and the termination position by precisely controlling the time and position of laser heating and cooling quenching, as well as the power of the laser source and the translation speed of the strengthened display glass, thereby achieving precise segmentation of the strengthened display glass. This control method allows the strengthened display glass to be precisely separated without affecting the unscratched area, thereby ensuring the neatness of the scratch channel and the quality of the segmentation surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] FIG. 1( a ) is a schematic diagram of a non-edge defect on a strengthened display glass of the present invention and an elliptical spot of a laser beam;

[0022] Figure 1b is a perspective schematic diagram of a cooling point of a cooling nozzle of the present invention;

[0023] Figure 2 is a cross section of the laser beam, cooling nozzle and strengthened display glass of the present invention;

[0024] Figure 3 is the relative position of the elliptical light spot and the cooling point of the present invention;

[0025] Figure 4 is a cross section of the scratch channel and the front end of the channel of the present invention;

[0026] Figure 5 is a perspective view of a scratch channel of the present invention;

[0027] Figure 6 is a perspective view of a laser protection cover on a surface of a reinforced display glass according to the present invention;

[0028] Figure 7 is a top view of a plurality of non-edge defects and a desired separation line in a first direction of the present invention;

[0029] Figure 8 is a top view of two non-edge defects and the intersecting desired separation line in the first and second scratch directions of the present invention;

[0030] Fig. 9 is a perspective view of first and second score channels intersecting at an intersection location of the present invention;

[0031] Fig. 10A is a side view of a first scratch channel of the present invention along a first scratch direction;

[0032] Fig. 10B is a side view of a second scratch channel along a second scratch direction intersecting with a first scratch channel along a first scratch direction of the present invention;

[0033] Fig. 10C is a side view of a second scratch channel along a second scratch direction intersecting with a first scratch channel along a first scratch direction of the present invention;

[0034] Fig.11 It is a top view of multiple non-edge defects and desired separation lines in the first scratch direction and the second scratch direction of the present invention. DETAILED DESCRIPTION

[0035] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0036] As shown in Figure 1-11:

[0037] refer to Figure 1(a) , 2 5, an exemplary system is schematically depicted for forming a controlled crack or scratch channel 109 extending partially through the thickness of a strengthened display glass 100. The system generally includes a laser source 150 for heating the strengthened display glass 100 along a desired separation line 104, and a nozzle 160 for directing a cooling jet 105 to cool the heated surface of the strengthened display glass 100 along the desired separation line 104. The change in temperature of the strengthened display glass due to the application of the beam spot 102 and the cooling spot 106 generates a tensile stress at the desired separation line 104 in a direction perpendicular to the desired separation line 104, thereby forming the channel 109 that extends partially through the thickness of the strengthened display glass 100. The completed scratch channel 109 is located at the desired location where the strengthened display glass 100 may be separated by applying a mechanical force.

[0038] In the embodiment described herein, the strengthened display glass 100 has a first surface 130, a second surface 132, edges (e.g., a first edge 114 and a second edge 116), and a thickness h. It should be understood that the strengthened display glass may have other shapes, such as a circle. The strengthened display glass may be chemically strengthened by an ion exchange process to produce a compressive surface layer 111 extending to the depth of layer (DOL) and a tensile stress layer 115 located inside the strengthened display glass. The strengthened display glass can be composed of various glasses, including but not limited to borosilicate glass, aluminosilicate glass, and aluminoborosilicate glass.

[0039] The strengthened display glass 100 can be held firmly within the system by using mechanical or vacuum chucks. The vacuum chuck can be achieved by a series of vacuum holes spaced a certain distance apart in a vacuum plate. However, the stress gradients generated by the holes may be sufficient to distort the stress field and thus affect the laser scratching process of the strengthened display glass. The stress gradients generated by the vacuum suction can be minimized by using closely spaced holes or a porous plate, both of which reduce the vacuum requirements to hold the glass.

[0040] The laser source 150 can emit a beam of light of a suitable wavelength to transfer heat energy to the strengthened display glass 100, so that the laser energy is strongly absorbed by the glass thickness h, thereby heating the strengthened display glass. For example, the laser source 150 generally emits a laser beam 101 having a wavelength in the infrared range. Suitable laser sources include a CO laser having a wavelength of about 5 microns to 6 microns, a HF laser having a wavelength of about 2.6 microns to 3.0 microns, or an Erbium YAG laser having a wavelength of about 2.9 microns. In the embodiment described herein, the laser source is a CO2 laser, which produces an infrared beam having a wavelength of about 9.4 microns to 10.6 microns. The CO2 laser source can be a radio frequency excited laser source, operating in a quasi-continuous wave mode. In one embodiment, the laser source 150 is operated to produce an output beam in a TEM00 mode, so that the laser beam 101 of the laser source 150 has a Gaussian intensity distribution. Alternatively, the laser source can be operated to produce an output beam in a TEM01 mode, so that the output beam has a "D" shape or a planar mode intensity distribution. The output power of the laser source can be varied from approximately 20 watts to over 500 watts, depending on the desired scratching speed, the composition of the glass being scratched, and the depth of the compressed surface.

[0041] In order to avoid overheating the surface of the strengthened display glass 100 (which may cause the glass to peel off or evaporate from the surface of the strengthened display glass, or residual stress to weaken the cut edge), the light beam 101 emitted by the laser source can be shaped by various optical elements (not shown) so that the light beam 101 has an elliptical spot 102 on the surface of the strengthened display glass 100. For example, in one embodiment, a pair of cylindrical lenses (not shown) are placed in the path of the laser beam 101 emitted by the laser source 150. Alternatively, the cylindrical lens and / or other optical elements for shaping the laser beam to form an elliptical spot are integrated with the laser source 150. The cylindrical lens shapes the laser beam 101 so that the light spot incident on the surface of the strengthened display glass is generally elliptical in shape, as shown in FIG. 1(a). Although the light spot described herein may be elliptical in shape, it should be understood that the embodiments are not limited thereto, and the light spot may also have other shapes, including circular, square, rectangular, etc.

[0042] refer to Figure 3 , the elliptical light spot 102 generally has a short axis 124 of width b and a long axis 125 of length a. Figure 3 As shown, the minor axis 124 intersects the midpoint of the elliptical spot 102. In one embodiment, the width b of the minor axis 124 is approximately the same as the diameter of the cooling spot 106 formed when the cooling nozzle contacts the strengthened display glass surface.

[0043] The major axis 125 generally has a length a from the leading edge 120 to the trailing edge 122 of the elliptical spot 102. Figure 3 As shown. The length a of the elliptical spot 102 can generally control the depth of the channel created by the laser. The longer the laser beam spot, the deeper the channel. If the length a is fixed, an increase in the scratching speed v will produce a shallower channel. Conversely, the slower the scratching speed v, the deeper the channel created. For laser scratching strengthened display glass, the channel depth should be controlled so that the channel grows slowly enough to complete the laser scratching operation. This means that the length of the laser beam should be fixed according to the desired scratching speed for a given strengthened display glass thickness.

[0044] Regarding the laser power of the laser beam 101, the laser power used to heat the strengthened display glass may be limited by the instantaneous power density and the average power density. The instantaneous power density can be defined as the instantaneous laser power Pinst divided by the spot area. The average power density Iaverage can be defined as the laser power P divided by the sum of the laser beam spot size and the lateral coverage area of ​​the laser beam per unit time:

[0045]

[0046] The maximum permissible laser power density to heat the strengthened display glass without causing stress relaxation depends on the properties of the glass, such as heat capacity, thermal diffusivity, light absorption at the laser wavelength, glass softening point, etc. If Iaverage is set equal to Imax, the following results can be derived:

[0047]

[0048] Therefore, the width b of the elliptical spot can be controlled to achieve the desired average power density, since the length a may be fixed to achieve the desired channel depth. More specifically, equation (2) states that: 1) given a fixed laser power and a maximum allowable laser power density, the width b of the elliptical spot should increase as the laser scratching speed decreases; 2) since the laser scratching speed decreases with increasing layer depth, the width b of the laser beam should increase accordingly; 3) increasing the laser power requires increasing the laser beam width b, provided that the laser scratching speed is maintained at a constant speed. As the glass thickness and layer depth increase, the volume of glass that needs to be heated also increases. Since the power density is limited to a certain value, in order to increase the laser power, the width b of the elliptical spot should be increased.

[0049] There will also be heat loss due to thermal diffusion during the scratching process. Thermal diffusion will reduce the local glass temperature heated by the laser. Since the heat loss is proportional to the local temperature gradient, in order to produce the required tensile stress at the front end of the propagating channel, it may be necessary to reduce the temperature gradient at the front end of the channel before and during cooling. This can be achieved by using a wider elliptical spot to heat the volume of the enhanced display glass near the front end of the channel. Alternatively, in one embodiment, a laser beam with a uniformly distributed intensity profile along the short axis can be used to reduce the temperature gradient and increase the temperature at the front end of the channel. Generally, the thicker the enhanced display glass and the deeper the channel, the wider the laser beam along the width b.

[0050] refer to Figure 2 and 3 , the cooling jet 105 typically includes a pressurized fluid ejected from a nozzle 160 and directed to the surface of the strengthened display glass 100. The pressurized fluid may include liquids such as water, ethanol, liquid nitrogen and / or chemical coolants. Alternatively, the cooling jet 105 may include, for example, compressed air, compressed nitrogen, compressed helium, or similar compressed gases. The cooling jet may also include a mixture of liquid and compressed gas (i.e., a mist jet including compressed deionized water and air or nitrogen). In the embodiment described herein, the cooling jet is deionized water. Typically, a solid water jet may be effective in creating a shallow channel because it concentrates cooling on a small area, while a mist jet may produce a deeper channel and have a wider process window. A mist jet can be applied to a larger area and remove most of the heat from the surface of the strengthened display glass.

[0051] A cooling jet 105 is emitted from a hole at the end of a nozzle. When the cooling jet strikes the surface of the strengthened display glass, a cooling spot 106 is formed having a diameter dj that is greater than the diameter of the hole in the nozzle 160. The nozzle 160 is located behind the laser source 150 relative to the scratching direction 110 (i.e., the cutting axis). In the embodiment described herein, the nozzle 160 is angled relative to the surface 130 of the strengthened display glass 100 so that the cooling jet 105 strikes the surface of the strengthened display glass at an angle α that is less than 90 degrees. In one embodiment, the cooling jet 105 can be translated in coordination with the translated beam spot 102. In another embodiment, the strengthened display glass 100 can be mounted on a translation stage that can translate the strengthened display glass 100 under the beam 101 and the cooling jet 105. The cooling jet 105 can be directed to an area on the surface of the strengthened display glass 100 adjacent to the elliptical spot.

[0052] In summary, by controlling the width b and length a of the elliptical spot, the heating effect of the laser beam on the strengthened display glass can be adjusted, thereby controlling the depth and formation process of the channel. The design and operation of the cooling jet 105, such as the position of the nozzle, the type and flow rate of the cooling medium, and the jet angle, all have an impact on the formation of the channel and the quality of the final separation process. By precisely controlling these parameters, the scratch channel can be effectively formed on the strengthened display glass so that it can be subsequently separated into the desired size and shape.

[0053] refer to Figures 1(a) to 5 , a method for forming a scratch channel, wherein the channel extends partially through the thickness h of the strengthened display glass 100, may include first introducing a defect 112 on the first surface 130 (i.e., the surface of the compression surface layer 111) of the strengthened display glass 100 to form a starting point for the scratch channel. The defect 112 is offset from the first edge 114 of the strengthened display glass by a defect offset distance ddef. The defect 112 may be a starting crack formed mechanically or by laser ablation. The defect offset distance ddef may depend on the desired scratching speed, the composition of the scratched glass, and the depth of the compression surface layer 111. In one embodiment, the defect offset distance ddef is approximately 6 mm. In other embodiments, the offset distance may be in the range of approximately 3 mm to approximately 10 mm. As described in more detail below, the channel starts at the defect and propagates along the relative motion direction of the strengthened display glass 100 relative to the laser beam and the cooling jet.

[0054] Defect 112 may be an initiating crack perpendicular to the scratch direction and the desired separation line. A defect 112 having a perpendicular orientation may have higher mechanical repeatability than a defect parallel to the scratch direction. For example, a defect 112 having a perpendicular orientation may prevent the formation of a full-body channel during the scratching process. However, in certain embodiments, it may be desirable to provide a defect 112' parallel to the scratch direction, as shown in FIG. 1B , depending on the composition and physical cracking mechanism of the strengthened display glass being separated.

[0055] Defect 112 is preferably mechanically formed by applying a diamond scriber, although other mechanical devices may be used, such as mechanical scribing wheels, grinding wheels, carbide tips, engravers, etc. The depth of defect 112 should be equal to or slightly greater than the layer depth in order to expose the internal tensile stress layer. Care should be taken when forming the defect to ensure that the defect does not extend too deeply into the internal tensile stress layer. Therefore, the mechanical device should not be too sharp and the force applied should not be too great to avoid causing the defect to penetrate too deeply into the interior of the strengthened display glass. Deep median cracks caused by the application of sharp mechanical devices may penetrate too deeply into the internal tensile stress layer and cause full body cracks during the laser scratching process. Shallow median cracks with many lateral and radial cracks and only partial exposure of the internal tensile stress layer can be achieved using blunt mechanical devices. The type of mechanical device selected may depend on the characteristics of the strengthened display glass, such as the strength of the glass. Conical diamond tips that are typically dragged across the surface of the strengthened display glass will produce more lateral cracks and fewer median cracks. Scribing wheels may produce deep median cracks, which may cause the strengthened display glass to completely separate during the laser scratching process.

[0056] A pneumatic cylinder was used to apply a conical diamond scriber to the surface of a 1.1 mm thick piece of ion exchange strengthened display glass having a 30 micron, 760 MPa compressive stress layer and a 21 MPa internal tensile stress layer. The strengthened display glass is an aluminosilicate glass composed of: 69.17 mol% SiO2; 8.53 mol% Al2O3; 0 mol% B2O3; 13.94 mol% Na2O; 1.17 mol% K2O; 6.45 mol% MgO; 0.54 mol% CaO; and 0.19 mol% SnO2. The angle of the conical diamond tip was about 105°. The pneumatic cylinder applied the diamond tip to the surface of the strengthened display glass with a force of about 9 Newtons, a scribing speed of about 5 mm / sec, and a drag angle of about 12°. The process created a vertical defect that partially exposed the internal tensile stress layer. The properties of the diamond tip and the scribing process may depend on the properties of the strengthened display glass (e.g., thickness of the display glass, thickness of the compressive stress layer and compressive stress, etc.). A conical diamond tip with an angle in the range of about 90° and 130°, and an applied force between about 5 and 20 Newtons, may be used depending on the properties of the strengthened display glass. As another example and not limitation, the conical diamond tip may have a cone angle of 120° and be applied to the strengthened display glass at a drag angle of 5°, a speed of 3 mm / sec, and an applied force of 13 Newtons.

[0057] After the defect 112 is formed, the beam 101 of the laser source 150 is directed to the surface of the strengthened display glass 100 so that the beam is incident on the desired separation line 104 at the defect 112. The beam is initially directed to the substrate so that the defect 112 is located within the elliptical spot 102 of the beam 101 and the major axis 125 of the elliptical spot 102 is substantially aligned with the desired separation line 104. When the beam of the laser source 150 is positioned on the surface 130 of the strengthened display glass 100, the beam transfers radiant heat energy to the compression surface layer 111, thereby heating the strengthened display glass along the desired separation line 104. The maximum temperature Tmax at which the glass surface is heated is generally below the strain point Tg of the glass to avoid stress relaxation during the heating process and the generation of undesirable residual stresses after the cooling spray. As described above, the temperature of the strengthened display glass can be controlled by adjusting various parameters, including, for example, the power of the laser source and the scratching speed v of the laser beam on the surface of the strengthened display glass along the desired separation line. After the beam 101 is initially positioned on the desired separation line 104, the elliptical spot 102 advances along the surface 130 of the strengthened display glass 100 at the desired separation line 104 at a scratching speed v until reaching a termination position 113 offset from the second edge 116, thereby heating the surface of the strengthened display glass along the desired separation line 104, extending from the defect 112 to the termination position 113. The elliptical spot can be translated on the surface by moving the laser source 150 relative to the strengthened display glass 100. In addition, the elliptical spot can be translated by moving the strengthened display glass 100 relative to the laser source 150 and the nozzle 160.

[0058] In order to form the scratch channel 109 on the surface 130 of the strengthened display glass, it is necessary to cool or quench the heated strengthened display glass surface using a cooling jet 105 emitted from a nozzle 160. The temperature change caused by the quenching causes tensile stress to be generated on the surface of the strengthened display glass in a direction perpendicular to the desired separation line 104. Figure 4 , these tensile stresses cause the channel front 140 to propagate below the surface of the strengthened display glass along the scratch direction 110 on the desired separation line 104 and stop near the end position 113 before the second edge 116. The end position 113 can be offset from the second edge 116 by the end distance dterm. In the embodiment described herein, the channel 109 can extend downward below the substrate surface to a depth d less than one-quarter of the thickness h of the strengthened display glass. In one embodiment, the depth d is approximately 15% of the thickness h of the strengthened display glass. In order to initiate and propagate the channel 109 along the surface of the strengthened display glass, it is necessary to generate sufficient tensile stress to initiate and propagate the channel by heating and then cooling the surface of the strengthened display glass beyond the temperature change threshold ΔTTH.

[0059] More specifically, by heating the strengthened display glass using a laser source 150 and quenching the heated strengthened display glass surface with a cooling jet 105, tensile stress is generated on the surface of the strengthened display glass in a direction perpendicular to the desired separation line 104. If the tensile stress exceeds the material's threshold tensile stress σTH, an existing crack or channel 109 in the strengthened display glass 100 may be propagated. The laser-induced tensile stress generated due to the heating and cooling cycles can be estimated as follows:

[0060]

[0061] Where α is the coefficient of thermal expansion, E is Young's modulus, and ΔT is the temperature drop of the laser beam and cooling spray quenching cycle. Using equation (3), the maximum tensile stress that can be generated during the laser heating and cooling spray quenching cycle cannot exceed about 100 to about 200 MPa for any type of glass. This value is significantly less than the surface compression generated by the ion exchange process (e.g., >500 MPa). Therefore, the laser scratching process does not generate sufficient tensile stress to propagate a scratch channel completely enclosed in the compressive layer. Instead, the scratching process for strengthened display glass is an indirect process.

[0062] refer to Figure 4 The tensile stress causes the channel front 140 to propagate along the desired separation line of the surface 130 of the strengthened display glass in the scratch direction 110. Figure 4 As shown, the channel front 140 moves below the surface 130 of the strengthened display glass 100. Since the channel 109 opens below the glass surface, the surface compressive stress is relieved, and after the channel front 140 propagates into the interior of the strengthened display glass, the channel 109 breaks through to the glass surface.

[0063] As the channel front 140 moves below the surface 130 and within the compression skin 111, effective and continuous quenching may be required to generate sufficient tensile stress to propagate the scratch channel 109 near the compression skin 111. The quenching efficiency may depend on the impact velocity of the cooling jet 105, the volume flow rate of the cooling jet 105 provided by the nozzle 160, and the temperature gradient of the cooling jet 105 relative to the heated strengthened display glass 100. In one embodiment, the temperature of the cooling jet 105 (e.g., water) is cooled to a constant temperature, slightly above 0° Celsius. The temperature and flow rate of the cooling jet 105 should be maintained stable throughout the process to achieve the appropriate scratch channel depth.

[0064] Qualitatively, in an ideal system, the characteristic residence cooling time of the cooling jet on the surface of the strengthened display glass is equal to dj / v, where dj is the diameter of the cooling jet core and v is the scratch velocity. The cooling jet core 107 is the central area of ​​the cooling point 106 where the cooling jet impacts the surface of the strengthened display glass. Assuming that the channel front is located at a depth l inside the strengthened display glass, the time required for the quenching effect to reach the layer depth value l can be estimated using a one-dimensional heat conduction model. The model predicts a characteristic time of l / 4D, where D is the thermal diffusivity of the strengthened display glass. Therefore, the diameter of the cooling jet dj can be qualitatively estimated as:

[0065]

[0066] The above equation describes the relationship between the cooling jet diameter dj and the depth of the strengthened display glass layer. As the layer depth increases, the cooling time should increase accordingly.

[0067] The cooling spot 106 may be located near the trailing edge 122 of the elliptical spot 102. Figure 1(a)-3 In one embodiment described herein, the nozzle 160 is oriented so that the cooling spot 106 is positioned on the desired separation line 104 on the surface 130 of the strengthened display glass 100 and within the elliptical spot 102. More specifically, the nozzle 160 of the illustrated embodiment is positioned so that the cooling spot 106 is between the center of the elliptical spot 102 and the trailing edge 122, such that the cooling spot is spaced a distance z from the trailing edge, such as Figure 3 As shown. At this position, the cooling spot 106 is located at or near the highest temperature on the surface of the strengthened display glass due to the heating of the laser source. Therefore, due to the quenching of the strengthened display glass by the cooling jet at or near the highest temperature, the resulting temperature change ΔT (assuming that the glass surface is heated to just below the strain temperature Tg) exceeds the temperature change threshold ΔTTH, thereby facilitating the formation of a channel 109 that propagates from the defect 112. Although the cooling spot is shown to be located within the elliptical spot and separated from the trailing edge by a certain distance z, the cooling spot can also be located on the trailing edge 122, or partially located outside the elliptical spot near the trailing edge, or a few millimeters behind the elliptical spot. For example, for thicker strengthened display glass, the cooling spot can be positioned closer to or within the elliptical spot. For thinner strengthened display glass, the cooling spot can be positioned within the elliptical spot. Generally, the thinner the strengthened display glass, the shorter the distance of the cooling jet to the highest temperature position.

[0068] refer to Figure 1(a) , 25. After the cooling jet 105 and the cooling spot 106 are properly aligned with the elliptical spot 102, the cooling jet and the laser source are advanced along the surface 130 of the strengthened display glass 100 from the defect 112 to the end position 113 on the desired separation line 104 in the scratching direction 110. When the surface of the strengthened display glass is heated to the maximum temperature and quenched at or near the maximum temperature, the scratch channel 109 is propagated along the desired separation line 104 from the defect 112 to the end position 113. The cooling jet / laser source and the strengthened display glass 100 are relatively moved to advance at a scratching speed v, which in turn is also the speed at which the channel propagates along the desired separation line 104. The scratching speed v is generally selected to avoid overheating the surface of the strengthened display glass while still allowing the surface of the strengthened display glass to be heated to just below the strain temperature of the glass. Ensuring that the scratch channel 109 extends between the defect and the end position, rather than from the first edge to the second edge, can prevent uncontrollable full-body channel propagation and damage to the strengthened display glass 100. After the scratch channel 109 is formed, a bending moment may be applied (eg, manually) to the strengthened display glass 100 on one or both sides of the channel to mechanically separate the strengthened display glass along the scratch channel 109 .

[0069] In one embodiment, the system can be operated so that the beam spot advances along the desired separation line starting before the first edge and continuing after the second edge so that the beam spot crosses the first and second edges. In order to create a scratch channel that is only located between the defect and the end point, and does not extend from the first edge to the second edge, the cooling jet can be operated in an "off" mode when the beam spot is generated by the laser beam and incident on the strengthened display glass before the defect and after the end position, and the cooling jet can be operated in an "on" mode when the beam spot is incident on the strengthened display glass on the defect and between the defect and the end position. Therefore, the cooling spot is only provided on the surface of the strengthened display glass from the defect to the end position. Operating the cooling jet in this manner can prevent the strengthened display glass before the defect and after the end position from being quenched, thereby preventing the channel from opening at these locations and causing the scratch channel to extend from the defect to the end position.

[0070] In another embodiment, the cooling jet can be operated in a continuous on mode to provide a cooling spot on the surface of the strengthened display glass from the first edge to the second edge. In this embodiment, the laser source can be operated at a low power level when the laser beam is incident on the strengthened display glass before the defect and after the termination position, and operated at a high power level when the laser beam is incident on the strengthened display glass between the defect and the termination position. The low power level may be an off mode (i.e., zero radiation), or a power level low enough that the laser beam does not heat the strengthened display glass to a temperature sufficient to open the channel. The high power level may be a power level capable of opening the channel as described above. Operating the laser source in this manner can provide controlled channel propagation between the defect and the termination position, rather than at the edge of the strengthened display glass.

[0071] Preventing the channel from extending past the end position in the direction of the second edge may also be achieved by increasing the power level of the laser source as it approaches the end position. In a laser scribing operation, the laser-generated channel typically propagates at the relative speed of the laser beam and the cooling jet relative to the strengthened display glass. However, increasing the laser power of the laser source may cause the channel to exceed the translation speed of the strengthened display glass, causing the channel to propagate into the laser heating region provided by the laser beam spot. When the front end 140 of the channel enters the laser heating region, it is quenched and stops propagating due to the combined effect of the increased power of the laser source and the cooling jet. Therefore, by increasing the power of the laser source as it approaches the end position, the propagation of the channel may be stopped in a controlled manner.

[0072] In addition, preventing the channel from opening between the first edge and the defect and between the end position and the second edge can also be achieved by translating the strengthened display glass at a high speed when the laser beam is between the first edge and the defect and between the end position and the second edge, and translating at a low speed when the laser beam is between the defect and the end position. This can be described as a speed profile of the relative motion between the strengthened display glass and the laser beam. The high speed should be the glass translation speed fast enough to prevent the channel from opening, and the low speed should be the glass translation speed enough to open the channel to form a scratch channel (i.e., the scratch speed v). By speeding up the glass translation speed before the defect and after the end point, the scratch channel may only be formed between the defect and the end position.

[0073] By precisely controlling the time and position of laser heating and cooling quenching, as well as the power of the laser source and the translation speed of the strengthened display glass, it is possible to ensure that the scratch channel is formed only between the defect and the termination position, thereby achieving precise segmentation of the strengthened display glass. This control method allows the precise separation of the strengthened display glass without affecting the unscratched area, ensuring the neatness of the scratch channel and the quality of the segmentation surface.

[0074] refer to Figure 6, the method embodiments described herein may also use laser shields 141, 142 to prevent beam spots and cooling points from reaching the surface of the strengthened display glass in shielded areas located around the edge of the strengthened display glass and between the edge of the display glass and the respective defects and end positions. For example, a shielded area may extend from the defect 112 to the first edge 114 and from the end position 113 to the second edge 116. The laser shields 141, 142 may include, for example, a metal material that is capable of preventing laser radiation from entering and heating the strengthened display glass within the shielded area. Figure 6 In the embodiment shown in , the first laser shield 141 is configured to be applicable to the first edge 114 of the strengthened display glass 100, so that the first protective surface 141 covers the first shielding area. Similarly, the second laser shield 142 is configured to be applicable to the second edge 116 of the strengthened display glass 100, so that the second protective surface 143 covers the second shielding area. It should be understood that other laser shield configurations can be used. For example, the laser shield can be configured as a flat metal sheet attached to the strengthened display glass 100 (e.g., shielding only the top surface of the strengthened display glass at the first edge and the second edge). As the strengthened display glass translates relative to the beam spot and the cooling jet, the laser shields 141, 142 prevent the channel from opening in the first and second shielding areas, thereby allowing the scratch channel to extend from the defect to the termination point.

[0075] In another embodiment, a thin thermally conductive coating can be deposited on the edge of the strengthened display glass 100 as a laser shield. For example, the thin thermally conductive coating can be a metal electrode material commonly used to form contacts on touch sensitive screens. The thermally conductive coating can be applied to the strengthened display glass 100 using a mask. This material can also provide the heat shielding effect described above.

[0076] The method described above can be used to form one or more channels in a strengthened display glass so that such strengthened display glass can be separated into multiple smaller segments using scratch and break techniques. For example, Figure 7-11 A method of segmenting strengthened display glass 100 into a plurality of segments using the channel forming methods described herein is graphically depicted.

[0077] refer to Figure 7, a piece of strengthened display glass 100 having an upper or first surface 130 is shown. As described above, the strengthened display glass 100 is separated into a plurality of segments by introducing a first vertical defect 112a on the first surface 130 at an offset relative to the first edge 114. The first vertical defect 112a can be formed on the surface of the strengthened display glass 100 using a mechanical scribing tool (e.g., a diamond tip or carbide point or wheel) or by laser ablation. Additional vertical defects, such as a second vertical defect 112b and a third vertical defect 112c, can also be introduced on the first surface 130 to create additional scratch channels, thereby enabling the strengthened display glass 100 to be separated into a plurality of segments. Any number of additional defects can be introduced on the first surface 130.

[0078] A channel can then be opened in the strengthened display glass 100 along a first desired separation line 104a, extending from the first vertical defect 112a to the first end position 113a, using one or more of the channel forming techniques described above. For example, in one embodiment, an elliptical spot of a CO2 laser is directed onto the first vertical defect 112a such that the major axis of the elliptical spot is substantially aligned with the first desired separation line 104a. A cooling jet is also directed onto the strengthened display glass such that the cooling point of the cooling jet is located near the trailing edge of the spot.

[0079] The elliptical light spot and the cooling spot are then directed along the first desired separation line 104a on the surface of the strengthened display glass, thereby opening a first channel in the strengthened display glass that partially passes through the thickness of the strengthened display glass and forms a first scratch channel, as described above. Generally speaking, the first channel in the strengthened display glass 100 usually passes through less than a quarter of the thickness h of the strengthened display glass.

[0080] Similarly, a second scratch channel can be formed along the second desired separation line 104b starting from the second vertical defect 112b and terminating at the second termination position 113b, and a third scratch channel can be formed along the third desired separation line 104c starting from the third vertical defect 112c and terminating at the third termination position 113c, as described above with respect to the formation process of the first scratch channel.

[0081] After forming the first, second, and third scratch channels in the strengthened display glass 100, the strengthened display glass can be mechanically divided into a plurality of segments along the scratch channels by applying a bending moment to the strengthened display glass. For example, once the strengthened display glass is divided along the first scratch channel by applying a bending moment to the strengthened display glass 100, the resulting segment can be further divided into smaller segments by applying a bending moment to the second and third scratch channels. In this way, the strengthened display glass 100 can be divided into four independent segments. It should be understood that more or fewer scratch channels can be formed to divide the strengthened display glass into more or fewer independent segments.

[0082] The methods of forming the scratch channels described herein can also be used to cross-scratch a strengthened display glass. To cross-scratch a strengthened display glass, two intersecting scratch channels can be formed inside the strengthened display glass. Laser cross-scratching includes laser scribing in one direction and then laser scribing in a second direction.

[0083] refer to Figure 8 , a first vertical defect 112a can be introduced near the first edge 114, and a second vertical defect 112b can be introduced near the third edge 117. The first and second vertical defects 112a, 112b are located on the first and second desired separation lines 104a, 104b, respectively. The first and second desired separation lines 104a, 104b intersect at the intersection location 170. As described above, the laser beam and the cooling jet can be translated on the surface of the strengthened display glass 100 to open the scratch channels 109a and 109b, which terminate at the first and second termination locations 113a and 113b, respectively, as shown in FIG. Fig. 9 As shown. The first and second end positions 113a and 113b are near the second and fourth edges 116 and 119, respectively. Although the strengthened display glass 100 is shown as a square configuration, other configurations are possible, such as a circular configuration. In such a circular configuration, there may not be clear edges such as the first, second, third, and fourth edges. The edges are defined as the first, second, third, and fourth edges for ease of discussion and are not intended to be limiting.

[0084] refer to Fig. 9 , the cross-scratching of the display glass requires that the second scratch channel 109b passes through the first scratch channel 109a at the intersection position 170 during the second laser scratching process. Due to the discontinuity at the first scratch channel 109a formed during the first scratching process, the local display glass temperature at the intersection position 170 during the second scratching process is higher than other areas along the second desired separation line 104b. Because the temperature at the intersection position 170 is higher, the second channel 109b will pass through the first scratch channel 109a at the intersection and penetrate into the internal tensile stress layer. This results in the channel front end 140 ( Figure 4The higher temperature and local thermal expansion at the intersection location 170 may cause the channel to grow deeper near the intersection location 170 than other areas along the second desired separation line 104b.

[0085] By this method, cross-scratching channels can be formed in the strengthened display glass, which allows the display glass to be subsequently separated into multiple independent parts along the cross-scratching channels by applying external force (e.g., by manual bending). By laser cross-scratching, complex segmentation patterns can be achieved, so that the strengthened display glass can be precisely separated into fragments of various shapes and sizes as needed.

[0086] These methods offer flexibility in manufacturing and designing glass parts, especially in the production of safety glass or decorative glass products that require precise dimensions. In addition, these techniques can be applied to the manufacture of smartphones, tablets, TV screens and other glass products where precise dimensions and smooth cut edges are critical. Laser scribing and cooling techniques offer a relatively simple and controllable method to manufacture these high-quality glass products.

[0087] Fig. 10A Schematically shows a cross-sectional view of a first scored channel 109a formed in a 1.1 mm thick aluminosilicate display glass chemically strengthened by an ion exchange process. The depth of the compressive stress layer is about 34 microns and the compressive stress is about 620 MPa. The internal tension layer has a central tension of about 21 MPa. Fig. 10A The first scored channel 109a shown in the figure was generated by using a CO2 laser beam operating at a frequency of 20 kHz, a duty cycle of 18% and an output power of 182 watts. The laser beam and the cooling jet were translated at a scoring speed of 162 mm / sec. The CO2 laser beam generated an elliptical spot with a length a of 42 mm and a width b of 2.5 mm. The cooling jet was water flowing at a flow rate of 16 standard cubic centimeters per minute. The first scored channel 109a thus generated had a channel depth di of about 155 microns.

[0088] Fig. 10B A cross-sectional view of a second score channel 109b' generated by the same scribing process as the first score channel 109a is shown. The location of the first score channel 109a is indicated by the arrow labeled 109a. The schematic diagram shows the reinforced display glass being mechanically broken first along the second score channel 109b'. Therefore, the first score channel 109a is illustrated as entering and exiting the paper. The second score channel 109b' has a channel depth d2' of approximately 158 microns in the area except for the intersection location 170'. However, the second score channel 109b' passes through the first score channel 109a below the intersection location 170', and its channel depth d2' at the intersection location 170' is approximately 175 microns.

[0089] In one embodiment, by increasing the scribing speed during the second scribing process so that the scribing speed of the second scribing process is greater than the scribing speed of the first scribing process, the channel depth d2i at the intersection position 170 can be minimized. When the second score channel 109b intersects the first score channel 109a at the intersection position 170, the channel depth dai of the second score channel 109b at the intersection position 170 can be similar to the channel depth di of the first score channel 109a.

[0090] Fig. 10C An example of the intersection of the scribe channels 109a and 109b is shown, where the scribe speed of the second scribe process is greater than the scribe speed of the first scribe process. The first scribe channel 109a is generated as described above, and its location is indicated by the arrow labeled 109a. In this example, the scribe speed of the second scribe process is about 172 mm / sec. Due to the higher scribe speed, the channel depth d2 of the second scribe channel 109b in the area outside the intersection location 170 is about 143 microns. Fig. 10C As shown, the channel depth dai of the second scribe channel 109b at the intersection position 170 is about 154 microns, which is smaller than the channel depth di of the first scribe channel 109a, which is 155 microns. Therefore, uncontrolled whole body separation at the intersection position 170 can be avoided by the shallower channel depth dai of the second scribe channel 109b at the intersection position 170.

[0091] In another embodiment, the channel depth dai of the second scribe channel 109b at the intersection location 170 may be minimized by first fusing the first scribe channel 109a at the intersection location 170 and then creating the second scribe channel 109b. By fusing the first scribe channel 109a, the second channel 109b may have less disturbance at the intersection location 170 during the second scribing process.

[0092] The first scribed channel 109a can be welded at the intersection location 170 by generating a channel preparation line during the channel preparation process of the laser beam and the cooling jet. The channel preparation line can be aligned with the second desired separation line 104b (eg, Figure 8 The laser beam and the cooling jet are aligned with each other (as shown) so that the laser beam and the cooling jet will follow the same path when forming the second scribe channel 109b. The movement speed of the laser beam and the cooling jet during the channel preparation process is greater than the scribing speed of the first and second scribing processes. For example, in one embodiment, the movement speed during the channel preparation process may be 10% or more faster than the scribing speed of the first and second scribing processes.

[0093] Due to the discontinuity created by the first scribe channel 109a at the intersection location 170, the glass material may be overheated at the intersection location 170 during the channel preparation process, thereby softening or melting the glass material. In this way, the first scribe channel 109a may be fused at the intersection location 170. The laser beam and cooling jet may be operated only at the intersection location(s) during the channel preparation process, or may be operated continuously on the second desired separation line 104b. The channel preparation process may be performed by the laser beam that creates the first and / or second scribe channels, or by using a separate laser beam.

[0094] After the channel preparation process is completed, the second scribe channel 109b can be formed using the same laser scribing process as the first scribe channel 109a. The second scribe channel 109b will pass through the first scribe channel 109a that is fused or closed at the intersection position 170. The channel preparation process can minimize the channel depth d2i of the second scribe channel 109b at the intersection position to reduce the occurrence of overall separation.

[0095] As an example but not limited thereto, a chemically strengthened aluminosilicate display glass having a compressive stress of about 625 MPa in a 36 micron deep compressive stress layer (layer depth) and a central tension of about 21 MPa was separated using the above-described channel preparation process method. The size of the strengthened display glass was 370 mm by 470 mm. The CO2 laser was operated at a frequency of 20 kHz, a duty cycle of 18%, and a laser power of 181 W. The laser beam was configured to produce an elliptical spot with a length of 41 mm and a width of 2.5 mm. The cooling jet was a water jet generated by a nozzle with a 150 micron diameter and a flow rate of 14 sccm. The scribing speed of the first scribing process was 162 mm / sec. A channel preparation process was performed before the second scribing process to generate a channel preparation line. The movement speed of the laser beam and the cooling jet during the channel preparation process was 180 mm / sec. After the channel preparation process, a second scribing channel was generated in a second scribing process, wherein the scribing speed of the second scribing process was 162 mm / sec. The tempered display glass was successfully cross-hatched.

[0096] Reference now Fig.11, a plurality of intersecting scribing channels can be formed in the strengthened display glass. Vertical edge defects (112d-112f) can be formed on the third edge 117 of the strengthened display glass to form a second set of scribing channels that intersect with the first set of scribing channels, the first set of scribing channels including the first, second and third scribing channels described above, respectively, at intersections 170a-170i. It should be understood that the first and second sets of scribing channels can include any number of scribing channels. A fourth defect 112d, a fifth defect 112e and a sixth defect 112f can be formed that are offset from the third edge 117. As described above, the defects can be formed by mechanical scribing or laser ablation, for example. Defects 112d-112f can be located and perpendicular to the fourth, fifth and sixth desired separation lines 104d-f, which intersect the first, second and third desired separation lines 104a-c that intersect at intersection locations 170a-i. Although the fourth, fifth and sixth desired separation lines 104d-f are depicted as being perpendicular to the first, second and third desired separation lines 104a-c, embodiments are not limited thereto. For example, the desired separation lines may be inclined or curved to create separated glass

[0097] The fourth, fifth and sixth scribe lanes may be generated between the fourth, fifth and sixth defects 112d-f and the fourth, fifth and sixth termination locations 113d-f.

[0098] The first and second groups of scribing channels can be formed according to the above-mentioned cross-scribing method. For example, the first group of scribing channels (i.e., the first, second, and third scribing channels) can be formed according to the above-mentioned method. After the first group of scribing channels are formed, the second group of scribing channels (i.e., the fourth, fifth, and sixth scribing channels) can be formed by a second scribing process with a scribing speed faster than the scribing speed of the first scribing process. In another embodiment, a channel preparation process can be used before forming the second group of scribing channels. A single laser beam and cooling jet can be used to form each scribing channel, or multiple laser beams and cooling jets can be used. For example, the number of laser beams and cooling jets can be equal to the desired number of scribing channels, so that each scribing channel is formed by a corresponding laser beam and cooling jet.

[0099] The methods described herein can be used to separate strengthened display glass, such as strengthened display glass made of borosilicate glass, and strengthened display glass made of aluminosilicate glass, including ion exchange strengthened aluminosilicate glass. The methods described herein allow the strengthened display glass to be separated by a scoring and breaking process, wherein a scoring channel is formed on the surface of the display glass, and the channel does not contact the edge of the display glass. The strengthened display glass applied with the scoring channel described herein can be separated by applying a force along the scoring channel. The methods described herein also allow the strengthened display glass to be cross-scored by forming intersecting scoring channels.

[0100] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A method for forming a scratch channel and separating a strengthened display glass, characterized in that: include: forming a vertical defect by compressing the surface layer such that the defect is offset from the first edge of the strengthened display glass; The exposed internal tensile stress layer beneath the compressive layer of glass helps initiate channels during laser scratching; directing a beam spot of a laser source onto the compression layer along the desired separation line, and directing a cooling spot generated by a cooling nozzle onto the compression layer such that the cooling spot is located near a trailing edge of the beam spot; By translating the laser source and the cooling nozzle, or by translating the strengthened display glass, the cooling point and the beam spot are advanced along the desired separation line until the beam spot is positioned at a termination position deviating from the second edge of the strengthened display glass, thereby forming a channel that partially passes through the thickness of the strengthened glass, and the formed scratch channel extends from the deviated defect to the termination position, thereby achieving precise separation of the strengthened display glass; The intersecting score channels are formed by forming a first score channel at a first score speed and forming an intersecting second score channel at a second score speed greater than the first score speed.

2. The method for forming a scratch channel and separating a strengthened display glass as claimed in claim 1, characterized in that: The strengthened display glass may be composed of various glasses, including one or more of borosilicate glass, aluminosilicate glass and aluminoborosilicate glass, and may be firmly held within the system by using a mechanical or vacuum suction cup, which may be achieved by a series of vacuum holes spaced a certain distance apart on a vacuum plate.

3. The method for forming a scratch channel and separating a strengthened display glass as claimed in claim 1, characterized in that: The cooling jet typically includes a pressurized fluid ejected from a nozzle and directed onto the surface of the strengthened display glass, the cooling jet including one of compressed air, compressed nitrogen, compressed helium or similar compressed gases, or a mixture of liquid and compressed gas, wherein the mixture of liquid and compressed gas is a mist gas mixture of one of compressed deionized water, air and nitrogen.

4. The method for forming a scratch channel and separating a strengthened display glass as claimed in claim 1, characterized in that: By controlling the width and length of the beam spot, the heating effect of the laser beam on the strengthened display glass can be adjusted, thereby controlling the depth and formation process of the channel.

5. The method for forming a scratch channel and separating a strengthened display glass as claimed in claim 1, characterized in that: The defect is mechanically formed by applying a diamond scriber, and the defect depth is not less than the layer depth.

6. The method for forming a scratch channel and separating a strengthened display glass as claimed in claim 1, characterized in that: In order to form the scratch channel on the surface of the strengthened display glass, it is necessary to cool or quench the heated strengthened display glass surface using a cooling jet emitted from a nozzle.

7. The method for forming a scratch channel and separating a strengthened display glass as claimed in claim 1, wherein: The strengthened glass includes strengthened display glass made of borosilicate glass, strengthened display glass made of aluminosilicate glass and ion exchange strengthened aluminosilicate glass.

Citation Information

Patent Citations

  • Methods for laser scribing and breaking thin glass

    CN102574722A

  • Methods for laser scribing and separating glass substrates

    CN102741179A

  • Methods of separating strengthened glass substrates

    CN103097313A

  • Methods of cutting glass using a laser

    CN104736489A