Vacuum glass sealing material with low thermal conductivity and preparation method thereof

By using metal powder, glass powder, organic solvent and other components in vacuum glass sealing materials, low thermal conductivity vacuum glass sealing materials are prepared, which solves the problem of high-temperature processing affecting the stickiness effect, and achieves low thermal conductivity and stability of the material. Suitable for a variety of industrial applications.

CN118930074APending Publication Date: 2024-11-12JIANGSU BAIFU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410890109.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The structure of the existing vacuum glass sealing materials is relatively simple, mainly through high-temperature processing, which leads to the transmission of higher temperatures and interferes with the sticking effect and affects the material packaging effect.

Method used

Using low heat conductivity vacuum glass sealing materials, its components include metal powder, glass powder, organic solvents, thickeners, thixotropic agents and surfactants, prepared, mixed and added, adjusted properties, dried, post-treatment and Prepare by stirring and other steps, using ingredients such as ethyl acetate and vegetable glue to reduce thermal conductivity.

Benefits of technology

It achieves low thermal conductivity, improves the stability and thermal insulation performance of vacuum glass sealing materials, has good biocompatibility and degradability, and is suitable for various industrial fields and friendly environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a vacuum glass sealing material with low thermal conductivity and a preparation method thereof. The vacuum glass sealing material with low thermal conductivity comprises the following main components: metal powder, glass powder, an organic solvent, a thickening agent, a thixotropic agent and a surfactant. The ethyl acetate is selected, so that the vacuum glass sealing material has relatively low heat-conducting property at normal temperature, and meanwhile, the vacuum glass sealing material has relatively high thickening effect and stability, is widely applied to various industrial fields, has good biocompatibility and degradability, is environment-friendly, and can be widely applied to various industrial fields. The copper-nickel alloy powder plays a key role in improving the heat insulation performance of the vacuum glass, the copper-nickel alloy powder can remarkably reduce the heat conduction performance of the vacuum glass by adjusting the nickel content, so that the copper-nickel alloy powder is also low-heat-conduction metal powder, and the copper-based composite material powder is prepared by adding ceramic or other low-heat-conduction materials into a copper matrix. And low heat conduction performance can also be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vacuum glass sealing materials, and in particular to a vacuum glass sealing material with low thermal conductivity and a preparation method thereof. Background Art

[0002] The selection of vacuum glass sealing materials is crucial to ensure the stability and sealing of glass. In the field of vacuum glass sealing, hot-melt butyl adhesive and two-component polysulfide adhesive or silicone sealant are also commonly used for vacuum glass sealing. These materials can provide reliable connection and support functions, and have corrosion resistance and stability. The selection of vacuum glass sealing materials needs to be based on specific application requirements and working environment to ensure that they can meet the sealing and stability requirements of vacuum glass. At the same time, during use, attention should also be paid to factors such as material matching, heat treatment during processing, and airtightness inspection to ensure that the sealing quality reaches the best state.

[0003] For example, the patent number disclosed in the China Patent Network is: 200910046493.1, and the patent name is: A high-temperature resistant sealing material for a dense oxygen-permeable ceramic membrane, especially a high-temperature sealing material between a dense oxygen-permeable ceramic membrane and its supporting components, and its application under high temperature conditions, belonging to the technical field of special ceramic bonding materials. The high-temperature resistant sealing material for a dense oxygen-permeable ceramic membrane in the method of the present invention has the following composition and its weight percentage: 55-65% ceramic material base material, 25-35% heat-resistant Pyres glass powder, and flux B2O3 or Li2O 4-6%, wetting agent NaAlO2 or NaSiO3 4-6%, the above four raw materials are weighed and mixed according to the formula, the mixed material is smelted in a high-temperature furnace at a temperature of 1150-1250°C for 20-40 minutes to melt it, and then cooled to room temperature, the frit is taken out, and the frit is ground and crushed to obtain a high-temperature resistant sealing material powder. The sealing material prepared by the method of the present invention has high sealing tightness, will not leak at high temperature, and has good stability to the dense oxygen-permeable ceramic membrane.

[0004] However, the structure of existing sealing materials is relatively simple, and they are mainly processed through high-temperature processing. The high temperature transmitted during the processing will cause the glass to be affected, interfere with the adhesion effect, and affect the material packaging effect.

[0005] Therefore, it is necessary to design and modify the low thermal conductivity vacuum glass sealing material and the preparation method thereof. Summary of the invention

[0006] In order to solve the problems raised in the above-mentioned background technology, the purpose of the present invention is to provide a low thermal conductivity vacuum glass sealing material and a preparation method thereof, which has the advantage of reducing thermal conductivity and solves the problem that the structure of the existing sealing materials is relatively simple and is mainly processed by high-temperature processing. The higher temperature transmitted during the processing will cause the glass to be affected, interfere with the adhesion effect, and affect the material packaging effect.

[0007] To achieve the above objectives, the present invention provides the following technical solutions: a low thermal conductivity vacuum glass sealing material and a preparation method thereof, wherein the main components of the low thermal conductivity vacuum glass sealing material are: metal powder, glass powder, organic solvent, thickener, thixotropic agent, and surfactant.

[0008] As preferred embodiment of the present invention, the metal powder is composed of mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder, the glass powder is composed of lead oxide, silicon dioxide and boron oxide, the organic solvent is ethyl acetate, the thickener is composed of plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite, the thixotropic agent is composed of a thermosensitive thixotropic agent and an electrosensitive thixotropic agent, and the surfactant is composed of a fluorocarbon surfactant and a polymer surfactant.

[0009] As preferred embodiment of the present invention, based on every 100g of low thermal conductivity vacuum glass sealing material, the content of each component is: mixed silver powder 0.1-0.2g, copper-nickel alloy powder 0.1-0.2g, aluminum-silicon alloy powder 0.1-0.2g, stainless steel powder 0.1-0.2g, lead oxide 0.1-0.2g, silicon dioxide 0.1-0.2g, boron oxide 0.1-0.2g, plant glue 0.1-0.2g, animal glue 0.1-0.2g, microbial polysaccharide 0.1-0.2g, magnesium aluminum silicate 0.1-0.2g, bentonite 0.1-0.2g, thermosensitive thixotropic agent 0.1-0.2g, electrosensitive thixotropic agent 0.1-0.2g, fluorocarbon surfactant 0.1-0.2g, polymer surfactant 0.1-0.2g, and ethyl acetate is used to make up to 100g.

[0010] A low thermal conductivity vacuum glass sealing material and a preparation method thereof, comprising the steps of a) powder preparation; b) mixing and adding; c) performance adjustment; d) drying; e) post-treatment; and f) stirring:

[0011] Step a) powder preparation: taking appropriate amounts of metallic silver, copper-nickel alloy, aluminum-silicon alloy and stainless steel, crushing them by pulverizing, and then grinding and powdering them to obtain mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder;

[0012] Step b) mixing and adding: mixing silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder according to the components and proportions, using ethyl acetate as an auxiliary agent, mixing in a blender and sequentially adding lead oxide, silicon dioxide and boron oxide materials during the mixing process, thereby obtaining a basic sealing material;

[0013] Step c) adjusting the performance: placing the thermosensitive thixotropic agent, the electrosensitive thixotropic agent, the fluorocarbon surfactant and the polymer surfactant into the interior of the sealing basic material in sequence according to the components and proportions.

[0014] Step d) drying: drying the material to volatilize the ethyl acetate inside it;

[0015] Step e) post-treatment: firstly, the plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite are stirred to form a jelly, and then the dried basic sealing material is added into the jelly.

[0016] Step f) stirring: using a crusher to stir the colloid and the basic sealing material, and after the mixture is evenly mixed, a low thermal conductivity vacuum glass sealing material is obtained.

[0017] As a preferred embodiment of the present invention, the step b) mixing and adding is carried out by a mixer corner plate for 2-4 hours, and the mixture is heated to 300 degrees by pre-burning during the stirring process, and lead oxide, silicon dioxide, and boron oxide materials are added during the stirring process, and the addition interval is greater than 5 minutes.

[0018] As a preferred embodiment of the present invention, in step d) drying, the material is purged by a hot air blower to volatilize the ethyl acetate inside the material, and the drying process is completed when the humidity inside the sealing basic material is less than 5%.

[0019] As a preferred method of the present invention, the post-treatment in step e) is to mix the plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite according to the components and proportions, and to perform an emulsification reaction in a reactor during the mixing process.

[0020] As a preferred embodiment of the present invention, in step f), the colloid and the basic sealing material are put into the shearing machine with stirring, and the temperature is raised to 500 degrees at a rate of 1-8°C / minute at first slowly and then quickly, and then raised to 500-800 degrees after being kept warm for 2 hours, and then cooled to 200 degrees at a rate of 1-8°C / minute at first slowly and then quickly, and then naturally cooled to room temperature.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention selects ethyl acetate, which has relatively low thermal conductivity at room temperature, and can make the vacuum glass sealing material have high thickening effect and stability, and is widely used in various industrial fields, has good biocompatibility and degradability, and is environmentally friendly. By setting mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder, the vacuum glass sealing material can have good electrical conductivity and thermal conductivity, which plays a key role in improving the thermal insulation performance of vacuum glass. The thermal conductivity of aluminum-silicon alloy powder is lower than that of pure aluminum, so aluminum-silicon alloy powder is also one of low thermal conductivity metal powders. The thermal conductivity of copper-nickel alloy powder can be significantly reduced by adjusting the nickel content, so copper-nickel alloy powder is also a low thermal conductivity metal powder. The copper-based composite material powder is a composite material powder made by adding ceramic or other low thermal conductivity materials into a copper matrix, and low thermal conductivity can also be achieved. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The present invention provides a low thermal conductivity vacuum glass sealing material and a preparation method thereof. The main components of the low thermal conductivity vacuum glass sealing material are: metal powder, glass powder, organic solvent, thickener, thixotropic agent and surfactant.

[0025] As a technical optimization scheme of the present invention, the metal powder is composed of mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder, the glass powder is composed of lead oxide, silicon dioxide and boron oxide, the organic solvent is ethyl acetate, the thickener is composed of plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite, the thixotropic agent is composed of a thermosensitive thixotropic agent and an electrosensitive thixotropic agent, and the surfactant is composed of a fluorocarbon surfactant and a polymer surfactant.

[0026] As a technical optimization scheme of the present invention, based on every 100g of low thermal conductivity vacuum glass sealing material, the content of each component is: mixed silver powder 0.1-0.2g, copper-nickel alloy powder 0.1-0.2g, aluminum-silicon alloy powder 0.1-0.2g, stainless steel powder 0.1-0.2g, lead oxide 0.1-0.2g, silicon dioxide 0.1-0.2g, boron oxide 0.1-0.2g, plant glue 0.1-0.2g, animal glue 0.1-0.2g, microbial polysaccharide 0.1-0.2g, magnesium aluminum silicate 0.1-0.2g, bentonite 0.1-0.2g, thermosensitive thixotropic agent 0.1-0.2g, electrosensitive thixotropic agent 0.1-0.2g, fluorocarbon surfactant 0.1-0.2g, polymer surfactant 0.1-0.2g, and ethyl acetate is used to make up to 100g.

[0027] A low thermal conductivity vacuum glass sealing material and a preparation method thereof, comprising the steps of a) powder preparation; b) mixing and adding; c) performance adjustment; d) drying; e) post-treatment; and f) stirring:

[0028] Step a) powder preparation: taking appropriate amounts of metallic silver, copper-nickel alloy, aluminum-silicon alloy and stainless steel, crushing them by pulverizing, and then grinding and powdering them to obtain mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder;

[0029] Step b) mixing and adding: mixing silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder according to the components and proportions, using ethyl acetate as an auxiliary agent, mixing in a blender and sequentially adding lead oxide, silicon dioxide and boron oxide materials during the mixing process, thereby obtaining a basic sealing material;

[0030] Step c) adjusting the performance: placing the thermosensitive thixotropic agent, the electrosensitive thixotropic agent, the fluorocarbon surfactant and the polymer surfactant into the interior of the sealing basic material in sequence according to the components and proportions.

[0031] Step d) drying: drying the material to volatilize the ethyl acetate inside it;

[0032] Step e) post-treatment: firstly, the plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite are stirred to form a jelly, and then the dried basic sealing material is added into the jelly.

[0033] Step f) stirring: using a crusher to stir the colloid and the basic sealing material, and after the mixture is evenly mixed, a low thermal conductivity vacuum glass sealing material is obtained.

[0034] As a technical optimization scheme of the present invention, through step b) mixing and adding, the angle plate of the mixer is used for 2-4 hours, and the mixture is heated to 300 degrees by pre-burning during the stirring process, and lead oxide, silicon dioxide, and boron oxide materials are added during the stirring process, and the addition interval time is greater than 5 minutes.

[0035] As a technical optimization scheme of the present invention, through step d) drying, the material is blown through by a hot air blower to volatilize the ethyl acetate inside, and the drying process is completed when the humidity inside the sealing basic material is less than 5%.

[0036] As a technical optimization scheme of the present invention, through step e) post-treatment, the plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite are mixed according to the components and proportions, and an emulsification reaction is carried out in a reactor during the mixing process.

[0037] As a technical optimization scheme of the present invention, through step f) stirring, the colloid and the basic sealing material are put into the inside of the shearing machine, and the temperature is raised to 500 degrees at a rate of 1-8°C / minute at a slow speed first and then a fast speed. After keeping warm for 2 hours, the temperature is raised to 500-800 degrees, and then the temperature is lowered to 200 degrees at a rate of 1-8°C / minute at a slow speed first and then a fast speed, and then naturally cooled to room temperature.

[0038] First embodiment: Based on every 100g of low thermal conductivity vacuum glass sealing material, the contents of the various components are as follows: 20g of mixed silver powder, 20g of copper-nickel alloy powder, 20g of aluminum-silicon alloy powder, 10g of stainless steel powder, 3g of lead oxide, 4g of silicon dioxide, 3g of boron oxide, 5g of plant glue, 8g of animal glue, 3g of microbial polysaccharide, 3g of magnesium aluminum silicate, 3g of bentonite, 3g of thermosensitive thixotropic agent, 3g of electrosensitive thixotropic agent, 3g of fluorocarbon surfactant, 8g of polymer surfactant, and supplemented with ethyl acetate to make up to 100g.

[0039] Second embodiment: Based on every 100g of low thermal conductivity vacuum glass sealing material, the contents of the various components are as follows: 10g of mixed silver powder, 10g of copper-nickel alloy powder, 20g of aluminum-silicon alloy powder, 5g of stainless steel powder, 3g of lead oxide, 4g of silicon dioxide, 3g of boron oxide, 5g of plant glue, 8g of animal glue, 3g of microbial polysaccharide, 3g of magnesium aluminum silicate, 3g of bentonite, 3g of thermosensitive thixotropic agent, 3g of electrosensitive thixotropic agent, 3g of fluorocarbon surfactant, 5g of polymer surfactant, and supplemented with ethyl acetate to make up to 100g.

[0040] In summary: the low thermal conductivity vacuum glass sealing material and the preparation method thereof, by selecting ethyl acetate, have relatively low thermal conductivity at room temperature, and at the same time can make the vacuum glass sealing material have high thickening effect and stability, and are widely used in various industrial fields, have good biocompatibility and degradability, and are environmentally friendly. By setting mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder, the vacuum glass sealing material can have good electrical conductivity and thermal conductivity, which plays a key role in improving the thermal insulation performance of vacuum glass. The thermal conductivity of aluminum-silicon alloy powder is lower than that of pure aluminum, so aluminum-silicon alloy powder is also one of the low thermal conductivity metal powders. The thermal conductivity of copper-nickel alloy powder can be significantly reduced by adjusting the nickel content, so copper-nickel alloy powder is also a low thermal conductivity metal powder. Copper-based composite material powder is a composite material powder made by adding ceramic or other low thermal conductivity materials into a copper matrix, and low thermal conductivity can also be achieved.

[0041] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0042] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A low thermal conductivity vacuum glass sealing material and a preparation method thereof, characterized in that: The main components of the low thermal conductivity vacuum glass sealing material are: metal powder, glass powder, organic solvent, thickener, thixotropic agent and surfactant.

2. The low thermal conductivity vacuum glass sealing material and preparation method thereof according to claim 1, characterized in that: The metal powder is composed of mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder, the glass powder is composed of lead oxide, silicon dioxide and boron oxide, the organic solvent is ethyl acetate, the thickener is composed of plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite, the thixotropic agent is composed of a thermosensitive thixotropic agent and an electrosensitive thixotropic agent, and the surfactant is composed of a fluorocarbon surfactant and a polymer surfactant.

3. The low thermal conductivity vacuum glass sealing material and preparation method thereof according to claim 1, characterized in that: Based on every 100g of the low thermal conductivity vacuum glass sealing material, the content of the components is: 10-20g of mixed silver powder, 10-20g of copper-nickel alloy powder, 10-20g of aluminum-silicon alloy powder, 5-10g of stainless steel powder, 1-3g of lead oxide, 2-4g of silicon dioxide, 1-3g of boron oxide, 2-5g of plant glue, 5-8g of animal glue, 1-3g of microbial polysaccharide, 2-3g of magnesium aluminum silicate, 1-3g of bentonite, 1-3g of thermosensitive thixotropic agent, 1-3g of electrosensitive thixotropic agent, 2-3g of fluorocarbon surfactant, 5-8g of polymer surfactant, and ethyl acetate is used to make up to 100g.

4. A low thermal conductivity vacuum glass sealing material and a preparation method thereof according to claims 1-3, characterized in that: The method comprises the steps of a) preparing powder; b) mixing and adding; c) adjusting performance; d) drying; e) post-treatment; and f) stirring. Step a) powder preparation: taking appropriate amounts of metallic silver, copper-nickel alloy, aluminum-silicon alloy and stainless steel, crushing them by pulverizing, and then grinding and powdering them to obtain mixed silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder; Step b) mixing and adding: mixing silver powder, copper-nickel alloy powder, aluminum-silicon alloy powder and stainless steel powder according to the components and proportions, using ethyl acetate as an auxiliary agent, mixing in a blender and sequentially adding lead oxide, silicon dioxide and boron oxide materials during the mixing process, thereby obtaining a basic sealing material; Step c) adjusting the performance: placing the thermosensitive thixotropic agent, the electrosensitive thixotropic agent, the fluorocarbon surfactant and the polymer surfactant into the interior of the sealing basic material in sequence according to the components and proportions. Step d) drying: drying the material to volatilize the ethyl acetate inside it; Step e) post-treatment: firstly, the plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite are stirred to form a jelly, and then the dried basic sealing material is added into the jelly. Step f) stirring: using a crusher to stir the colloid and the basic sealing material, and after the mixture is evenly mixed, a low thermal conductivity vacuum glass sealing material is obtained.

5. The low thermal conductivity vacuum glass sealing material and the preparation method thereof according to claim 4, characterized in that: The step b) mixing and adding is carried out by a mixer for 2-4 hours, and during the mixing process, the mixture is heated to 300 degrees by pre-burning, and lead oxide, silicon dioxide, and boron oxide materials are added during the mixing process, with the addition interval being greater than 5 minutes.

6. The low thermal conductivity vacuum glass sealing material and the preparation method thereof according to claim 4, characterized in that: In the step d) drying, the material is purged by a hot air blower to volatilize the ethyl acetate inside the material, and the drying process is completed when the humidity inside the sealing basic material is less than 5%.

7. The low thermal conductivity vacuum glass sealing material and the preparation method thereof according to claim 4, characterized in that: In the post-treatment of step e), the plant glue, animal glue, microbial polysaccharide, magnesium aluminum silicate and bentonite are mixed according to the components and proportions, and an emulsification reaction is carried out in a reactor during the mixing process.

8. The low thermal conductivity vacuum glass sealing material and the preparation method thereof according to claim 4, characterized in that: In the step f), the colloid and the basic sealing material are put into the shearing machine with stirring, and the temperature is raised to 500 degrees at a rate of 1-8 degrees Celsius per minute at first slowly and then quickly, and then raised to 500-800 degrees Celsius after being kept for 2 hours, and then cooled to 200 degrees at a rate of 1-8 degrees Celsius per minute at first slowly and then quickly, and then naturally cooled to room temperature.