Building glass supporting wireless communication and preparation method thereof

By setting the composite glass structure of the signal penetration area of ​​the non-metallic material and the Low-E film area in the low-radiation glass, the electromagnetic shielding problem caused by the low-radiation glass is solved, and the smooth flow of wireless communication signals and thermal insulation performance are achieved. Taking into account both, improving user experience and energy efficiency.

CN118930076APending Publication Date: 2024-11-12SHENZHEN CSG APPLIED TECH CO LTD +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411096943.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Low-radiation glass leads to electromagnetic shielding effects in buildings and automobiles, weakening or blocking wireless communication signals, resulting in a decline in communication quality, especially in large-scale deployment, affecting user experience and resource and energy utilization efficiency.

Method used

A composite glass structure with at least two single-piece glass pieces is used, in which a signal penetration area and a coating area are set on the glass surface of one single-piece glass pieces. The signal penetration area is a dielectric film coverage area of ​​non-metallic materials, and the coating area is Low -E film coverage area, formed by glue or hollow structure, the signal penetration area can be a dot or rectangular frame arranged in a matrix, and the Low-E film layer is single silver, double silver, triple silver or four silver film, combined with silk Screen printing, magnetron sputtering and clamping sheet processes.

Benefits of technology

While maintaining thermal insulation performance, it improves the penetration ability of wireless communication signals, improves user network experience, reduces the energy efficiency and consumption of communication infrastructure, promotes energy-saving and low-carbon development, and does not affect the beauty of glass and signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930076A_ABST
    Figure CN118930076A_ABST
Patent Text Reader

Abstract

The invention provides building glass supporting wireless communication and a preparation method thereof, and belongs to the technical field of glass deep processing and application. Comprising a body, the body is composite glass formed by overlapping at least two single glass sheets, a signal penetrating area and a film coating area are arranged on the same glass surface of one single glass sheet and cover the glass surface where the signal penetrating area and the film coating area are located, the film coating area is a Low-E film covering area, and the signal penetrating area is a non-metal material dielectric film covering area; a laminated structure or a hollow structure is arranged between the adjacent single glass sheets of the body, and a film coating area and a signal penetration area are respectively formed by using a mask technology. The invention has the advantages of good energy-saving effect, no interference on indoor and outdoor transmission of communication signals and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass deep processing and application, and relates to architectural glass supporting wireless communication and a preparation method thereof. Background Art

[0002] Low-emissivity glass (Low-E glass) is made by coating one or more layers of metal or other compounds on the surface of the glass substrate to reduce the penetration of infrared and ultraviolet rays. Due to its excellent heat insulation and thermal insulation properties, Low-E glass is widely used in building energy-saving windows, curtain walls, and automotive glass. However, the low-emissivity film layer with metallic properties will also produce an electromagnetic shielding effect on the transmission of radio waves (such as base station signals), weakening or even blocking the propagation of wireless communication signals, thereby causing a rapid decline in communication quality. Especially for modern buildings that deploy Low-E glass over a large area and cars that use Low-E glass over a large area, the electromagnetic shielding effect is more obvious, which not only leads to a decline in the user's communication experience, but also causes a waste of resources and energy.

[0003] Therefore, the research on low-emissivity glass that supports wireless communication is of great significance and application prospects. On the one hand, it can ensure smooth communication signals while maintaining its excellent thermal insulation performance, thus improving the user's network experience; on the other hand, it can improve the energy efficiency of communication infrastructure, reduce indoor network costs, and promote energy-saving and low-carbon development. Summary of the invention

[0004] The first objective of the present invention is to provide a building glass that supports wireless communication in view of the above-mentioned problems existing in the prior art. The technical problem to be solved by the present invention is how to make the Low-E glass used for building curtain walls have good wireless communication penetration capability.

[0005] The objective of the present invention can be achieved through the following technical solutions: an architectural glass supporting wireless communication, characterized in that it comprises a main body, which is a composite glass formed by stacking at least two glass monoliths, wherein a signal penetration area and a coating area are arranged on the same glass surface of one glass monolith, the signal penetration area and the coating area cover the glass surface, the coating area is a Low-E film covering area, and the signal penetration area is a dielectric film covering area of ​​a non-metallic material; the adjacent glass monoliths of the main body are a laminated structure or a hollow structure.

[0006] Furthermore, the main body has three glass monoliths, and the inner side surface of the outermost glass monolith is provided with a coating area and a signal penetration area.

[0007] Furthermore, the signal penetration area is a plurality of dots arranged in a matrix on the glass surface, and the diameter of the dots is 0.1 mm to 30 mm.

[0008] Furthermore, the signal penetration area is a plurality of rectangular frames arranged in a matrix on the glass surface, and the side length of the rectangular frames is 0.2 mm to 60 mm.

[0009] Furthermore, the Low-E film layer is a single-silver Low-E film, a double-silver Low-E film, a triple-silver Low-E film, or a quad-silver Low-E film.

[0010] The second object of the present invention is to provide a method for processing the above-mentioned architectural glass.

[0011] Specifically, the steps include:

[0012] 1. Perform basic processing on each glass sheet: including cutting into specified size and shape, and then grinding and cleaning;

[0013] 2. Masking the coating area of ​​the glass monolith where the coating area and the signal penetration area are to be set: using a screen printing process to cover the coating area of ​​the first glass monolith to form a dielectric mask of the coating area;

[0014] 3. Dielectric film coating: After the glass monolithic sheet to be coated with the coating area and the signal penetration area is cleaned with pure water, a dielectric film of non-metallic material is coated;

[0015] 4. Remove the dielectric mask on the glass monolithic sheet in the area to be coated and the signal penetration area (the mask area can be removed by cleaning, light removal, high temperature burning or tearing off);

[0016] 5. Masking the signal penetration area of ​​the glass monolithic sheet to be provided with the coating area and the signal penetration area: after cleaning the glass monolithic sheet, the signal penetration area of ​​the glass monolithic sheet is covered by a screen printing process to form a signal penetration area mask;

[0017] 6. Low-e film coating: Low-e film is coated on the attachment surface of the glass monolith in the coating area and signal penetration area by magnetron sputtering;

[0018] 7. Combine the glass sheets by laminating and / or punching holes.

[0019] Furthermore, between step 6 and step 7, each glass sheet can be tempered as required; after the tempering treatment, it can also be bent and formed as required.

[0020] The advantage of this solution is that, for architectural glass, it has the thermal insulation performance of existing architectural glass, that is, the characteristics of Low-E glass. In addition, a signal penetration area of ​​a certain range is set on the glass surface. The signal penetration area is essentially an area without Low-E film. The signal penetration area can be in the form of scattered points or form a grid with the coating area. Generally speaking, the signal penetration area and the coating area should not be easily distinguished by the naked eye, which will neither affect the appearance of the glass nor the signal transmission. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is one of the plan view styles of architectural glass.

[0022] Figure 2 It is one of the plan view styles of architectural glass.

[0023] Figure 3 It is one of the plan view styles of architectural glass.

[0024] Figure 4 It is a cross-sectional view of architectural glass.

[0025] Figure 5 This is a process flow chart for the preparation of architectural glass. DETAILED DESCRIPTION

[0026] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0027] like Figure 1 and Figure 4 As shown, the main body includes a composite glass formed by stacking at least two glass monoliths, wherein a signal penetration area and a coating area are arranged on the same glass surface of one glass monolith, the signal penetration area and the coating area cover the glass surface, the coating area is a Low-E film covering area, and the signal penetration area is a dielectric film covering area of ​​non-metallic materials; a laminated structure or a hollow structure is formed between adjacent glass monoliths of the main body.

[0028] In short, the coating area and the signal penetration area are located on the same glass surface of the same glass sheet. Composite glass can be formed by lamination first and then hollowing. Alternatively, multiple glass sheets can be composited by lamination. Alternatively, multiple glass sheets can be composited by hollowing, and the hollow cavity can be an inert gas.

[0029] The signal penetration area is a number of dots arranged in a matrix on the glass surface, with a dot diameter of 0.1mm to 30mm. Figure 2 shown.

[0030] The signal penetration area is a number of rectangular frames arranged in a matrix on the glass surface, with a side length of 0.2mm to 60mm. Figure 1 and Figure 3 shown.

[0031] The Low-E film layer is a single silver Low-E film, a double silver Low-E film, a triple silver Low-E film, or a quadruple silver Low-E film.

[0032] The Low-E film layer is a single silver Low-E film, a double silver Low-E film, a triple silver Low-E film, or a quadruple silver Low-E film; the mainstream methods are double silver Low-E film and triple silver Low-E film. As for its film layer structure, it can be one of the many Low-E glasses previously applied for by our company, such as CN201610781775.6, CN201610782431.7, etc.

[0033] A processing method for the above-mentioned architectural glass.

[0034] Specifically, if Figure 5 As shown, the following steps are included:

[0035] Perform basic processing on each glass sheet: including cutting into specified size and shape, followed by edge grinding and cleaning;

[0036] Masking is performed on the coating area of ​​the glass monolith to be provided with the coating area and the signal penetration area: the coating area of ​​the first glass monolith is covered by a screen printing process to form a dielectric mask of the coating area; the dielectric mask of the coating area is formed, and the attachment of the mask of the coating area is to plate a dielectric film in the signal penetration area;

[0037] Dielectric film coating: After the glass monolithic sheet to be provided with the coating area and the signal penetration area is cleaned with pure water, a dielectric film of non-metallic material is coated;

[0038] Remove the dielectric mask on the glass monolithic sheet in the area to be coated and the signal penetration area (the mask area can be removed by cleaning, light removal, high temperature burning or tearing off, and the removal method depends on the form of the mask);

[0039] The signal penetration area of ​​the glass monolithic sheet to be provided with the coating area and the signal penetration area is subjected to masking treatment: after cleaning the glass monolithic sheet, the signal penetration area of ​​the glass monolithic sheet is covered by a screen printing process to form a signal penetration area mask (the mask evaporates during the high-temperature tempering process, such as the tempered heat-absorbing coating involved in CN202310289797.0, and the tearable film involved in CN202310275694.9 may also be used. If it is a tearable film, it needs to be torn off before tempering);

[0040] Coating Low-e film: Coating Low-e film on the attachment surface of the glass monolith in the coating area and signal penetration area by magnetron sputtering;

[0041] The glass sheets are joined together by laminating and / or forming holes.

[0042] For architectural glass, it has the thermal insulation performance of existing architectural glass, that is, the characteristics of Low-E glass. In addition, a signal penetration area of ​​a certain range is set on the glass surface. The signal penetration area is essentially an area without Low-E film. The signal penetration area can be in the form of scattered points, or it can form a grid with the coated area. Generally speaking, the signal penetration area and the coated area should not be easily distinguished by the naked eye, which will neither affect the appearance of the glass nor the signal transmission.

[0043] It should be noted that the dielectric film coating, Low-E film coating, mask attachment, mask removal, sandwiching and gluing methods involved in this solution are all existing technical methods. The applicant has prior patent applications for related technical methods, and bending forming is also an existing technical method. The core of this application is to overcome the communication signal interference problem caused by the use of Low-E glass in architectural glass.

[0044] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A building glass supporting wireless communication, characterized in that: The invention comprises a main body, which is a composite glass formed by stacking at least two glass monoliths, wherein a signal penetration area and a coating area are arranged on the same glass surface of one glass monolith, the signal penetration area and the coating area cover the glass surface, the coating area is a Low-E film covering area, and the signal penetration area is a dielectric film covering area of ​​non-metallic material; the adjacent glass monoliths of the main body are a laminated structure or a hollow structure.

2. According to the architectural glass supporting wireless communication as described in claim 1, the main body has three glass sheets, and the inner side surface of the outermost glass sheet is provided with a coating area and a signal penetration area.

3. According to the architectural glass supporting wireless communication as described in claim 1, the signal penetration area is a plurality of dots arranged in a matrix on the glass surface, and the diameter of the dots is 0.1 mm to 30 mm.

4. The architectural glass supporting wireless communication according to claim 1, wherein the signal penetration area is a plurality of rectangular frames arranged in a matrix on the glass surface, and the side length of the rectangular frames is 0.2 mm to 60 mm.

5. According to the architectural glass supporting wireless communication as claimed in claim 1, the Low-E film layer is a single silver Low-E film, a double silver Low-E film, a triple silver Low-E film, or a quadruple silver Low-E film.

6. A method for preparing the architectural glass according to any one of claims 1 to 5, characterized in that: The steps include: 1) Perform basic processing on each glass sheet: including cutting into specified size and shape, and then grinding and cleaning; 2) Masking the coating area of ​​the glass monolith where the coating area and the signal penetration area are to be set: using a screen printing process to cover the coating area of ​​the first glass monolith to form a dielectric mask of the coating area; 3) Dielectric film coating: After the glass monolithic sheet in the coating area and signal penetration area is cleaned with pure water, it is coated with a dielectric film of non-metallic material; 4) Remove the dielectric mask on the glass monolithic sheet in the area to be coated and the signal penetration area (the mask area can be removed by cleaning, light removal, high temperature burning or tearing off); 5) Masking the signal penetration area of ​​the glass monolithic sheet to be provided with the coating area and the signal penetration area: after cleaning the glass monolithic sheet, the signal penetration area of ​​the glass monolithic sheet is covered by a screen printing process to form a signal penetration area mask; 6) Low-e film coating: Low-e film is coated on the attachment surface of the glass monolith in the coating area and the signal penetration area by magnetron sputtering; 7) The glass sheets are joined together by laminating and / or forming holes.

7. A method for preparing architectural glass according to claim 6, characterized in that: Between step 6) and step 7), each glass sheet can be tempered as required; after the tempering, it can also be bent and formed as required.

Citation Information

Patent Citations

  • Coated glass and laminated glass thereof

    CN112456811A

  • 5G signal anti-reflection Low-E glass and design method thereof

    CN115557711A

  • Glass processing method, pattern coated glass and hollow glass

    CN117585913A

  • Low emissivity glass, method for manufacturing the same and vehicle window

    WO2016192569A2

  • Window structure and manufacturing method therefor

    WO2024136133A1