Gradient composite protective coating for hydraulic concrete and preparation method thereof
By using gradient composite protective coating on hydraulic concrete structures, combined with YEP toughened epoxy putty and high-performance elastic coating, the problem of insufficient water resistance and strength in hydraulic concrete is solved, and the existing coating is achieved All-round protection and structural stability.
Patent Information
- Application Number
- CN202411288463.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-12
AI Technical Summary
The existing protective coatings do not have enough water resistance and strength requirements in hydraulic concrete structures, and are prone to decay, cracking and leakage due to differences in physical and mechanical properties, and cannot effectively protect the concrete structure.
A gradient composite protective coating system is adopted, including an isolation layer and a protective layer. The isolation layer is YEP toughened epoxy putty, the protective layer is a high-performance elastic or high-toughness coating, and an interface layer is added between the two, through physical Performance gradient reduces the risk of coating failure.
It significantly reduces the occurrence of coating protection failure problems, provides comprehensive media isolation protection and impact wear functions, enhances the water resistance and strength of concrete, and extends the service life of the structure.
Smart Images

Figure CN118930318A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of protective coatings, and in particular to a gradient composite protective coating for hydraulic concrete and a preparation method thereof. Background Art
[0002] Concrete structure is one of the main hydraulic structures in water conservancy projects, such as concrete dams, water diversion tunnels, aqueducts, gates, etc. Concrete structures are affected by factors such as temperature, stress, and media in the natural environment, which can cause various diseases such as freeze-thaw erosion, cracking, leakage, carbonization, etc., resulting in damage to the concrete structure and shortened service life. Therefore, coatings are often used to protect the concrete surface, isolating the infiltration of external media through the coating, thereby avoiding various diseases of the concrete.
[0003] However, in actual applications, the coating often suffers from various problems such as hollowing, cracking, and blistering, which leads to protection failure. One of the main reasons is that the physical and mechanical properties between the protective coating and concrete are too different. For example, the modulus of ordinary concrete is between 20GPa and 40GPa, and the linear expansion coefficient is between 5 and 8×10 -6 / k, while the modulus of the protective layer material is generally between 10MPa and 500MPa, and the linear expansion coefficient is between 150 and 300 -6 / k. This difference may cause damage to the coating under conditions such as temperature changes and water pressure, resulting in protection failure.
[0004] Hydraulic concrete structures are exposed to water for a long time, and the operating environment is complex and the conditions are very harsh. Therefore, the protective coatings used in general construction projects cannot meet the requirements of hydraulic concrete for water resistance and strength. At present, the design of hydraulic protective coatings can be divided into two categories according to coating performance: (1) rigid / tough coatings, represented by epoxy materials such as epoxy paint, epoxy mortar, etc.; (2) elastic coatings, represented by elastic polyurethane / polyurea materials. In the application process, the following problems mainly exist: (1) Rigid / tough material systems represented by epoxy resin-based coatings have excellent bonding properties and good isolation and protection properties, but are prone to cracking or degassing in high temperature difference environments; (2) Elastic material systems represented by high-performance polyurethane / polyurea coatings do not crack or degass in high temperature difference environments, but their resistance to backwater pressure and substrate moisture is poor. Since concrete is a porous material, these situations are difficult to completely avoid, resulting in problems such as bulging and leakage in the flexible coating during operation. In addition, there are many defects on the concrete surface, especially a large number of pores often appear on the surface after surface grinding. Before applying the protective coating, the base defects and pores need to be repaired and filled. This is a tedious and important process. The repair materials used directly affect the quality of the base surface repair and are one of the decisive factors for the overall protective effect.
[0005] In summary, providing a performance gradient composite protective coating system to form a physical property transition from the base concrete material to the surface material, and significantly reduce the occurrence of coating protection failure problems, is an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0006] The purpose of the present invention is to provide a gradient composite protective coating for hydraulic concrete and a preparation method thereof, so as to solve the problem that the protective coating used in general construction projects cannot meet the requirements of hydraulic concrete for coating water resistance and strength.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a gradient composite protective coating for hydraulic concrete, comprising an isolation layer and a protective layer;
[0009] The isolation layer is a YEP toughened epoxy putty isolation layer;
[0010] The protective layer is a high-performance elastic coating or a high-toughness coating.
[0011] Preferably, the thickness of the isolation layer is 0.7 to 1.3 mm;
[0012] The tensile modulus of the isolation layer is 1 to 10 GPa.
[0013] Preferably, the linear expansion coefficient of the isolation layer is 30×10 -6 / k~100×10 -6 / k.
[0014] Preferably, the material of the high-performance elastic coating includes one or more of a single-component scraping polyurea coating, a two-component scraping polyurea coating, a spraying polyurea coating and a high-performance polyurethane coating;
[0015] The material of the high-toughness coating includes one or more of solvent-free spray-coated epoxy protective coating, solvent-free scraping-coated epoxy protective coating and solvent-free weather-resistant topcoat.
[0016] Preferably, the thickness of the protective layer is 1.0 to 2.0 mm;
[0017] The tensile modulus of the protective layer is 10 to 500 MPa.
[0018] Preferably, the linear expansion coefficient of the protective layer is 150×10 -6 / k~300×10 -6 / k.
[0019] Preferably, an interface layer is further included between the isolation layer and the protective layer;
[0020] The interface layer is made of epoxy adhesive material.
[0021] Preferably, the epoxy adhesive material is SK solvent-free epoxy interface agent and / or SK polyurea special interface agent.
[0022] The present invention also discloses a method for preparing the gradient composite protective coating for hydraulic concrete, comprising the following steps:
[0023] Clean the base layer of the hydraulic concrete surface, and then apply an isolation layer and a protective layer on the hydraulic concrete surface in sequence;
[0024] Or clean the base layer of the hydraulic concrete surface, and then apply an isolation layer, an interface layer and a protective layer on the hydraulic concrete surface in sequence.
[0025] Preferably, the coating of the protective layer needs to be carried out within 3 to 8 hours after coating the interface layer.
[0026] The present invention has at least the following beneficial effects:
[0027] The composite protective coating consists of an isolation layer and a protective layer, and whether to add an interface layer in the middle can be determined according to specific conditions. The base concrete-isolation layer-protective layer forms a performance gradient of rigidity-toughness-elasticity / high toughness in the vertical direction of the base surface, forming a performance gradient composite coating structure. The tough isolation layer is used to isolate the water seepage channel of the porous concrete, prevent the elastic coating from bulging and cracking, and provide a good base surface condition for the elastic coating, and seal the surface defects and pores of the concrete; the role of the elastic coating is to provide all-round medium isolation protection for the concrete, and can provide functional effects such as surface roughness reduction and impact resistance for water supply projects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of the structure of the gradient composite protective coating for hydraulic concrete in Example 1;
[0029] Figure 2 Schematic diagram of the structure of the gradient composite protective coating for hydraulic concrete in Example 2;
[0030] Among them, 1-concrete base, 2-isolation layer, 3-protective layer, 4-interface layer. DETAILED DESCRIPTION
[0031] The present invention provides a gradient composite protective coating for hydraulic concrete, comprising an isolation layer and a protective layer;
[0032] The isolation layer is a YEP toughened epoxy putty isolation layer;
[0033] The protective layer is a high-performance elastic coating or a high-toughness coating.
[0034] In the present invention, the thickness of the isolation layer is 0.7 to 1.3 mm, preferably 0.8 to 1.2 mm, more preferably 0.9 to 1.1 mm, and even more preferably 1.0 mm.
[0035] In the present invention, the tensile modulus of the isolation layer is 1 to 10 GPa, preferably 2 to 8 GPa, more preferably 4 to 6 GPa, and even more preferably 5 GPa.
[0036] In the present invention, the linear expansion coefficient of the isolation layer is 30×10 -6 / k~100×10 -6 / k, preferably 40×10 -6 / k~90×10 -6 / k, more preferably 50×10 -6 / k~80×10 -6 / k, more preferably 60×10 -6 / k~70×10 -6 / k.
[0037] In the present invention, the material of the high-performance elastic coating includes one or more of a single-component scraping polyurea coating, a two-component scraping polyurea coating, a spraying polyurea coating and a high-performance polyurethane coating.
[0038] In the present invention, the material of the high-toughness coating includes one or more of solvent-free spray-coated epoxy protective coating, solvent-free scraping-coated epoxy protective coating and solvent-free weather-resistant topcoat.
[0039] In the present invention, the thickness of the protective layer is 1.0 to 2.0 mm, preferably 1.2 to 1.8 mm, more preferably 1.4 to 1.6 mm, and even more preferably 1.5 mm.
[0040] In the present invention, the tensile modulus of the protective layer is 10 to 500 MPa, preferably 100 to 400 MPa, more preferably 200 to 350 MPa, and even more preferably 250 to 300 MPa.
[0041] In the present invention, the linear expansion coefficient of the protective layer is 150×10 -6 / k~300×10 -6 / k, preferably 180×10 -6 / k~280×10 -6 / k, more preferably 200×10 -6 / k~260×10 -6 / k, more preferably 230×10 -6 / k~250×10 -6 / k.
[0042] In the present invention, an interface layer is further included between the isolation layer and the protective layer.
[0043] In the present invention, the interface layer is an epoxy adhesive material.
[0044] In the present invention, the epoxy adhesive material is a solvent-free epoxy interface agent and / or a high-solid epoxy interface agent.
[0045] The present invention also discloses a method for preparing the gradient composite protective coating for hydraulic concrete, comprising the following steps:
[0046] Clean the base layer of the hydraulic concrete surface, and then apply an isolation layer and a protective layer on the hydraulic concrete surface in sequence;
[0047] Or clean the base layer of the hydraulic concrete surface, and then apply an isolation layer, an interface layer and a protective layer on the hydraulic concrete surface in sequence.
[0048] In the present invention, the coating of the protective layer needs to be carried out within 3 to 8 hours after coating the interface layer, preferably within 4 to 7 hours, and more preferably within 5 to 6 hours.
[0049] In the present invention, the isolation layer is coated by scraping.
[0050] In the present invention, the coating method of the protective layer and the interface layer is independently selected from one of blade coating, roller coating or spray coating.
[0051] In the present invention, when SK single-component polyurea material is used as the high-performance elastic coating, the thickness of a single coating is preferably 0.4-0.6 mm, more preferably 0.45-0.55 mm, and more preferably 0.5 mm; the thickness of a single coating of the high-performance elastic coating SK two-component polyurea material or the high-toughness coating is preferably 0.5-2 mm, more preferably 0.8-1.8 mm, and more preferably 1.2-1.6 mm; the latter coating is carried out after the surface of the former coating is dried.
[0052] In the present invention, the overlap width of the non-continuous coating work surface during the coating process should be ≥50mm, and the previous coating of the overlapping part should be finished with a slope to facilitate the overlap and smoothness of the next coating.
[0053] In the present invention, the time interval between multiple application is ≤24h, preferably ≤12h, and more preferably ≤8h.
[0054] In the present invention, after the gradient composite protective coating is applied, the step of curing and curing the gradient composite protective coating is also included. The requirements for curing and curing are: (1) curing at 10-25°C for 7-14 days. The lower the curing temperature, the longer the required curing time; and (2) curing components must be protected from physical contact, rain and immersion.
[0055] In the present invention, the relationship between the tensile modulus of the isolation layer, the protective layer and the hydraulic concrete is: hydraulic concrete>isolation layer>surface protective layer.
[0056] In the present invention, the relationship between the linear expansion coefficients of the isolation layer, the protective layer and the hydraulic concrete is: surface protective layer>isolation layer>hydraulic concrete.
[0057] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0058] Example 1
[0059] Mechanical grinding, high-pressure water cleaning and chiseling were used to remove the floating slurry, deterioration layer, dust, oil stains and loose particles on the concrete surface. After treatment, the surface of the concrete base was exposed to fresh and solid concrete, and the surface was clean and pollution-free. The isolation layer material (YEP-Ⅰ epoxy putty, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) was scraped on the treated concrete surface to repair and seal the defects such as honeycomb surface and pores on the concrete surface. After curing for 12 hours, an isolation layer with a thickness of 1mm was obtained. The tensile modulus of the isolation layer material was 5GPa, and the linear expansion coefficient was 35×10 -6 / k.
[0060] After the isolation layer is completed, the interface agent (SK polyurea special interface agent, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) is applied on its surface by roller coating to obtain an interface layer with a thickness of 200um. After waiting for about 4 hours, the protective layer material (SK polyurea protective coating, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) is scraped on the surface. The thickness of a single scraping is 0.5mm. The latter scraping is carried out 6 hours after the previous scraping is completed until the coating thickness is 1.5mm. After drying for 24 hours, the protective layer is obtained. The tensile modulus of the protective layer is about 10MPa, and the linear expansion coefficient is about 250×10 -6 / k.
[0061] The schematic diagram of the structure of the gradient composite protective coating for hydraulic concrete obtained after the isolation layer is coated and dried is as follows: Figure 1 As shown, after testing, the bonding strength between the composite coating and the concrete is 3.5MPa, the concrete base is damaged, and the back water pressure resistance exceeds 1.0MPa.
[0062] Example 2
[0063] The floating slurry, deterioration layer, dust, oil stains and loose particles on the concrete surface were removed by mechanical grinding, high-pressure water cleaning and chiseling. The surface of the treated concrete base exposed fresh and solid concrete, and the surface was clean and pollution-free. The isolation layer material (YEP-Ⅱ epoxy putty, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) was scraped on the treated concrete surface to repair and seal the defects such as honeycomb surface and pores on the concrete surface. After curing for 12 hours, an isolation layer with a thickness of 1mm was obtained. The tensile modulus of the isolation layer was 3GPa, and the linear expansion coefficient was 50×10 -6 / k.
[0064] The protective layer material (YEC-S spray-type solvent-free epoxy protective coating, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) was sprayed on the surface of the epoxy putty isolation layer. The thickness of a single spray was 1.5 mm, which met the thickness requirements. After drying for 24 hours, the protective layer was obtained. The tensile modulus of the protective layer was 300 MPa and the linear expansion coefficient was 140×10 -6 / k.
[0065] The schematic diagram of the structure of the gradient composite protective coating for hydraulic concrete obtained after the isolation layer is coated and dried is as follows: Figure 2 As shown, the bonding strength between the composite coating and concrete was tested to be 3.7 MPa, and the concrete base was damaged; the coating was intact after the temperature change cycle test (-20℃~60℃, 20 times).
[0066] Example 3
[0067] The floating slurry, deterioration layer, dust, oil stains and loose particles on the concrete surface were removed by mechanical grinding, high-pressure water cleaning and chiseling. The surface of the treated concrete base exposed fresh and solid concrete, and the surface was clean and pollution-free. The isolation layer material (YEP-Ⅱ epoxy putty, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) was scraped on the treated concrete surface to repair and seal the defects such as honeycomb surface and pores on the concrete surface. After curing for 12 hours, an isolation layer with a thickness of 1mm was obtained. The tensile modulus of the isolation layer was 3GPa, and the linear expansion coefficient was 50×10 -6 / k.
[0068] The protective layer material (YEC-W solvent-free weather-resistant topcoat, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) was sprayed on the surface of the epoxy putty isolation layer. The thickness of a single spraying layer was 1.0 mm, which met the thickness requirements. After drying for 24 hours, the protective layer was obtained. The tensile modulus of the protective layer was 100 MPa and the linear expansion coefficient was 160×10 -6 / k.
[0069] The schematic diagram of the structure of the gradient composite protective coating for hydraulic concrete obtained after the isolation layer is coated and dried is as follows: Figure 2 As shown, after testing, the bonding strength between the composite coating and the concrete is 3.3MPa, and the concrete base is damaged; after passing the temperature change cycle test (-20℃~60℃, 20 times), the coating is intact; after a 1000h xenon arc lamp aging test, there is no discoloration or powdering.
[0070] Example 4
[0071] The floating slurry, deterioration layer, dust, oil stains and loose particles on the concrete surface were removed by mechanical grinding, high-pressure water cleaning and chiseling. The surface of the treated concrete base exposed fresh and solid concrete, and the surface was clean and pollution-free. The isolation layer material (YEP-Ⅱ epoxy putty, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) was scraped on the treated concrete surface to repair and seal the defects such as honeycomb surface and pores on the concrete surface. After curing for 12 hours, an isolation layer with a thickness of 1mm was obtained. The tensile modulus of the isolation layer was 3GPa, and the linear expansion coefficient was 50×10 -6 / k.
[0072] The protective layer material (YEC solvent-free epoxy protective coating, produced by Beijing Zhongshui Kehaili Engineering Technology Co., Ltd.) was scraped on the surface of the epoxy putty isolation layer. The thickness of a single coat was 1.5 mm, meeting the thickness requirement. After drying for 24 hours, the protective layer was obtained. The tensile modulus of the protective layer was 400 MPa and the linear expansion coefficient was 120×10 -6 / k.
[0073] The schematic diagram of the structure of the gradient composite protective coating for hydraulic concrete obtained after the isolation layer is coated and dried is as follows: Figure 2 As shown, the bonding strength between the composite coating and the concrete was tested to be 3.5MPa, and the concrete base was damaged; the coating was intact after the temperature change cycle test (-20℃~60℃, 20 times).
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A gradient composite protective coating for hydraulic concrete, characterized in that: Including isolation layer and protective layer; The isolation layer is a YEP toughened epoxy putty isolation layer; The protective layer is a high-performance elastic coating or a high-toughness coating.
2. The gradient composite protective coating for hydraulic concrete according to claim 1, characterized in that: The thickness of the isolation layer is 0.7 to 1.3 mm; The tensile modulus of the isolation layer is 1 to 10 GPa.
3. The gradient composite protective coating for hydraulic concrete according to claim 2, characterized in that: The linear expansion coefficient of the isolation layer is 30×10 -6 / k~100×10 -6 / k.
4. The gradient composite protective coating for hydraulic concrete according to claim 3, characterized in that: The material of the high-performance elastic coating includes one or more of a single-component scraping polyurea coating, a two-component scraping polyurea coating, a spraying polyurea coating and a high-performance polyurethane coating; The material of the high-toughness coating includes one or more of solvent-free spray-coated epoxy protective coating, solvent-free scraping-coated epoxy protective coating and solvent-free weather-resistant topcoat.
5. The gradient composite protective coating for hydraulic concrete according to claim 4, characterized in that: The thickness of the protective layer is 1.0 to 2.0 mm; The tensile modulus of the protective layer is 10 to 500 MPa.
6. The gradient composite protective coating for hydraulic concrete according to claim 5, characterized in that: The linear expansion coefficient of the protective layer is 150×10 -6 / k~300×10 -6 / k.
7. A gradient composite protective coating for hydraulic concrete according to any one of claims 1 to 6, characterized in that: An interface layer is also included between the isolation layer and the protective layer; The interface layer is made of epoxy adhesive material.
8. The gradient composite protective coating for hydraulic concrete according to claim 7, characterized in that: The epoxy adhesive material is a solvent-free epoxy interface agent and / or a high-solid epoxy interface agent.
9. The method for preparing a gradient composite protective coating for hydraulic concrete according to any one of claims 1 to 8, characterized in that: The following steps are involved: Clean the base layer of the hydraulic concrete surface, and then apply an isolation layer and a protective layer on the hydraulic concrete surface in sequence; Or clean the base layer of the hydraulic concrete surface, and then apply an isolation layer, an interface layer and a protective layer on the hydraulic concrete surface in sequence.
10. The method for preparing a gradient composite protective coating for hydraulic concrete according to claim 9, characterized in that: The coating of the protective layer needs to be carried out within 3 to 8 hours after coating the interface layer.
Citation Information
Cited By
Universal concrete surface epoxy sealing coating and preparation method thereof
CN120484630A
A temperature-difference freeze-thaw resistant multilayer hydrophobic-aerogel composite protective coating suitable for highland environment and a preparation method thereof
CN122809927A