Novel grafting modification method for oxidized polyethlene wax with high acid value
By conducting an esterification reaction on the carbon chain of oxidized polyethylene wax, its acid value and grafting rate are improved, the problems of low acid value and complex preparation are solved, and high acid value oxidized polyethylene wax is prepared, which improves its performance and application and simplify the process flow.
Patent Information
- Application Number
- CN202411227640.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
The existing oxidized polyethylene wax has low acid value and complex preparation methods, which are not suitable for industrial production. In addition, traditional modification methods have problems such as uneven oxidation, slow grafting rate and side reactions.
Polar functional groups such as hydroxyl groups and carboxyl groups on the carbon chain of oxidized polyethylene wax are esterified with acid anhydrides and amino acids. Through the steps of oxidation, esterification and precipitation, the acid value and grafting rate are improved, and high acid value oxidized poly Vinyl wax.
The preparation of high acid value and controllable oxidized polyethylene wax is achieved, which improves its compatibility, lubricity, adhesion and weather resistance, broadens the application range, and is simple in process suitable for large-scale production.
Smart Images

Figure CN118930693A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of oxidized polyethylene wax, in particular to a novel grafting modification method of oxidized polyethylene wax with high acid value. Background Art
[0002] Polyethylene wax, also known as low molecular weight polyethylene, is divided into polymerized polyethylene wax and cracked polyethylene wax according to different manufacturing methods. The former is a by-product of ethylene polymerization, and the latter is made by heating and cracking polyethylene resin. As a type of low molecular weight polyethylene, they all have the characteristics of high softening point, low melt viscosity, odorless, non-toxic, good chemical stability, excellent miscibility and dielectric properties. Polyethylene wax that has not been modified is actually a mixture of low molecular weight polyethylene with different molecular weight distributions and physical properties. It is only used as a general dispersant and additive, cannot meet special purposes, and has a low value.
[0003] Oxidized polyethylene wax is the product obtained by oxidation of polyethylene wax. With the rapid development of industries such as masterbatch, plastics, coatings, and inks, the demand for high-performance additives is also increasing. Oxidized polyethylene wax has attracted widespread attention due to its unique properties. Traditional polyethylene wax has limitations in some applications, such as compatibility, dispersibility, and wettability. Through oxidation treatment, oxygen-containing functional groups such as carboxyl and hydroxyl groups can be introduced into the polyethylene wax molecular chain to improve its performance. Oxidized polyethylene wax has the following advantages: ① good compatibility, which can be compatible with a variety of polymers and resins to improve the comprehensive performance of the material; ② excellent dispersibility, which helps to evenly disperse pigments, fillers, etc. in the matrix; ③ good lubricity, reducing the friction coefficient and improving processing performance; ④ enhanced surface activity, improving the surface properties of the material, such as improving the adhesion and gloss of the coating.
[0004] With the continuous advancement of technology, the production process of oxidized polyethylene wax is also constantly improving and perfecting to meet the higher performance requirements of different industries. At present, the commonly used oxidation methods include air oxidation, peroxide oxidation, etc. Different methods have their own characteristics and scope of application.
[0005] Academics and industry have been actively carrying out the modification of polyethylene wax. The main purpose is to introduce polar groups such as hydroxyl and carboxyl groups into non-polar polyethylene wax, so as to improve its solubility, emulsification and other properties. Chemical oxidation and maleic anhydride grafting modification are two commonly used methods. Chemical oxidation introduces various polar functional groups such as hydroxyl and carboxyl groups by oxidation to enhance its hydrophilicity and emulsification. Maleic anhydride grafting modification is to graft polar groups such as maleic anhydride into the carbon chain of polyethylene wax through free radical-induced polymerization. However, both methods have obvious shortcomings. For example, the oxidation method often uses gas oxidation, which involves gas-solid two-phase reaction, poor mass transfer, uneven oxidation and low oxidation efficiency. Maleic anhydride grafting from polyethylene wax has a slow grafting rate, accompanied by side reactions such as chain breaking and cross-linking, and a low grafting rate.
[0006] Patent CN202410415239.9 proposes to use mixed foaming agent technology to first prepare foamed polyethylene wax, then immerse it in an initiator solution to absorb the initiator, and then carry out an oxidation reaction in an autoclave to obtain a new type of oxidized polyethylene wax. Although this technology realizes the control of polymer pore density and pore size, which is advantageous over solid-phase oxidation, it still uses high-temperature and high-pressure reactions, and the operation process is relatively complicated, and the acid value does not exceed 30 mgKOH / g. Patent CN202311039555.2 proposes a method for preparing high-density oxidized polyethylene wax in a solid phase. The screened resin particles are placed in an oven and oxidized in a solid phase state to obtain oxidized polyethylene wax with an acid value of 10-50 mgKOH / g. However, this method has too high requirements on raw materials, and a vibrating screen is required to screen out resin particles with an average particle size of 60-100 mesh, and the whiteness value is unknown. Patent CN202110095685.2 discloses a method for preparing high-density oxidized polyethylene wax. The process first performs thermal cracking, then uses a high-pressure plunger pump to spray the high-density polyethylene wax into powder, and then oxidizes it in the air to prepare oxidized polyethylene wax. However, the thermal cracking step of up to 500°C is very likely to cause the problem of numerical carbonization of polyethylene, and the acid value of the prepared oxidized polyethylene wax is less than 30 mgKOH / g. The polyethylene wax modification methods proposed in patents CN201910790539.4, CN201911269909.6, etc. are similar to most other reported modification methods. They all use polyethylene wax as a raw material, and react with maleic anhydride under the action of an initiator to undergo a free radical reaction to graft maleic anhydride on the carbon chain of the polyethylene wax. The present invention utilizes polar functional groups such as hydroxyl and carboxyl groups on the carbon chain of oxidized polyethylene wax to further react with acid anhydride, amino acid, etc. for efficient esterification, and can easily graft material structures such as acid anhydride and amino acid onto the carbon chain of polyethylene wax to achieve a higher acid value and grafting rate. This process has not been reported. Therefore, improving the polyethylene wax modification method, increasing polar groups, and increasing the acid value are of great value for broadening the application of oxidized polyethylene wax. Summary of the invention
[0007] The purpose of the present invention is to provide a novel high acid value oxidized polyethylene wax graft modification method to solve the problem that the acid value of the above-prepared oxidized polyethylene wax is low and the preparation method is complex and difficult for industrial production.
[0008] To achieve the above object, the first aspect of the present invention provides a novel high acid value oxidized polyethylene wax graft modification method, comprising the following steps:
[0009] S1: Oxidation reaction: Place the polyethylene wax in a solvent and dissolve and stir at 90-150°C for 2-4 hours, then add an oxidant to carry out oxidation reaction for 4-12 hours, and then add deionized water for washing;
[0010] S2: Esterification reaction: The oxidized polyethylene wax solution obtained in step S1 is heated to 100-140°C for dissolution and stirring, and then an activator is added, and then an anhydride reactant or an amino acid reactant is slowly added dropwise to carry out esterification reaction for 2-8 hours, and then the temperature is cooled to room temperature and the solvent is recovered by vacuum distillation;
[0011] S3: Precipitation: Add the polyethylene wax obtained in step S2 into a solvent, stir and react at 90-120°C for 1-3 hours, then lower the temperature to 40-60°C, slowly add a precipitant to crystallize the polyethylene wax, and obtain a high acid value oxidized polyethylene wax.
[0012] Preferably, the solvent in step S1 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, tetrahydrofuran, and dioxane.
[0013] Preferably, in step S1, the mass volume ratio of the polyethylene wax to the solvent is 0.1-1 g / mL.
[0014] Preferably, the oxidant in step S1 is one or more of air, oxygen, hydrogen peroxide, sodium hypochlorite, and nitric acid.
[0015] Preferably, the gas flow rate of the gaseous oxidant is 25-100 mL / min, and the mass ratio of the liquid and solid oxidants to the polyethylene wax is (0.05-0.2):1.
[0016] Preferably, the temperature of the oxidation reaction in step S1 is 90-150°C.
[0017] During the oxidation reaction, the present invention can generate polar groups such as hydroxyl groups and carboxyl groups in the carbon chain of the polyethylene wax, thereby forming a certain degree of oxidized polyethylene wax.
[0018] Preferably, the activator in step S2 is one or more of sulfuric acid, acetic acid, triethylamine, sodium bicarbonate, dicyclohexylcarbodiimide (DCC), diisopropylcarbodiimide (DIC), and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDCI).
[0019] Preferably, the acid anhydride reactant in step S2 is one or more of maleic anhydride, acetic anhydride, propionic anhydride, succinic anhydride, Boc anhydride, and propionic anhydride; the amino acid reactant is one or more of glycine, alanine, leucine, aspartic acid, glutamic acid, and lysine.
[0020] Preferably, in step S2, the mass ratio of the anhydride reactant to the polyethylene wax is (0.01-0.1):1.
[0021] Preferably, in step S2, the mass ratio of the amino acid reactant to the polyethylene wax is (0.01-0.1):1.
[0022] Under the conditions, the present invention performs an esterification reaction, and part of the carboxyl groups and hydroxyl groups in the oxidized polyethylene wax can further undergo an anhydride reaction with an acid anhydride substance, and the acid anhydride substance can be grafted into the carbon chain of the oxidized polyethylene wax to further enhance the polar group. Part of the carboxyl groups and hydroxyl groups in the oxidized polyethylene wax can undergo an esterification reaction with an amino acid substance to produce an amide structure, and the amino acid can be smoothly grafted into the polyethylene wax carbon chain, which can also further enhance the polar group.
[0023] Preferably, the solvent in step S3 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, toluene, xylene, tetrahydrofuran, and dioxane.
[0024] Preferably, the precipitant in step S3 is one or more of methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, and dimethyl sulfoxide.
[0025] Preferably, in step S3, the mass volume ratio of the polyethylene wax to the precipitant is 0.5-4 g / mL.
[0026] Preferably, the temperature for precipitation crystallization in step S3 is 40-60°C.
[0027] In the present invention, when the polyethylene wax is fully dissolved in a solvent, a suitable precipitant is used to slowly crystallize the polyethylene wax, so that the polyethylene wax can maintain a high crystallinity, and then high-quality oxidized polyethylene wax with high purity, good whiteness value and high acid value is precipitated.
[0028] The polyethylene wax prepared by the method of the invention has a white microbead-like appearance, contains sufficient polar functional groups such as carboxyl groups, and has a high and controllable acid value.
[0029] The second aspect of the present invention provides a high acid value oxidized polyethylene wax prepared by the above method.
[0030] The third aspect of the present invention provides an application of a high acid value oxidized polyethylene wax, which is applied in the fields of masterbatch, coating, ink, plastic processing, adhesive, rubber, textile and papermaking.
[0031] Therefore, the present invention adopts a novel high acid value oxidized polyethylene wax graft modification method of the above structure, which has the following beneficial effects:
[0032] (1) The process of the present invention is simple. With polyethylene wax as raw material, an oxidized polyethylene wax with high whiteness value, high acid value and controllable white micro-bead appearance can be prepared through oxidation, esterification, precipitation and other steps. The process is simple to operate, has good repeatability, and is suitable for large-scale production.
[0033] (2) The present invention can introduce polar groups such as carboxyl and hydroxyl groups into the carbon chain of polyethylene wax through oxidation and esterification treatment processes. In particular, the esterification reaction can further graft carboxyl and hydroxyl groups with acid anhydrides, amino acids, etc. to strengthen the polar groups in the carbon chain of polyethylene wax. The esterification process is different from the commonly used maleic anhydride grafting method. It does not require an initiator and further reacts with the original carboxyl and hydroxyl groups, resulting in a higher yield.
[0034] (3) The acid value of the oxidized polyethylene wax prepared by the present invention is high and controllable, and can significantly achieve the following advantages: ① Improve compatibility, have good compatibility with a variety of resins and polymers, and improve the comprehensive performance of the product; ② Improve lubricity, improve fluidity during processing, and make the product easier to form; ③ Enhance surface activity, improve the dispersibility of pigments and fillers, and improve the color uniformity and surface quality of the product; ④ Increase adhesion. For some applications that require good adhesion, high acid value oxidized polyethylene wax can improve the adhesion between the coating and the substrate; ⑤ Improve weather resistance, enhance the anti-aging performance of the product, and increase its service life in outdoor environments.
[0035] (4) The oxidized polyethylene wax prepared by the present invention has comprehensive properties such as good compatibility, lubricity, adhesion and excellent weather resistance, and can be applied in many fields such as masterbatch, coatings, inks, plastic processing, adhesives, rubber, textiles, papermaking, etc., and has a wider range of uses.
[0036] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The process flow chart of the grafting modification method of high acid value oxidized polyethylene wax in the present invention;
[0038] Figure 2 This is a picture of the appearance of the high acid value oxidized polyethylene wax prepared in Example 1;
[0039] Figure 3 This is a scanning electron microscope image of the high acid value oxidized polyethylene wax prepared in Example 1;
[0040] Figure 4 This is a transmission electron microscope image of the high acid value oxidized polyethylene wax prepared in Example 1;
[0041] Figure 5 This is the infrared spectrum picture of the high acid value oxidized polyethylene wax prepared in Example 1. DETAILED DESCRIPTION
[0042] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.
[0043] Example 1
[0044] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0045] (1) Oxidation reaction
[0046] Polyethylene wax (500 g) was placed in petroleum ether (500 mL), stirred and reacted at 90° C. for 2 hours, and then air was continuously introduced into the reaction solution (25 mL / min), and then stirred vigorously for 4 hours, and then deionized water was added for washing.
[0047] (2) Esterification reaction
[0048] Heat the polyethylene wax solution to 100°C, then add sulfuric acid (10g), and then slowly add maleic anhydride (5g) in batches, stir and react at 100°C for 2 hours, then cool to room temperature and wash with deionized water, and recover the solvent by reduced pressure distillation.
[0049] (3) Precipitation
[0050] The polyethylene wax was added into petroleum ether (2500 mL), stirred and reacted at 90° C. for 1 hour, then cooled to 40° C., and then the oxidized polyethylene wax was slowly crystallized using methanol (1000 mL) as a precipitant.
[0051] Example 2
[0052] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0053] (1) Oxidation reaction
[0054] Polyethylene wax (500 g) was placed in n-hexane (500 mL) and toluene (500 mL), and stirred at 100°C for 3 hours. Oxygen was then continuously introduced into the reaction solution (50 mL / min), and then stirred vigorously for 6 hours. Deionized water was then added for washing.
[0055] (2) Esterification reaction
[0056] Heat the polyethylene wax solution to 100°C, then add acetic acid (25g), and then slowly drop acetic anhydride (25g), stir and react at 100°C for 4 hours, then cool to room temperature and wash with deionized water, and recover the solvent by reduced pressure distillation.
[0057] (3) Precipitation
[0058] The polyethylene wax was added to n-hexane (950 mL) and toluene (50 mL), stirred and reacted at 100° C. for 2 hours, then cooled to 50° C., and then ethanol (500 mL) was used as a precipitant to slowly crystallize the oxidized polyethylene wax.
[0059] Example 3
[0060] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0061] (1) Oxidation reaction
[0062] Polyethylene wax (500 g) was placed in cyclohexane (400 mL) and xylene (100 mL), and stirred at 110°C for 4 hours. Then, hydrogen peroxide (25 g) was added to the reaction solution, and then stirred vigorously for 8 hours, and then deionized water was added for washing.
[0063] (2) Esterification reaction
[0064] Heat the polyethylene wax solution to 110°C, then add acetic acid (25g), and then slowly drop propionic anhydride (25g), stir and react at 110°C for 6 hours, then cool to room temperature and wash with deionized water, and recover the solvent by distillation under reduced pressure.
[0065] (3) Precipitation
[0066] The polyethylene wax was added to cyclohexane (450 mL) and xylene (50 mL), stirred and reacted at 110° C. for 3 hours, then cooled to 60° C., and then the oxidized polyethylene wax was slowly crystallized using isopropanol (250 mL) as a precipitant.
[0067] Example 4
[0068] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0069] (1) Oxidation reaction
[0070] Polyethylene wax (500 g) was placed in n-heptane (1000 mL) and tetrahydrofuran (100 mL), and stirred at 110° C. for 2 hours. Then, sodium hypochlorite (50 g) was added to the reaction solution, and then stirred vigorously for 12 hours, and then deionized water was added for washing.
[0071] (2) Esterification reaction
[0072] Heat the polyethylene wax solution to 110°C, then add triethylamine (50g), and then slowly drop succinic anhydride (50g), stir and react at 110°C for 8 hours, then cool to room temperature and wash with deionized water, and recover the solvent by distillation under reduced pressure.
[0073] (3) Precipitation
[0074] The polyethylene wax was added to n-heptane (950 mL) and tetrahydrofuran (50 mL), stirred and reacted at 110° C. for 2 hours, then cooled to 50° C., and then n-butanol (500 mL) was used as a precipitant to slowly crystallize the oxidized polyethylene wax.
[0075] Example 5
[0076] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0077] (1) Oxidation reaction
[0078] Polyethylene wax (500 g) was placed in petroleum ether (1000 mL) and dioxane (100 mL), and stirred at 120° C. for 2 hours. Then, nitric acid (50 g) was added to the reaction solution, and then stirred vigorously for 8 hours, and then deionized water was added for washing.
[0079] (2) Esterification reaction
[0080] The polyethylene wax solution was heated to 120°C, and then sodium bicarbonate (50g) was added, followed by slow addition of Boc anhydride (50g), and the mixture was stirred and reacted at 120°C for 8 hours, then cooled to room temperature and washed with deionized water, and the solvent was recovered by reduced pressure distillation.
[0081] (3) Precipitation
[0082] The above polyethylene wax was added to petroleum ether (850 mL) and dioxane (50 mL), stirred and reacted at 120° C. for 2 hours, then the temperature was cooled to 40° C., and then the oxidized polyethylene wax was slowly crystallized using a mixed solution of ethanol (350 mL) and N,N-dimethylformamide (50 mL) as a precipitant.
[0083] Example 6
[0084] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0085] (1) Oxidation reaction
[0086] Polyethylene wax (500 g) was placed in petroleum ether (800 mL) and carbon tetrachloride (100 mL), and stirred at 120 ° C for 2 hours. Then, oxygen was continuously introduced into the reaction solution (100 mL / min), and then stirred vigorously for 8 hours, and then deionized water was added for washing.
[0087] (2) Esterification reaction
[0088] Heat the polyethylene wax solution to 120°C, then add sulfuric acid (25g), and then slowly add ethyl propionic anhydride (25g), stir and react at 120°C for 8 hours, then cool to room temperature and wash with deionized water, and recover the solvent by distillation under reduced pressure.
[0089] (3) Precipitation
[0090] The polyethylene wax was added to petroleum ether (750 mL) and carbon tetrachloride (50 mL), stirred at 120°C for 2 hours, then cooled to 40°C, and then the oxidized polyethylene wax was slowly crystallized using a mixture of ethanol (250 mL) and dimethyl sulfoxide (50 mL) as a precipitant.
[0091] Example 7
[0092] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0093] (1) Oxidation reaction
[0094] Polyethylene wax (500 g) was placed in petroleum ether (800 mL) and carbon tetrachloride (100 mL), stirred at 120 ° C for 2 hours, and then air was continuously introduced into the reaction solution (100 mL / min), and then vigorously stirred for 8 hours, and then deionized water was added for washing.
[0095] (2) Esterification reaction
[0096] Heat the polyethylene wax solution to 120°C, then add sulfuric acid (25g), and then slowly add ethyl propionic anhydride (25g), stir and react at 120°C for 8 hours, then cool to room temperature and wash with deionized water, and recover the solvent by distillation under reduced pressure.
[0097] (3) Precipitation
[0098] The polyethylene wax was added to petroleum ether (750 mL) and carbon tetrachloride (50 mL), stirred at 120°C for 2 hours, then cooled to 40°C, and then the oxidized polyethylene wax was slowly crystallized using a mixture of ethanol (250 mL) and dimethyl sulfoxide (50 mL) as a precipitant.
[0099] Example 8
[0100] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0101] (1) Oxidation reaction
[0102] Polyethylene wax (500 g) was placed in petroleum ether (1000 mL) and toluene (200 mL), and stirred at 130°C for 2 hours. Then, oxygen was continuously introduced into the reaction solution (50 mL / min), and then stirred vigorously for 12 hours, and then deionized water was added for washing.
[0103] (2) Esterification reaction
[0104] The polyethylene wax solution was heated to 140°C, and then DCC (50g) was added, followed by slow addition of glycine (50g). The mixture was stirred and reacted at 140°C for 6 hours, then cooled to room temperature and washed with deionized water, and the solvent was recovered by reduced pressure distillation.
[0105] (3) Precipitation
[0106] The polyethylene wax was added to petroleum ether (650 mL) and toluene (50 mL), stirred and reacted at 110° C. for 2 hours, then cooled to 50° C., and then the oxidized polyethylene wax was slowly crystallized using a mixture of ethanol (100 mL) and isopropanol (25 mL) as a precipitant.
[0107] Example 9
[0108] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0109] (1) Oxidation reaction
[0110] Polyethylene wax (500 g) was placed in petroleum ether (1000 mL) and xylene (300 mL), stirred at 150 ° C for 2 hours, and then oxygen was continuously introduced into the reaction solution (100 mL / min), and then stirred vigorously for 8 hours, and then deionized water was added for washing.
[0111] (2) Esterification reaction
[0112] The polyethylene wax solution was heated to 140°C, and then DIC (50 g) was added, followed by slow addition of alanine (50 g). The mixture was stirred and reacted at 140°C for 4 hours, then cooled to room temperature and washed with deionized water, and the solvent was recovered by reduced pressure distillation.
[0113] (3) Precipitation
[0114] The polyethylene wax was added to petroleum ether (550 mL) and xylene (50 mL), stirred and reacted at 120° C. for 2 hours, then cooled to 40° C., and then ethanol (200 mL) was used as a precipitant to slowly crystallize the oxidized polyethylene wax.
[0115] Example 10
[0116] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0117] (1) Oxidation reaction
[0118] Polyethylene wax (500 g) was placed in petroleum ether (900 mL) and xylene (200 mL), and stirred at 130°C for 2 hours. Then, nitric acid (50 g) was added to the reaction solution, and then stirred vigorously for 8 hours, and then deionized water was added for washing.
[0119] (2) Esterification reaction
[0120] The polyethylene wax solution was heated to 120°C, and then EDCI (25 g) was added, followed by slow addition of leucine (25 g), and the mixture was stirred and reacted at 120°C for 6 hours, then cooled to room temperature and washed with deionized water, and the solvent was recovered by reduced pressure distillation.
[0121] (3) Precipitation
[0122] The polyethylene wax was added to petroleum ether (650 mL) and xylene (50 mL), stirred and reacted at 100° C. for 2 hours, then cooled to 50° C., and then the oxidized polyethylene wax was slowly crystallized using methanol (500 mL) as a precipitant.
[0123] Embodiment 11
[0124] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0125] (1) Oxidation reaction
[0126] Polyethylene wax (500 g) was placed in n-hexane (800 mL) and xylene (100 mL), and stirred at 120°C for 2 hours. Then, hydrogen peroxide (100 g) was added to the reaction solution, and then stirred vigorously for 12 hours, and then deionized water was added for washing.
[0127] (2) Esterification reaction
[0128] The polyethylene wax solution was heated to 120°C, and then EDCI (25 g) was added, and then aspartic acid (25 g) was slowly added. The mixture was stirred and reacted at 120°C for 8 hours, then cooled to room temperature and washed with deionized water, and the solvent was recovered by reduced pressure distillation.
[0129] (3) Precipitation
[0130] The polyethylene wax was added to n-hexane (650 mL) and xylene (50 mL), stirred and reacted at 110° C. for 2 hours, then cooled to 50° C., and then the oxidized polyethylene wax was slowly crystallized using methanol (400 mL) as a precipitant.
[0131] Example 12
[0132] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0133] (1) Oxidation reaction
[0134] Polyethylene wax (500 g) was placed in cyclohexane (700 mL) and toluene (100 mL), and stirred at 110°C for 2 hours. Then, hydrogen peroxide (50 g) was added to the reaction solution, and then stirred vigorously for 12 hours, and then deionized water was added for washing.
[0135] (2) Esterification reaction
[0136] Heat the polyethylene wax solution to 110°C, then add DCC (25g), and then slowly add glutamic acid (25g), stir and react at 110°C for 8 hours, then cool to room temperature and wash with deionized water, and recover the solvent by reduced pressure distillation.
[0137] (3) Precipitation
[0138] The polyethylene wax was added to cyclohexane (750 mL) and xylene (50 mL), stirred and reacted at 100° C. for 2 hours, then cooled to 40° C., and then n-butanol (300 mL) was used as a precipitant to slowly crystallize the oxidized polyethylene wax.
[0139] Embodiment 13
[0140] This embodiment provides a novel high acid value oxidized polyethylene wax graft modification method, and the reaction steps are as follows:
[0141] (1) Oxidation reaction
[0142] Polyethylene wax (500 g) was placed in petroleum ether (800 mL) and toluene (100 mL), and stirred at 100 °C for 2 hours. Then, oxygen was continuously introduced into the reaction solution (50 mL / min), and then stirred vigorously for 8 hours, and then deionized water was added for washing.
[0143] (2) Esterification reaction
[0144] The polyethylene wax solution was heated to 110°C, and then DIC (25 g) was added, followed by slow addition of lysine (25 g). The mixture was stirred and reacted at 100°C for 6 hours, then cooled to room temperature and washed with deionized water, and the solvent was recovered by reduced pressure distillation.
[0145] (3) Precipitation
[0146] The polyethylene wax was added to petroleum ether (800 mL) and toluene (50 mL), stirred and reacted at 100° C. for 2 hours, then cooled to 50° C., and then ethanol (400 mL) was used as a precipitant to slowly crystallize the oxidized polyethylene wax.
[0147] Comparative Example 1
[0148] The difference between this comparative example and Example 1 is that no maleic anhydride is added in step (2).
[0149] Comparative Example 2
[0150] The difference between this comparative example and Example 1 is that the oxidized polyethylene wax after the oxidation reaction in step (1) is directly used as the product.
[0151] Embodiment 14
[0152] The oxidized polyethylene wax prepared in Examples 1-13 and Comparative Examples 1-2 were used as samples for whiteness value test, respectively. Referring to the plastic whiteness test method of GB2913-82, the whiteness was measured using the whiteness meter WSB-2. Examples 1-13 and Comparative Examples 1-2 were evenly placed in the sample pool, covered with a smooth glass plate on the sample surface, pressed the sample, and then carefully removed the glass plate to keep the sample surface smooth and free of scattered particles. The pressed sample was placed in the sample stage of the instrument, and its whiteness value was measured to 0.1%. The acid value of the oxidized polyethylene wax prepared in Examples 1-13 and Comparative Examples 1-2 was measured with reference to the American material testing standard ASTMD-1386-78 and the national standard GB / 264-77. The test results are as follows:
[0153]
[0154]
[0155] As can be seen from the above table, the oxidized polyethylene wax prepared in Examples 1-13 has a very ideal whiteness value, all exceeding 80, indicating that the oxidized polyethylene wax grafting modification method developed by the present invention maintains the advantage of high brightness while increasing the acid value of polyethylene wax, and can well meet the market demand for high-whiteness oxidized polyethylene wax. In addition, the acid value of the oxidized polyethylene wax prepared in Examples 1-13 is between 35 and 60. This high acid value indicates that the present method can successfully produce carboxyl, hydroxyl and other groups on the carbon chain of polyethylene wax, and at the same time, the unique esterification process can further graft anhydrides, amino acids and the like. The idealized acid value can greatly broaden the application range of polyethylene wax and improve its advantages in compatibility, lubricity, stability, adhesion, and improved weather resistance.
[0156] Figure 2 This is a picture of the appearance of the high acid value oxidized polyethylene wax prepared in Example 1. It can be clearly seen that it presents a bright white color and has a white bead-like appearance. This bright white appearance helps to enhance the overall image of the product. During use, the white oxidized polyethylene wax has a relatively stable color, which helps to maintain the consistency of the product's appearance and also makes the product have good compatibility. In many applications, such as coatings, inks, plastics, etc., it has good compatibility with other ingredients and will not have an adverse effect on the color of the product, which is conducive to achieving accurate color matching.
[0157] Figure 3 This is a scanning electron microscope image of the high acid value oxidized polyethylene wax prepared in Example 1. It can be seen that the prepared oxidized polyethylene wax is composed of very fine particles. Figure 4 It is a transmission electron microscope, which shows that the oxidized polyethylene wax is a pile of fine particles or flakes, forming a significant waxy structure. This structural feature shows that it has good advantages in dispersibility, lubricity, etc., and can improve the compatibility and uniformity of oxidized polyethylene wax with other materials.
[0158] Figure 5 This is the infrared spectrum of the high acid value oxidized polyethylene wax prepared in Example 1. It can be clearly seen that the structure has a peak at 2919 cm -1 and 2848cm -1 A very obvious absorption peak appears at 1464cm, which is the stretching vibration peak of the saturated CH bond in the carbon chain of polyethylene wax. -1 is the deformation vibration peak of CH, and 720cm -1It is the horizontal swing vibration peak of -CH2. In addition, the more prominent feature is at 1793cm -1 and 1726cm -1 There is a significant absorption peak at 1299cm -1 The absorption peak at 3543-3759cm is the stretching vibration peak of COC in the anhydride, indicating that this process has successfully grafted the anhydride into the carbon chain of the oxidized polyethylene wax. -1 The peak at is the typical stretching vibration peak of -OH, which also indicates that there are a large number of hydroxyl groups in the carbon chain of polyethylene wax.
[0159] Therefore, the present invention adopts a novel high acid value oxidized polyethylene wax grafting modification method of the above structure, wherein the preparation method first performs an oxidation reaction on the polyethylene wax to produce polar functional groups such as hydroxyl and carboxyl, and then performs an esterification reaction on the hydroxyl, carboxyl and other groups with a series of acid anhydrides to further increase the polar functional groups; then precipitation is performed to obtain the grafted modified high acid value oxidized polyethylene wax. The prepared oxidized polyethylene wax presents a white microbead-like appearance, with a whiteness value exceeding 85 and an acid value of 35-60. The process of the present invention is simple, and the prepared oxidized polyethylene wax contains sufficient polar functional groups such as carboxyl, with a high and controllable acid value, which can significantly improve the advantages in terms of compatibility, lubricity, surface activity, adhesion, weather resistance, etc.
[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A novel high acid value oxidized polyethylene wax grafting modification method, characterized in that: The following steps are involved: S1: Oxidation reaction: Place the polyethylene wax in a solvent and dissolve and stir at 90-150°C for 2-4 hours, then add an oxidant to carry out oxidation reaction for 4-12 hours, and then add deionized water for washing; S2: Esterification reaction: The oxidized polyethylene wax solution obtained in step S1 is heated to 100-140°C for dissolution and stirring, and then an activator is added, and then an anhydride reactant or an amino acid reactant is slowly added dropwise to carry out esterification reaction for 2-8 hours, and then the temperature is cooled to room temperature and the solvent is recovered by vacuum distillation; S3: Precipitation: Add the polyethylene wax obtained in step S2 into a solvent, stir and react at 90-120°C for 1-3 hours, then lower the temperature to 40-60°C, slowly add a precipitant to crystallize the polyethylene wax, and obtain a high acid value oxidized polyethylene wax.
2. A novel high acid value oxidized polyethylene wax graft modification method according to claim 1, characterized in that: The solvent in step S1 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, tetrahydrofuran, and dioxane.
3. A novel high acid value oxidized polyethylene wax graft modification method according to claim 1, characterized in that: The oxidant in step S1 is one or more of air, oxygen, hydrogen peroxide, sodium hypochlorite, and nitric acid.
4. A novel high acid value oxidized polyethylene wax graft modification method according to claim 1, characterized in that: The activating agent in step S2 is one or more of sulfuric acid, acetic acid, triethylamine, sodium bicarbonate, dicyclohexylcarbodiimide, diisopropylcarbodiimide, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide.
5. A novel high acid value oxidized polyethylene wax graft modification method according to claim 1, characterized in that: In step S2, the acid anhydride reactant is one or more of maleic anhydride, acetic anhydride, propionic anhydride, succinic anhydride, Boc anhydride, and propionic anhydride; the amino acid reactant is one or more of glycine, alanine, leucine, aspartic acid, glutamic acid, and lysine.
6. A novel high acid value oxidized polyethylene wax graft modification method according to claim 1, characterized in that: The solvent in step S3 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, toluene, xylene, tetrahydrofuran, and dioxane.
7. A novel high acid value oxidized polyethylene wax graft modification method according to claim 1, characterized in that: The precipitant in step S3 is one or more of methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, and dimethyl sulfoxide.
8. A novel high acid value oxidized polyethylene wax graft modification method according to claim 1, characterized in that: The temperature for precipitation crystallization in step S3 is 40-60°C.
9. A high acid value oxidized polyethylene wax, characterized in that: The method is prepared by any one of claims 1 to 8.