Preparation method for refining, decolorizing and whitening polyethylene wax
Through the steps of oxidation, reduction, extraction and washing and physical adsorption, the problems of unsatisfactory color and complex process are solved, and polyethylene wax with high whiteness and high crystallinity are prepared, which solves the color and color of the product in the existing technology. The problem of process difficulty has achieved efficient decolorization and whitening and performance improvement of polyethylene wax.
Patent Information
- Application Number
- CN202411231174.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
The existing polyethylene wax preparation methods have problems such as darker color and poor whiteness, which leads to limited application scope and product quality. The existing decolorization and whitening process is complex and difficult to control, and it is impossible to take into account both the narrow melting range and the whiteness. Comprehensive properties such as high degree value and concentrated molecular weight.
By oxidation, reduction, extraction and washing, physical adsorption and precipitation, the pigments and impurities in the polyethylene wax are gradually removed through solvent selection and reaction conditions optimization, forming products with high crystallinity and high whiteness.
It has achieved simplification of the process flow and prepared polyethylene wax with high melting point, short melting range, high whiteness value and narrow molecular weight distribution, which has significantly improved the whiteness and purity of the product and broadened its fields in plastics, coatings, inks, etc. scope of application.
Smart Images

Figure CN118930694A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyethylene wax preparation, in particular to a polyethylene wax refining, decoloring and whitening preparation method. Background Art
[0002] Polyethylene wax is an important additive widely used in the fields of plastics, coatings, inks, rubbers, etc. It has good lubricity, dispersibility, demoulding properties and wear resistance, and can significantly improve the performance and quality of products. Traditional methods for preparing polyethylene wax mainly include high-pressure polyethylene cracking method and polymerization method. The high-pressure polyethylene cracking method is to crack high-pressure polyethylene at high temperature to obtain polyethylene wax with a lower molecular weight. Although this method has a simple process, the molecular weight distribution of the product is wide, the performance is unstable, and a large amount of by-products will be produced during the cracking process, causing environmental pollution. The polymerization method is to prepare polyethylene wax through the polymerization reaction of ethylene monomers. This method can obtain products with a narrow molecular weight distribution and better performance, but the reaction conditions are harsh and the cost is high, which limits its wide application.
[0003] In recent years, some new polyethylene wax preparation technologies have gradually emerged. For example, the method of preparing polyethylene wax by catalyzing ethylene polymerization with a metallocene catalyst can obtain a product with extremely narrow molecular weight distribution and excellent performance, but the high price of the metallocene catalyst limits its large-scale application. In addition, some studies have used emulsion polymerization, suspension polymerization and other methods to prepare polyethylene wax. These methods have improved the performance and quality of the product to a certain extent, but there are still some problems, such as complex reaction process and difficulty in product separation.
[0004] In the existing preparation process of polyethylene wax, the product is often faced with the problem of dark color, light yellow, and poor whiteness value, which limits its application range and product quality to a certain extent. Pure polyethylene wax is mainly composed of CC and CH bonds, and generally has no unsaturated groups. However, in the actual production process, unsaturated olefins, metal elements of catalysts or solid impurity particles are introduced, which may cause the polyethylene wax to have an unsatisfactory color. The selection and quality of raw materials may affect the color of the final product. For example, the use of polyethylene raw materials containing impurities or darker colors may result in unsatisfactory color of the prepared polyethylene wax. Improper control of preparation process conditions is also an important factor. During the reaction process, unreasonable settings of parameters such as temperature, pressure, and reaction time may lead to the occurrence of side reactions, thereby producing colored substances and deepening the color of the polyethylene wax.
[0005] At present, in order to solve the problem of dark color and poor whiteness value of polyethylene wax, some methods have been proposed, such as using polyethylene raw materials with less impurity content or improving the preparation process conditions to optimize the temperature, pressure, reaction time and other parameters in the reaction process. In addition, refining polyethylene wax is a very economical and feasible solution, and polyethylene wax can be refined, decolorized and whitened by some physical and chemical methods. However, in the prior art, most of the crude polyethylene wax products are refined, and there are few reports on decolorization and whitening at the same time.
[0006] Chinese patent CN200410043806.5 proposes to use C5~C 12 Alkanes, C6-C8 benzenes or their mixtures are used as solvents, C2-C4 monohydric alcohols are used as precipitants, the temperature and solvent ratio during dissolution are changed, and the steps of dissolution, concentration, precipitation, separation, drying, etc. are repeated to obtain polyethylene wax products with different average molecular weight levels. Although the whiteness value of the polyethylene wax prepared by this technology reaches 90, the melting range is still about 10°C, and the molecular weight of the polyethylene wax is greatly affected by the dissolution temperature and the solvent ratio, the molecular weight distribution is too wide, and the actual operation of the process conditions is difficult. Therefore, it is of great application value to develop a method for refining, decolorizing and whitening polyethylene wax with controllable conditions and the ability to prepare polyethylene wax with a narrow melting range, high whiteness value and concentrated molecular weight. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing polyethylene wax by refining, bleaching and whitening, so as to solve the problems that the refining and bleaching and whitening processes of the above-mentioned polyethylene wax are complicated and difficult to control, and the prepared product cannot take into account the comprehensive properties such as narrow melting range, high whiteness value and concentrated molecular weight.
[0008] To achieve the above object, the first aspect of the present invention provides a method for refining, decolorizing and whitening polyethylene wax, comprising the following steps:
[0009] S1: Oxidation: Place the polyethylene wax in a solvent and dissolve it at 50-120°C and stir for 2-4 hours, then add an oxidant to carry out oxidation reaction for 4-8 hours, and then add deionized water to wash and remove the oxidant;
[0010] S2: Reduction: Add a reducing agent to the polyethylene wax solution oxidized in step S1, carry out a reduction reaction at 50-120°C for 2-8 hours, then filter and recover the reducing agent, and then add deionized water for washing;
[0011] S3: Extraction and washing: dissolving the polyethylene wax solution obtained in step S2 at 60-120°C and stirring for 2-4 hours, then adding the extractant and continuing stirring for 2-4 hours, then standing to separate the layers and the solution, repeating the operation 2-4 times;
[0012] S4: Physical adsorption decolorization: add an adsorbent to the polyethylene wax mixture obtained in step S3, stir and react at 90-120°C for 4-8 hours, then filter and recover the adsorbent, and distill under reduced pressure to recover the solvent;
[0013] S5: Precipitation: Add the polyethylene wax obtained in step S4 into a solvent, stir and react at 90-120°C for 3-6 hours, then lower the temperature to 25-50°C, slowly add a precipitant to crystallize the polyethylene wax, and prepare a polyethylene wax with high crystallinity.
[0014] Preferably, the solvent in step S1 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, chloroform, tetrahydrofuran, dioxane, n-butanol, isopropanol, ethanol, and methanol.
[0015] Preferably, in step S1, the mass volume ratio of the polyethylene wax to the solvent is 0.2-1 g / mL.
[0016] Preferably, the oxidant in step S1 is one or more of hydrogen peroxide, sodium hypochlorite, potassium chlorate, nitric acid, and ammonium persulfate.
[0017] Preferably, in step S1, the mass ratio of the oxidant to the polyethylene wax is (0.01-0.1):1.
[0018] Preferably, the temperature of the oxidation reaction in step S1 is 50-120°C.
[0019] The present invention performs oxidation under such conditions, so that some double bonds and other chromophores in the polyethylene wax can be opened, and the chemical structure of the pigment can be destroyed, thereby achieving a decolorization and whitening effect.
[0020] Preferably, the reducing agent in step S2 is one or more of palladium carbon / hydrogen, iron powder / ammonium chloride, Na2S, Na2S2O3, SnCl2, and NaBH4.
[0021] The reducing agent in the present invention is divided into a gas reducing agent and a solid reducing agent, the flow rate of hydrogen in palladium carbon / hydrogen is 25-100 mL / min, and the mass ratio of iron powder to ammonium chloride in iron powder / ammonium chloride is 1:1.
[0022] Preferably, in step S2, the mass ratio of the reducing agent to the polyethylene wax is (0.01-0.1):1.
[0023] Preferably, the temperature of the reduction reaction in step S2 is 50-120°C.
[0024] The present invention performs reduction under such conditions, so that the unsaturated bonds remaining in the polyethylene wax can be completely converted into saturated hydrocarbons, oxygen-containing functional groups can be eliminated, and factors such as chromophores can be completely removed, thereby further enhancing the decolorization and whitening effects.
[0025] Preferably, the extractant in step S3 is one or more of deionized water, ethyl acetate, methyl formate, dichloromethane, acetic acid, and triethylamine.
[0026] Preferably, in step S3, the mass volume ratio of the polyethylene wax to the extractant is 0.5-1 g / mL.
[0027] After the extraction of the present invention, the residual metal elements, soluble organic impurities and the like in the polyethylene wax can be removed, thereby providing a prerequisite for the formation of highly crystalline polyethylene wax.
[0028] Preferably, the adsorbent in step S4 is one or more of activated carbon, alumina, zeolite molecular sieve, diatomaceous earth, polyacrylamide, and crown ether.
[0029] Preferably, in step S4, the mass ratio of the adsorbent to the polyethylene wax is (0.02-0.2):1.
[0030] Preferably, the solvent in step S5 is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, chloroform, tetrahydrofuran, and dioxane;
[0031] The precipitant is one or more of methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide and dimethyl sulfoxide.
[0032] Preferably, in step S5, the mass volume ratio of the polyethylene wax to the solvent is 0.2-1 g / mL; the mass volume ratio of the polyethylene wax to the precipitant is 0.5-2 g / mL.
[0033] Preferably, the precipitation temperature in step S5 is 25-50°C.
[0034] The invention uses a suitable precipitant to slowly crystallize the polyethylene wax after the polyethylene wax is fully dissolved in a solvent, so that the polyethylene wax can maintain a high crystallinity, thereby achieving the purposes of narrow melting range, narrow molecular weight distribution, high whiteness value, good lubricity and the like.
[0035] The second aspect of the present invention provides a polyethylene wax, which is prepared by the above-mentioned preparation method. The polyethylene wax has a melting range of 111.8°C-113.3°C, a molecular weight distribution of 4000-5000, a whiteness value of more than 90, and a density of 0.93-0.96.
[0036] The polyethylene wax prepared by the invention presents a white microbead-like appearance and has the characteristics of high melting point, short melting range, low viscosity, high whiteness, good lubricity and dispersibility, good hardness and the like.
[0037] The third aspect of the present invention provides an application of polyethylene wax, which is used in the manufacture of masterbatch, granulation, plastic steel, PVC pipes, hot melt adhesives, floor wax, plastic profiles, inks, and injection molding.
[0038] Therefore, the present invention adopts a polyethylene wax refining and decolorizing and whitening preparation method of the above structure, which has the following beneficial effects:
[0039] 1. The method of the present invention has a simple process flow. Starting from the existing polyethylene wax product, a white microbead-like polyethylene wax with a high melting point, a short melting range, a high whiteness value and a narrow molecular weight distribution can be prepared through oxidation, reduction, extraction and washing, physical adsorption, precipitation and other steps. The process operation is simple, the repeatability is good, and it is suitable for large-scale production.
[0040] 2. The present invention can effectively remove colored impurities in polyethylene wax through a unique decolorization and whitening process, significantly improve the whiteness value of the product, make its appearance whiter and brighter, and meet the market demand for high-whiteness polyethylene wax. The decolorization and whitening treatment not only improves the color of the polyethylene wax, but also reduces the impact of impurities on product performance, improves its purity and stability, and thus improves the overall quality of the product.
[0041] 3. The high-whiteness polyethylene wax prepared by the present invention has a wider application prospect in the fields of plastics, coatings, inks, rubbers, etc., so that the polyethylene wax can better meet the requirements of these fields for color and performance, further broadening its application scope.
[0042] 4. The polyethylene wax prepared by the present invention has a melting range of 111.8°C-113.3°C, a molecular weight distribution of 4000-5000, a whiteness value of more than 90, a density of 0.93-0.96, and shows excellent crystallinity.
[0043] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The process flow chart of the preparation method of polyethylene wax refining, decolorization and whitening in the present invention;
[0045] Figure 2 This is the appearance morphology of the polyethylene wax prepared in Example 1;
[0046] Figure 3 This is a scanning electron microscope image of the polyethylene wax prepared in Example 1;
[0047] Figure 4 This is the infrared spectrum of the polyethylene wax prepared in Example 1. DETAILED DESCRIPTION
[0048] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.
[0049] Example 1
[0050] This embodiment provides a method for preparing polyethylene wax by refining, decolorizing and whitening, and the reaction steps are as follows:
[0051] (1) Oxidation
[0052] The raw polyethylene wax (500 g) was placed in petroleum ether (2500 mL), stirred and reacted at 50° C. for 2 hours, and then hydrogen peroxide (5 g) was added, followed by strong stirring and reaction for 4 hours, and then deionized water was added to wash and separate to remove the hydrogen peroxide.
[0053] (2) Restore
[0054] Palladium carbon (5 g) was added to the polyethylene wax solution obtained in step (1), and hydrogen (25 ml / min) was continuously introduced after replacing the internal air. The mixture was stirred at 50° C. for 2 hours, and then the palladium carbon was recovered by filtration and washed with deionized water to remove impurities.
[0055] (3) Extraction and washing
[0056] The polyethylene wax solution obtained in step (2) was stirred and reacted at 60° C. for 2 hours, and then deionized water (1000 mL) was added and stirred and reacted for another 2 hours. The mixture was then allowed to stand for stratification, and the aqueous solution was separated, while the petroleum ether solution was retained. The operation was repeated twice.
[0057] (4) Physical decolorization
[0058] Activated carbon (10 g) was added to the solution obtained in step (3), and the mixture was stirred at 90° C. for 4 hours. The activated carbon was then recovered by filtration, and the solvent was recovered by distillation under reduced pressure.
[0059] (5) Precipitation
[0060] The polyethylene wax obtained in step (4) was added to a mixture of petroleum ether (2000 mL) and toluene (500 mL), stirred at 90° C. for 3 hours, then cooled to 25° C., and then a mixture of methanol (500 mL) and N,N-dimethylformamide (500 mL) was used as a precipitant to slowly crystallize the polyethylene wax.
[0061] Example 2
[0062] This embodiment provides a method for preparing polyethylene wax by refining, decolorizing and whitening, and the reaction steps are as follows:
[0063] (1) Oxidation
[0064] Polyethylene wax (500 g) was placed in n-hexane (1000 mL), and stirred at 80°C for 3 hours. Then, sodium hypochlorite (10 g) was added, and then stirred vigorously for 6 hours. Deionized water was added to wash and separate the sodium hypochlorite.
[0065] (2) Restore
[0066] Iron powder / ammonium chloride (10 g) was added to the polyethylene wax solution obtained in step (1) above, and the mixture was stirred and reacted at 60° C. for 4 hours. The iron powder was then recovered by filtration and washed with deionized water.
[0067] (3) Extraction and washing
[0068] The polyethylene wax solution obtained in the above step (2) was stirred and reacted at 80°C for 3 hours, and then ethyl acetate (800 mL) was added and stirred and reacted for another 3 hours. The mixture was then allowed to stand for stratification, and the ethyl acetate solution was separated, while the n-hexane solution was retained. The operation was repeated 3 times.
[0069] (4) Physical decolorization
[0070] Alumina (25 g) was added to the solution obtained in the above step (3), and the mixture was stirred and reacted at 100°C for 5 hours. The alumina was then recovered by filtration, and the solvent was recovered by distillation under reduced pressure.
[0071] (5) Precipitation
[0072] The polyethylene wax obtained in the above step (4) was added to a mixture of n-hexane (1500 mL) and tetrahydrofuran (200 mL), stirred at 100°C for 4 hours, then cooled to 35°C, and then the polyethylene wax was slowly crystallized using a mixture of ethanol (400 mL) and isopropanol (400 mL) as a precipitant.
[0073] Example 3
[0074] This embodiment provides a method for preparing polyethylene wax by refining, decolorizing and whitening, and the reaction steps are as follows:
[0075] (1) Oxidation
[0076] Polyethylene wax (500 g) was placed in cyclohexane (400 mL) and xylene (400 mL), and stirred at 100°C for 4 hours. Potassium chlorate (15 g) was then added, and then stirred vigorously for 8 hours. Deionized water was then added to wash and separate the potassium chlorate.
[0077] (2) Restore
[0078] Na2S (15 g) was added to the polyethylene wax solution obtained in the above step (1), and the mixture was stirred and reacted at 100°C for 6 hours, then filtered and washed with deionized water to remove impurities.
[0079] (3) Extraction and washing
[0080] The polyethylene wax solution obtained in the above step (2) was stirred at 100°C for 4 hours, and then methyl formate (600 mL) was added and stirred for 4 hours. The mixture was then allowed to stand for stratification, and the methyl formate solution was separated, while the cyclohexane / toluene solution was retained. The operation was repeated 4 times.
[0081] (4) Physical decolorization
[0082] Zeolite molecular sieve (50 g) was added to the solution obtained in the above step (3), and the mixture was stirred and reacted at 120° C. for 6 hours. The zeolite molecular sieve was then recovered by filtration, and the solvent was recovered by reduced pressure distillation.
[0083] (5) Precipitation
[0084] The polyethylene wax obtained in the above step (4) is added to a mixture of cyclohexane (1000 mL) and xylene (100 mL), stirred and reacted at 120°C for 6 hours, then cooled to 40°C, and then the polyethylene wax is slowly crystallized using a mixture of n-butanol (300 mL) and dimethyl sulfoxide (300 mL) as a precipitant.
[0085] Example 4
[0086] This embodiment provides a method for preparing polyethylene wax by refining, decolorizing and whitening, and the reaction steps are as follows:
[0087] (1) Oxidation
[0088] Polyethylene wax (500 g) was placed in n-heptane (400 mL) and dioxane (100 mL), stirred and reacted at 120°C for 2 hours, then nitric acid (25 g) was added, and then stirred vigorously for 6 hours, and then deionized water was added to wash and separate to remove the nitric acid.
[0089] (2) Restore
[0090] Na2S2O3 (25 g) was added to the polyethylene wax solution obtained in the above step (1), and the mixture was stirred and reacted at 120°C for 8 hours, then filtered and washed with deionized water to remove impurities.
[0091] (3) Extraction and washing
[0092] The polyethylene wax solution obtained in step (3) was stirred and reacted at 120°C for 2 hours, and then dichloromethane (500 mL) was added and stirred and reacted for 4 hours. The mixture was then allowed to stand and separate into layers. The dichloromethane solution was separated and the n-heptane / dioxane solution was retained. The operation was repeated twice.
[0093] (4) Physical decolorization
[0094] To the solution obtained in step (3) above, diatomaceous earth (80 g) was added, and the mixture was stirred and reacted at 120° C. for 3 hours. The diatomaceous earth was then recovered by filtration, and the solvent was recovered by distillation under reduced pressure.
[0095] (5) Precipitation
[0096] The polyethylene wax obtained in the above step (4) is added to a mixture of n-heptane (450 mL) and dioxane (50 mL), stirred and reacted at 120°C for 4 hours, then cooled to 50°C, and then the polyethylene wax is slowly crystallized using a mixture of ethanol (200 mL) and dimethyl sulfoxide (50 mL) as a precipitant.
[0097] Example 5
[0098] This embodiment provides a method for preparing polyethylene wax by refining, decolorizing and whitening, and the reaction steps are as follows:
[0099] (1) Oxidation
[0100] Polyethylene wax (500 g) was placed in carbon tetrachloride (600 mL) and chloroform (50 mL), and stirred at 100°C for 3 hours. Then, ammonium persulfate (50 g) was added, and then stirred vigorously for 6 hours. Deionized water was added to wash and separate to remove the ammonium persulfate.
[0101] (2) Restore
[0102] SnCl2 (50 g) was added to the polyethylene wax solution obtained in the above step (1), and the mixture was stirred and reacted at 120°C for 8 hours, then filtered and washed with deionized water to remove impurities.
[0103] (3) Extraction and washing
[0104] The polyethylene wax solution obtained in the above step (2) was stirred at 100°C for 3 hours, and then triethylamine (600 mL) was added and the stirring reaction was continued for 4 hours. Then, the mixture was allowed to stand for stratification, and the triethylamine solution was separated, and the carbon tetrachloride / chloroform solution was retained. The operation was repeated twice.
[0105] (4) Physical decolorization
[0106] Polyacrylamide (100 g) was added to the solution obtained in the above step (3), and the mixture was stirred and reacted at 100° C. for 3 hours. The polyacrylamide was then recovered by filtration, and the solvent was recovered by distillation under reduced pressure.
[0107] (5) Precipitation
[0108] The polyethylene wax obtained in the above step (4) was added to a mixture of carbon tetrachloride (600 mL) and chloroform (60 mL), stirred at 100°C for 4 hours, then cooled to 40°C, and then the polyethylene wax was slowly crystallized using a mixture of methanol (300 mL) and N,N-dimethylformamide (50 mL) as a precipitant.
[0109] Example 6
[0110] This embodiment provides a method for preparing polyethylene wax by refining, decolorizing and whitening, and the reaction steps are as follows:
[0111] (1) Oxidation
[0112] Polyethylene wax (500 g) was placed in petroleum ether (800 mL) and isopropanol (50 mL), and stirred at 60°C for 3 hours. Then, nitric acid (20 g) was added, and then stirred vigorously for 6 hours. Deionized water was added to wash and separate the nitric acid.
[0113] (2) Restore
[0114] NaBH4 (10 g) was added to the polyethylene wax solution obtained in step (1) above, and the mixture was stirred at 50°C for 4 hours, then filtered and washed with deionized water to remove impurities.
[0115] (3) Extraction and washing
[0116] The polyethylene wax solution obtained in step (2) was stirred and reacted at 60° C. for 3 hours, and then acetic acid (500 mL) was added and stirred and reacted for 2 hours. The mixture was allowed to stand for stratification, and the acetic acid solution was separated, and the petroleum ether / isopropanol solution was retained. The operation was repeated 3 times.
[0117] (4) Physical decolorization
[0118] Crown ether (50 g) was added to the solution obtained in the above step (3), and the mixture was stirred at 90° C. for 3 hours. The crown ether was then recovered by filtration, and the solvent was recovered by distillation under reduced pressure.
[0119] (5) Precipitation
[0120] The polyethylene wax obtained in the above step (4) was added to a mixture of petroleum ether (800 mL) and isopropanol (80 mL), stirred and reacted at 100° C. for 4 hours, then cooled to 40° C., and then a mixture of methanol (200 mL) and n-butanol (50 mL) was used as a precipitant to slowly crystallize the polyethylene wax.
[0121] Example 7
[0122] The polyethylene wax and intermediate product prepared in Examples 1-6 were used as samples for whiteness value test. Referring to GB2913-82 plastic whiteness test method, the whiteness was measured using a whiteness meter WSB-2. Examples 1-6 were evenly placed in a sample pool, covered with a smooth glass plate on the surface of the sample, the sample was pressed, and then the glass plate was carefully removed to keep the surface of the sample smooth and free of scattered particles. The pressed sample was placed in the sample stage of the instrument, and its whiteness value was measured to 0.1%.
[0123] The melting ranges of the polyethylene waxes and intermediate products prepared in Examples 1-6 were determined using an MP70 melting point apparatus.
[0124] The density of the polyethylene wax and intermediate product prepared in Examples 1 to 6 was tested using an ET-320 general solid density meter. The test results are as follows:
[0125]
[0126]
[0127]
[0128] It can be seen from the above table that the polyethylene wax prepared based on Examples 1-6 of the present invention has a very ideal whiteness value, all exceeding 90, indicating that the polyethylene wax refining and decolorization and whitening method developed by the present invention can successfully remove the pigment and other impurities in the original polyethylene wax. This high whiteness value improves the overall quality of the product and further expands its application in the fields of plastics, coatings, inks, rubbers, etc.
[0129] The melting range of the polyethylene wax prepared in Examples 1-6 is between 111.8°C and 113.3°C, and the melting range is very narrow, basically below 4°C. Such a narrow melting range means that the polyethylene wax melts within a narrow temperature range, making the molten state of the material more stable during processing, making it easier to control processing conditions, and reducing product quality problems caused by temperature fluctuations. It helps to ensure that the melting and flow behaviors of the polyethylene wax remain similar in the production of different batches, thereby improving the performance consistency of the product. The narrow melting range makes it easier for polyethylene wax to achieve good compatibility with other materials at a specific temperature, which is beneficial to improving the performance of the composite material.
[0130] The density of the polyethylene wax prepared in Examples 1-6 is in the range of 0.93-0.96, which is also ideal, and can make the products added with polyethylene wax have better mechanical properties, improve their durability and service life. As a filler or modifier, it can more effectively fill space and improve the overall performance of the material.
[0131] Figure 2 This is a picture of the actual appearance of Example 1. It can be seen that it has a white microbead appearance and is pure white in color.
[0132] Figure 3 It is the scanning electron microscope picture of embodiment 1, and it can be clearly seen that the prepared polyethylene wax is a very fine and smooth nanoparticle, which is gathered and stacked together to form a paraffin-like shape. The appearance of high brightness white is an important quality indicator of polyethylene wax. White polyethylene wax can avoid unnecessary color interference to the final product and ensure that the product has a pure and bright appearance. When mixed with other pigments, fillers or additives, it is easier to achieve the deployment and control of color. Many industries have specific requirements for the color of products, especially in some fields with high requirements for appearance, such as high-grade plastic products, automotive coatings, etc. White polyethylene wax can meet the strict requirements of these industries for color, thereby expanding its application range. The fine and smooth nanoparticle structure can enhance the dispersibility of polyethylene wax, improve the compatibility and uniformity of polyethylene wax with other materials, thereby improving the overall performance of the product. Nanoparticles can be more evenly distributed on the surface, which can significantly improve the surface properties of the material, increase the smoothness of the surface, reduce the friction coefficient, and improve the scratch resistance and wear resistance.
[0133] Figure 4 This is the infrared spectrum of the polyethylene wax prepared in Example 1. It can be seen that the polyethylene wax is very clean and has almost no impurities. -1 There is no absorption peak in the region, indicating that there are no polar groups such as hydroxyl and carboxyl in the structure. -1 and 2846cm -1 A very obvious absorption peak appears at 1600-1800cm, which is the stretching vibration peak of the saturated CH bond in the carbon chain of polyethylene wax. -1 There is no absorption peak in the region, indicating that there is no C=O functional group. -1 is the deformation vibration peak of CH, and 719cm -1 It is the horizontal rocking vibration peak of -CH2.
[0134] Therefore, the present invention adopts a polyethylene wax refining and decolorizing and whitening preparation method of the above structure, wherein the polyethylene wax is first subjected to an oxidation reaction to eliminate chromophores, followed by a reduction reaction to remove unsaturated bonds and oxygen-containing functional groups, and then subjected to extraction and washing to remove residual metal ions and other impurities; then subjected to physical adsorption and decolorization with an adsorbent; and finally subjected to precipitation to obtain crystalline polyethylene wax. The prepared polyethylene wax has a melting range of 111.8°C-113.3°C, a molecular weight distribution of 4000-5000, a whiteness value of more than 90, and a density of 0.93-0.96. It has the advantages of high melting point, short melting range, low viscosity, high whiteness, good lubricity and dispersibility, good hardness, etc., and shows excellent crystallinity. The quality exceeds that of most reported products and has very good practical application value.
[0135] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for refining, decolorizing and whitening polyethylene wax, characterized in that: The following steps are involved: S1: Oxidation: Place the polyethylene wax in a solvent and dissolve and stir at 50-120°C for 2-4 hours, then add an oxidant to carry out oxidation reaction for 4-8 hours, and then add deionized water to wash and remove the oxidant; S2: Reduction: Add a reducing agent to the polyethylene wax solution oxidized in step S1, carry out a reduction reaction at 50-120°C for 2-8 hours, then filter and recover the reducing agent, and then add deionized water for washing; S3: Extraction and washing: dissolving the polyethylene wax solution obtained in step S2 at 60-120°C and stirring for 2-4 hours, then adding the extractant and continuing stirring for 2-4 hours, then standing to separate the layers and the solution, repeating the operation 2-4 times; S4: Physical adsorption decolorization: add an adsorbent to the polyethylene wax mixture obtained in step S3, stir and react at 90-120°C for 4-8 hours, then filter and recover the adsorbent, and distill under reduced pressure to recover the solvent; S5: Precipitation: Add the polyethylene wax obtained in step S4 into a solvent, stir and react at 90-120°C for 3-6 hours, then lower the temperature to 25-50°C, slowly add a precipitant to crystallize the polyethylene wax, and prepare a polyethylene wax with high crystallinity.
2. The method for refining, decolorizing and whitening polyethylene wax according to claim 1, characterized in that: In step S1, the solvent is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, chloroform, tetrahydrofuran, dioxane, n-butanol, isopropanol, ethanol, and methanol.
3. The method for refining, decolorizing and whitening polyethylene wax according to claim 1, characterized in that: In step S1, the oxidant is one or more of hydrogen peroxide, sodium hypochlorite, potassium chlorate, nitric acid, and ammonium persulfate.
4. The method for refining, decolorizing and whitening polyethylene wax according to claim 1, characterized in that: In step S2, the reducing agent is one or more of palladium carbon / hydrogen, iron powder / ammonium chloride, Na2S, Na2S2O3, SnCl2, and NaBH4.
5. The method for refining, decolorizing and whitening polyethylene wax according to claim 1, characterized in that: In step S3, the extractant is one or more of deionized water, ethyl acetate, methyl formate, dichloromethane, acetic acid, and triethylamine.
6. The method for refining, decolorizing and whitening polyethylene wax according to claim 1, characterized in that: In step S4, the adsorbent is one or more of activated carbon, alumina, zeolite molecular sieve, diatomaceous earth, polyacrylamide, and crown ether.
7. The method for refining, decolorizing and whitening polyethylene wax according to claim 1, characterized in that: In step S5, the solvent is one or more of petroleum ether, n-hexane, cyclohexane, n-heptane, carbon tetrachloride, toluene, xylene, chloroform, tetrahydrofuran, and dioxane; and the precipitant is one or more of methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, and dimethyl sulfoxide.
8. The method for refining, decolorizing and whitening polyethylene wax according to claim 1, characterized in that: The precipitation temperature in step S5 is 25-50°C.
9. A polyethylene wax, characterized in that: The polyethylene wax prepared by the preparation method according to any one of claims 1 to 8 has a melting range of 111.8°C-113.3°C, a molecular weight distribution of 4000-5000, a whiteness value of more than 90, and a density of 0.93-0.
96.
10. The use of a polyethylene wax according to claim 9, characterized in that: Polyethylene wax is used in the manufacture of masterbatch, granulation, plastic steel, PVC pipes, hot melt adhesives, floor wax, plastic profiles, inks, and injection molding.
Citation Information
Patent Citations
Method of separating polyethylene wax
CN1597716A