High-transparency, low-gloss and high-performance water-based acrylate woodware emulsion and preparation method thereof

Through core-shell emulsion polymerization process and soap-free emulsion technology, the shortcomings of water-based wood coatings in water resistance and low gloss are solved, and the water-based acrylate wood emulsion with high transparency, low gloss and excellent performance are achieved, and the water-based acrylate wood emulsion with matte powder is combined with It has good compatibility, which improves the quality and convenience of the paint film.

CN118930747APending Publication Date: 2024-11-12SHANXI YUNYAN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185333.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing water-based wood coatings have shortcomings in water resistance and low gloss, especially the residue of emulsifier affects boiling water resistance, and the dispersion of silica matte powder is inconvenient, resulting in difficulty in using.

Method used

The core-shell emulsion polymerization process is adopted to form a high transparency and low gloss aqueous acrylate wood emulsion through the combination of different monomers. The soap-free emulsion and pre-emulsification technology are used to avoid the direct addition of the monomers to the reaction system, ensuring the stability and uniformity of the polymerization reaction.

Benefits of technology

It achieves high transparency, low gloss, excellent water resistance, stain resistance and chemical resistance, and has good compatibility with matte powder, improving the quality and convenience of the paint film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013336840000081
    Figure BDA0005013336840000081
  • Figure BDA0005013336840000091
    Figure BDA0005013336840000091
  • Figure BDA0005013336840000101
    Figure BDA0005013336840000101
Patent Text Reader

Abstract

The invention provides a high-transparency, low-gloss and high-performance water-based acrylate woodware emulsion and a preparation method thereof. The water-based acrylate emulsion is prepared through a soap-free emulsion and a core-shell emulsion polymerization process, and the prepared water-based acrylate emulsion has high transparency, low glossiness, excellent water resistance, excellent stain resistance, excellent chemical resistance and good compatibility with matt powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water-based acrylic emulsions, and in particular relates to a high-transparency, low-gloss, high-performance water-based acrylic wood emulsion and a preparation method thereof. Background Art

[0002] Waterborne wood coatings are a kind of coatings known for being healthy and environmentally friendly. With the improvement of people's environmental awareness and high attention to health, as well as the advancement of waterborne wood coating technology, waterborne wood coatings have become the development trend of wood coatings. Waterborne wood coatings will definitely occupy an important position in the home decoration and furniture coatings market in the future due to their low-hazard and low-pollution characteristics.

[0003] The main functions of water-based wood coatings are: decorative, water-resistant, weather-resistant, tough, environmentally friendly and safe. Wood coatings can also protect wood and effectively extend the service life of wood. In particular, some high-end solid wood furniture requires wood paints with high transparency and low gloss in addition to water resistance, hardness, stain resistance and other properties.

[0004] Existing water-based resin wood latex is prepared by ordinary emulsion polymerization process, which has poor water resistance due to the residual emulsifier, especially the requirement of boiling water resistance. Soap-free emulsion polymerization can greatly improve the water resistance of the emulsion because there is no emulsifier or only a trace amount of emulsifier. The water-based resin produced by soap-free emulsion polymerization process will have excellent water resistance.

[0005] At present, low-gloss or matte water-based wood paint generally reduces the gloss by adding silica matte powder. However, the surface of silica is very hydrophobic, and when adding matte powder, a dispersant needs to be added to disperse the matte powder in advance, which causes inconvenience in use. Summary of the invention

[0006] In view of the defects of the prior art, the purpose of the present invention is to provide a high-transparency, low-gloss high-performance water-based acrylic wood emulsion and a preparation method thereof. The present invention uses a core-shell emulsion polymerization process to match the core and the shell with different monomers to give them different refractive indices, thereby achieving the purpose of high transparency and low gloss.

[0007] To achieve the above purpose, the solution adopted by the present invention is as follows:

[0008] In a first aspect, the present invention provides a method for preparing a high-transparency, low-gloss, high-performance water-based acrylic wood emulsion, comprising the following steps:

[0009] Step (1), preparation of seed emulsion: uniformly mixing a first hard monomer, a first soft monomer, a carboxylic acid unsaturated monomer and a first functional monomer to prepare a core monomer mixed solution; mixing a buffer, water and a first emulsifier, adding the mixture to a reactor, stirring and heating, and when the temperature reaches a set temperature, adding a first initiator solution, and taking a portion of the core monomer mixed solution and adding it to the reactor, keeping the temperature for a period of time, to prepare a seed emulsion;

[0010] Step (2), preparation of the core layer emulsion: adding the remaining core monomer mixture to the reaction kettle, keeping the mixture warm for a period of time, and forming the core layer emulsion;

[0011] Step (3), adding alkaline solution for neutralization: adding alkaline solution to the reaction kettle at a set temperature, adjusting the pH value of the emulsion obtained in step (2) to 7-10, and then keeping the temperature for a period of time;

[0012] Step (4), preparation of shell monomer pre-emulsion: uniformly mixing water, the second emulsifier, the second hard monomer, the second soft monomer and the second functional monomer to prepare a shell monomer pre-emulsion;

[0013] Step (5), preparation of the finished product: adding part of the second initiator and reducing agent solution to the reaction kettle at a set temperature, then adding the shell monomer pre-emulsion obtained in step (4), then heating to the set temperature, keeping the temperature for a certain period of time, then cooling to room temperature, filtering the material, and obtaining the water-based acrylic wood emulsion;

[0014] The raw materials used to prepare the waterborne acrylic wood emulsion include the following components in parts by weight: 20-30 parts by weight of all hard monomers, 15-25 parts by weight of all soft monomers, 0-3 parts by weight of carboxylic acid unsaturated monomers, 0-5 parts by weight of all functional monomers, 0-1 parts by weight of all emulsifiers, 0-5 parts by weight of all initiators, 0-0.5 parts by weight of buffers, 0-1 parts of pH regulators, and the balance of water.

[0015] The water-based acrylic wood emulsion provided by the present invention is prepared by a soap-free emulsion and a core-shell emulsion process, and a self-crosslinking acrylic emulsion of a core layer and a shell layer is formed successively on the basis of a soap-free seed emulsion, and different monomers are used in the core layer material and the shell layer material to prepare water-based acrylic wood emulsions with different refractive indices, thereby achieving the purpose of high transparency and low gloss; and both the core layer emulsion and the shell layer emulsion use a pre-emulsified emulsion, which can avoid the monomer being directly added to the reaction system, resulting in an unstable polymerization system and the generation of gel, and can provide stability for the polymerization reaction to generate a uniform polymer emulsion.

[0016] Preferably, the amount of the first emulsifier is 0.01wt%-0.1wt% of the total amount of all monomers, the amount of the second emulsifier is 0.01wt%-1.0wt% of the total amount of all monomers, the amount of the first initiator is 0.01wt%-3.0wt% of the total amount of all monomers, the amount of the second initiator is 0.01wt%-0.1wt% of the total amount of all monomers, the amount of the buffer is 0.01wt%-0.1wt% of the total amount of all monomers, the amount of the first functional monomer is 0.01wt%-1.0wt% of the total amount of all monomers, and the amount of the second functional monomer is 0.01wt%-5.0wt% of the total amount of all monomers.

[0017] According to the water-based acrylic wood emulsion provided by the present invention, in the process of self-crosslinking of the core layer and the shell layer, the amount of the initiator determines the conversion rate of the monomer. Too little initiator will result in a low conversion rate of the monomer, affecting the film-forming quality of the water-based acrylic emulsion. Too much initiator will cause the molecular weight of the water-based acrylic ester formed by polymerization to decrease, the molecular weight distribution to be too wide, and the particle size distribution of the emulsion will also become wider, which also affects the film-forming quality. The use of an emulsifier can avoid the instability and gel generation caused by the direct addition of the monomer to the reaction system during polymerization. The emulsifier in an appropriate range can reduce the generation of gel, the polymerization tends to be stable, and the particle size of the formed water-based acrylic emulsion can be reduced and the particle size distribution range can be narrowed, so that the water-based acrylic emulsion is more delicate and more uniform, which is conducive to improving the quality of the formed paint film.

[0018] Preferably, the first hard monomer and the second hard monomer are independently selected from one or more of methyl methacrylate (MMA), styrene (SM), acrylonitrile (CAN) and vinyl acetate (PEVA); the first soft monomer and the second soft monomer are independently selected from one or more of ethyl acrylate (EA), butyl acrylate (BA), isooctyl acrylate (2-EHA) and hydroxyethyl acrylate (HEA); the carboxylic acid unsaturated monomer is selected from one or more of acrylic acid (AA), methacrylic acid (MAA), itaconic acid (ITA) and maleic acid (MA).

[0019] Preferably, the first functional monomer and the second functional monomer are independently selected from cross-linking monomers and / or molecular weight regulators, the cross-linking monomers are selected from one or more of diacetone acrylamide (DAAM), adipic acid dihydrazide (ADH), organic zinc salts, organic aluminum salts, diallyl phthalate (DAP) and ethylene glycol dimethacrylate (EGDMA), and the molecular weight regulator is selected from one or more of mercaptoethanol (ME), mercaptopropionic acid (3-MPA), n-butyl mercaptopropionate, α-methylstyrene dimer (AMSD), n-dodecyl mercaptan and tert-dodecyl mercaptan.

[0020] Preferably, the first functional monomer is a molecular weight regulator, and the second functional monomer is a cross-linking monomer; preferably, the second functional monomer is diacetone acrylamide (DAAM).

[0021] Preferably, the first emulsifier and the second emulsifier are independently selected from one or more of a polymerizable emulsifier, a phosphate ester, sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate and sodium benzene sulfonate; wherein the polymerizable emulsifier is selected from sodium vinyl sulfonate (SVS), sodium allyl sulfonate (SAS), allyloxy nonylphenol polyoxyethylene (10) ether (ANPEO10), allyloxy nonylphenol polyoxyethylene (10) ether monophosphate (ANPEO10-P1), allyloxy nonylphenol polyoxyethylene (10) ether ammonium sulfate (DNS-86), allyloxy hydroxypropane sulfonic acid sodium salt (HAPS), methacrylate hydroxypropane sulfonic acid sodium salt (HPMAS), 2-acrylamido-2-methylpropanesulfonic acid Acid sodium salt (AMPS-NA), sodium dioctyl sulfosuccinate (OT-75), sodium tridecanol sulfosuccinate (TR-70), disodium salt of ethoxylated nonylphenol sulfosuccinate half ester (DNS-1035), disodium salt of ethoxylated alkyl alcohol ether sulfosuccinate half ester (DNS-330), sodium salt of diisobutyl sulfosuccinate (IB-45), sodium salt of dibutyl sulfosuccinate (DBMS-45), ammonium sulfate of alkyl alcohol polyoxyethylene (3) (DNS-28A), sodium sulfate of alkyl alcohol polyoxyethylene (1-4) ether (DNS-360S), ammonium sulfate of alkyl alcohol polyoxyethylene (3) ether (DNS-18), ammonium sulfate of fatty alcohol ether (DP-70), sodium salt of succinic acid monooctadecylamide (DNS- A-18), disodium salt of sulfosuccinic acid monoamide (DP-25), sodium salt of alkyl alcohol polyoxyethylene (2) ether sulfate (DNS-328), ammonium sulfate of alkyl alcohol polyoxyethylene (1-4) ether (DNS-360), sodium isobutyl methyl sulfosuccinate (DNS-80), sodium dicyclohexyl sulfosuccinate (DNS-196), sodium isodecyl sulfosuccinate (DNS-268) and disodium decyl polyoxyethylene (6) sulfosuccinate (DNS-628).

[0022] Preferably, the first initiator and the second initiator are independently selected from one or more of ammonium persulfate (APS), potassium persulfate, sodium persulfate, tert-butyl hydroperoxide (TBHP), hydrogen peroxide and sodium hyposulfite; the buffer is selected from one or more of sodium bicarbonate, ammonium bicarbonate, sodium carbonate and ammonium carbonate; the pH adjuster is selected from one or more of ammonia water, sodium hydroxide and potassium hydroxide; the reducing agent is selected from sodium bisulfite or sodium sulfite.

[0023] Preferably, in step (1), the temperature is set to 70-90°C, 1%-20% of the total mass of the core monomer mixture is added to the reactor and kept warm for 15-30 minutes; in step (2), the mixture is kept warm for 15-60 minutes; in step (3), an alkaline solution is added at a temperature of 70-90°C; in step (5), the temperature is set to 40-90°C, a solution containing 10%-50% of the total mass of the second initiator and a reducing agent solution are added to the reactor, and the shell monomer pre-emulsion obtained in step (4) is added by continuous dropwise addition or all-in-one addition, and the continuous dropwise addition time of the shell monomer pre-emulsion obtained in step (4) is 1-3 hours, and then the temperature is raised to 70-90°C and kept warm for 1-3 hours.

[0024] Preferably, in step (5), after keeping the temperature at 70-90° C. for 1-3 hours, the following steps are further included: cooling to 60° C., adding the remaining solution containing 10%-50% of the total mass of the second initiator and the reducing agent solution to eliminate residual monomers; then, cooling to 40° C., adding 0.5wt%-1.5wt% of the total monomer amount of the third functional monomer, wherein the third functional monomer is a cross-linking monomer selected from diacetone acrylamide (DAAM), adipic acid dihydrazide (ADH ), one or more of organic zinc salts, organic aluminum salts, diallyl phthalate (DAP) and ethylene glycol dimethacrylate (EGDMA), preferably, the third functional monomer is adipic acid dihydrazide (ADH), and the added amount is 0.5wt%-1.5wt% of the total amount of all monomers; further preferably, the molar ratio of the second functional monomer diacetone acrylamide (DAAM) to the third functional monomer adipic acid dihydrazide (ADH) is (2.5-3):1.

[0025] According to the water-based acrylic wood emulsion provided by the present invention, diacetone acrylamide (DAAM) and adipic acid dihydrazide (ADH) hydrophilic cross-linking monomers are used in the shell material. The addition of DAAM and ADH in the emulsion may affect the structure of the shell material and the distribution of groups such as carboxyl groups, thereby affecting the compatibility with matte powder used in wood coatings. It is confirmed by the embodiments of the present invention that the molar ratio of DAAM to ADH is (2.5-3):1, and the compatibility with matte powder is the best.

[0026] According to the water-based acrylic wood emulsion provided by the present invention, after forming the core layer material, the present invention uses an alkaline solution to adjust the pH value of the system to 7-10, so that DAAM and ADH in the shell layer material of the subsequently formed self-crosslinking system will not undergo a crosslinking reaction during storage, thereby maintaining the storage stability of the emulsion, while ensuring that the alkaline environment of the emulsion is released during the film-forming process of application, and the self-crosslinking reaction proceeds normally during the film-forming process.

[0027] In a second aspect, the present invention also provides a high-transparency, low-gloss, high-performance water-based acrylic wood emulsion prepared by the preparation method as described above, wherein the molecular weight of the water-based acrylic wood emulsion is 10 4 -10 6 , molecular weight distribution is 1-50, emulsion particle size is 40-150nm, particle size distribution is 0.01-0.30, and glass transition temperature is 0-50℃.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The present invention provides a high-transparency, low-gloss high-performance water-based acrylic wood emulsion and a preparation method thereof. The emulsion is prepared by soap-free emulsion and core-shell emulsion polymerization process. The prepared water-based acrylic emulsion has high transparency, low gloss, excellent water resistance, excellent stain resistance, excellent chemical resistance, and good compatibility with matte powder. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with examples, the purpose of which is to better understand the content of the present invention and reflect the essential characteristics of the present invention, so the examples cited should not be regarded as limiting the scope of protection of the present invention. It is also particularly pointed out here that the specific experimental methods and equipment involved in the examples are conventional methods or implemented under the conditions recommended by the manufacturer's instructions unless otherwise specified, and the reagents involved are commercially available unless otherwise specified.

[0031] Embodiment 1:

[0032] This embodiment provides a high-transparency, low-gloss, high-performance water-based acrylic wood emulsion, and the preparation method thereof comprises the following steps:

[0033] 1. Add 0.05 parts of phosphate emulsifier and 106 parts of water into a reactor, start stirring at a stirring speed of 160 rpm, and then raise the temperature of the reactor to 80 degrees; mix 3 parts of MAA (unsaturated carboxylic acid monomer), 16.3 parts of MMA (hard monomer), 0.7 parts of mercaptopropionic acid (molecular weight regulator in functional monomers) and 7 parts of EHA (soft monomer) to prepare a core monomer mixed solution; when the temperature of the reactor is stable, add 0.1 parts of APS (initiator) solution, and then add 10% of the core monomer mixed solution, react for 15 minutes, and control the temperature between 70-90°C to prepare a soap-free seed emulsion;

[0034] 2. After the reaction is finished, the remaining 90% of the nuclear monomer mixture is added dropwise. The addition is completed within 1 hour and the mixture is kept warm for 1 hour to form a nuclear layer emulsion on the surface of the soap-free seed emulsion.

[0035] 3. Then add 25% ammonia water to neutralize, adjust the pH value to between 7.5-8.5, and keep warm for another 1 hour;

[0036] 4. Mix 2.7 parts of DAAM (cross-linking monomer in functional monomer), 39 parts of MMA (hard monomer), 10 parts of BA (soft monomer), and 26 parts of EHA (soft monomer) to prepare a shell monomer mixture;

[0037] 5. At 50°C, add all the shell monomer mixture to the emulsion obtained in step 3 at once, then add 0.1 parts of TBHP (initiator) and 0.13 parts of reducing agent solution, raise the temperature to 70-90°C, and then keep it warm for 1H;

[0038] 6. Then cool to 60°C, add 0.05 parts of TBHP (initiator) and 0.06 parts of reducing agent to eliminate residual monomers;

[0039] 7. Then cool to 40°C and add 1 part of ADH (cross-linking monomer in functional monomer) solution; finally filter the material to obtain high-transparency, low-gloss, high-performance water-based acrylic wood emulsion.

[0040] (Note: The sum of all monomers is 100 parts, and the amounts of other raw materials are equivalent to the proportion of monomers)

[0041] Embodiment 2:

[0042] This embodiment provides a high-transparency, low-gloss, high-performance water-based acrylic wood emulsion, and the preparation method thereof comprises the following steps:

[0043] 1. Add 0.05 parts of phosphate emulsifier and 80 parts of water into a reactor, start stirring at a stirring speed of 160 rpm, and then raise the temperature of the reactor to 80 degrees; mix 3 parts of MAA (unsaturated carboxylic acid monomer), 16.3 parts of MMA (hard monomer), 0.7 parts of mercaptopropionic acid (molecular weight regulator in functional monomers) and 7 parts of EHA (soft monomer) to prepare a core monomer mixed solution; when the temperature of the reactor is stable, add 0.1 parts of APS (initiator) solution, and then add 10% of the core monomer mixed solution, react for 15 minutes, and control the temperature between 70-90°C to prepare a soap-free seed emulsion;

[0044] 2. After the reaction is finished, the remaining 90% of the nuclear monomer mixture is added dropwise. The addition is completed within 1 hour and the mixture is kept warm for 1 hour to form a nuclear layer emulsion on the surface of the soap-free seed emulsion.

[0045] 3. Then add 25% ammonia water to neutralize, adjust the pH value to between 7.5-8.5, and keep warm for another 1 hour;

[0046] 4. Mix 26 parts of deionized water, 0.3 parts of phosphate emulsifier, 2.7 parts of DAAM (cross-linking monomer in functional monomer), 39 parts of MMA (hard monomer), 10 parts of BA (soft monomer), and 26 parts of EHA (soft monomer) to prepare a shell monomer pre-emulsion;

[0047] 5. At 80°C, add 0.1 parts of APS (initiator) solution to the emulsion obtained in step 3, then drop the shell monomer pre-emulsion and 0.3 parts of APS solution, dropwise for 2 hours, control the temperature between 70-90°C, and then keep warm for 1 hour;

[0048] 6. Then cool to 60°C, add 0.05 parts of TBHP (initiator) and 0.06 parts of reducing agent to eliminate residual monomers;

[0049] 7. Then cool to 40°C and add 1 part of ADH (cross-linking monomer in functional monomer) solution; finally filter the material to obtain high-transparency, low-gloss, high-performance water-based acrylic wood emulsion.

[0050] Embodiment 3:

[0051] On the basis of Example 1, MMA was replaced by SM, and other materials and process conditions were the same as those in Example 1.

[0052] Embodiment 4:

[0053] On the basis of Example 1, mercaptopropionic acid was replaced with dodecyl mercaptan, and other materials and process conditions were the same as those in Example 1.

[0054] Embodiment 5:

[0055] On the basis of Example 1, DAAM was added to the seed emulsion, and other materials and process conditions were the same as those in Example 1.

[0056] Embodiment 6:

[0057] On the basis of Example 2, the preparation of the seed emulsion remained unchanged, the hard monomer MMA in the shell monomer pre-emulsion was replaced with SM, and the other materials and process conditions were the same as in Example 2.

[0058] Embodiment 7:

[0059] On the basis of Example 2, the phosphate emulsifier was replaced with sodium diethylhexyl sulfosuccinate, and other materials and process conditions were the same as those in Example 2.

[0060] Embodiment 8:

[0061] On the basis of Example 1, the two parts of the monomer mixture were divided into two equal parts and added into the reaction kettle twice.

[0062] Embodiment 9:

[0063] On the basis of Example 2, the amount of mercaptopropionic acid added was adjusted to 0.3 parts, and other materials and process conditions were the same as in Example 2.

[0064] Embodiment 10:

[0065] On the basis of Example 2, the "16.3 parts of MMA" in step 1 was replaced by "10 parts of SM and 6.3 parts of MMA", and the "39 parts of MMA" in step 4 was replaced by "10 parts of SM and 29 parts of MMA", and the other materials and process conditions were the same as those in Example 2.

[0066] Embodiment 11:

[0067] On the basis of Example 2, the amount of ADH in step 7 was changed to 1.39 parts, and other materials and process conditions were the same as in Example 2.

[0068] Process comparison:

[0069] In Example 1, the initial temperature rise of the reaction in step 5 is very fast, and a sharp temperature drop is required to ensure that no material is sprayed.

[0070] Example 2: The reaction is normal, the temperature fluctuation is small, and it is easy to control.

[0071] Example 3, soap-free seed emulsion, is turbid after neutralization, and the monomer conversion rate in the fifth step reaction is low.

[0072] Example 4, soap-free seed emulsion, when neutralized, has high viscosity, and the 5th step reaction causes gelation due to high viscosity and difficulty in heat dissipation.

[0073] Example 5 is the same as Example 1.

[0074] Example 6 is basically the same as Example 2, except that the color of the emulsion is whiter and the particle size is larger.

[0075] In Example 7, the transparency of the emulsion is slightly higher, especially after the seed emulsion is neutralized, it is almost a completely transparent solution.

[0076] In Example 8, the monomer mixture for the two-step reaction is prepared in two equal portions, and the temperature rises gently without the need for rapid cooling.

[0077] Example 9 is basically the same as Example 2, except that the color of the emulsion is whiter and the particle size is larger.

[0078] Example 10 is basically the same as Example 2.

[0079] Example 11 is basically the same as Example 2.

[0080] In Examples 1, 3, 4, and 5, since the core layer emulsion is a pre-emulsified emulsion and the shell layer emulsion is a non-pre-emulsified emulsion, the viscosity is high during the preparation process, which easily causes gelation and a low conversion rate of the reaction monomers. In Examples 2, 6, 7, 9, 10, and 11, since both the core layer emulsion and the shell layer emulsion are pre-emulsified emulsions, the preparation process is more stable, the process is easier to control, the conversion rate of the reaction monomers is high, and the transparency of the prepared emulsion is high.

[0081] Performance Testing:

[0082] The performance of the high-transparency, low-gloss high-performance water-based acrylic wood emulsion prepared by the present invention can be characterized by the following method: the particle size and distribution of the emulsion are measured by using an Autosizer Lo-C automatic particle size analyzer; the pencil hardness of the paint film is measured according to ASTM-3364; the adhesion is measured according to the cross-hatch method of GB / T9286-88; the chemical solvent resistance (ethanol) is measured by placing non-woven cotton soaked in ethanol on the paint film; the water resistance test is to directly immerse the paint film in water; the stain resistance is to place non-woven cotton soaked in ethanol on the paint film for immersion (tea stains, coffee, cola, etc.), and other properties are tested according to corresponding standards.

[0083] The performance indicators of the high-transparency, low-gloss, high-performance water-based acrylic wood emulsions prepared in Examples 1 to 11 are listed in Table 1.

[0084] Table 1

[0085]

[0086]

[0087] As can be seen from Table 1, the water-based acrylic wood emulsions prepared in Examples 1, 4, and 5 have small particle sizes, high viscosities, or form gels, which do not meet the requirements. The emulsion formed in Example 3 exhibits stratification, which also does not meet the requirements. Examples 2, 6, 7, 9, 10, and 11 can all form uniform transparent liquids with low viscosity and can form core-shell structured emulsion particles with larger particle sizes.

[0088] Wood coating properties:

[0089] The water-based acrylic emulsions prepared in Examples 1 to 11 were applied to water-based wood coatings. The formulations of the water-based wood coatings are listed in Table 2.

[0090] Table 2

[0091] Serial number composition percentage 1 Aqueous acrylic emulsion of the present invention 80 2 Film-forming agent DPM 5 3 Wetting agent TEGO 245 0.1 4 Defoamer TEGO 805 0.03 5 Leveling agent BYK330 0.1 6 Thickener SN-612 0.18 7 Deionized water 14.59 total 100

[0092] The performance indicators of wood coatings are listed in Table 3.

[0093] Table 3

[0094]

[0095] As can be seen from Table 3, the water-based acrylic emulsions of Examples 1, 5, and 8 are applied to water-based wood coatings, and the resulting wood coatings have high gloss, while the wood coatings of Examples 2, 6, 7, 9, 10, and 11 have low gloss. However, the viscosity of Example 9 is relatively high, and the subsequent adjustment of the finished product formula and construction requirements are higher; the other properties of Examples 10 and 11 are relatively poor. The water resistance of the product of Example 10 is affected by the high content of SM in the seed emulsion, and the reduction in the amount of ADH in Example 11 reduces the cross-linking density of the product, and the overall performance of the product is reduced; Examples 2, 6, and 7, the three groups of experiments illustrate that the water-based acrylic emulsion prepared by the present invention can obtain a high-transparency, low-gloss, and high-performance water-based wood coating by combining different core and shell monomers.

[0096] When silica matt powder is added to the system, Examples 2, 6, 7, and 9 have good compatibility with matt powder and can be made into full matt wood paint with a glossiness of less than 5. Examples 1, 5, and 8 have poor compatibility with matt powder, and are prone to slag when matt powder is added, and the film surface has a strong granular feel.

[0097] According to Examples 2, 6 and 7, a high-transparency, low-gloss and high-performance wood paint emulsion can be prepared.

[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high-transparency, low-gloss, high-performance water-based acrylic wood emulsion. It is characterized in that The steps include: Step (1), preparation of seed emulsion: uniformly mixing a first hard monomer, a first soft monomer, a carboxylic acid unsaturated monomer and a first functional monomer to prepare a core monomer mixed solution; mixing a buffer, water and a first emulsifier, adding the mixture to a reactor, stirring and heating, and when the temperature reaches a set temperature, adding a first initiator solution, and taking a portion of the core monomer mixed solution and adding it to the reactor, keeping the temperature for a period of time, to prepare a seed emulsion; Step (2), preparation of the core layer emulsion: adding the remaining core monomer mixture to the reaction kettle, keeping the mixture warm for a period of time, and forming the core layer emulsion; Step (3), adding alkaline solution for neutralization: adding alkaline solution to the reaction kettle at a set temperature, adjusting the pH value of the emulsion obtained in step (2) to 7-10, and then keeping the temperature for a period of time; Step (4), preparation of shell monomer pre-emulsion: uniformly mixing water, the second emulsifier, the second hard monomer, the second soft monomer and the second functional monomer to prepare a shell monomer pre-emulsion; Step (5), preparation of the finished product: adding part of the second initiator and reducing agent solution to the reaction kettle at a set temperature, then adding the shell monomer pre-emulsion obtained in step (4), then heating to the set temperature, keeping the temperature for a certain period of time, then cooling to room temperature, filtering the material, and obtaining the water-based acrylic wood emulsion; The raw materials used to prepare the waterborne acrylic wood emulsion include the following components in parts by weight: 20-30 parts by weight of all hard monomers, 15-25 parts by weight of all soft monomers, 0-3 parts by weight of carboxylic acid unsaturated monomers, 0-5 parts by weight of all functional monomers, 0-1 parts by weight of all emulsifiers, 0-5 parts by weight of all initiators, 0-0.5 parts by weight of buffers, 0-1 parts of pH regulators, and the balance of water.

2. The preparation method according to claim 1, It is characterized in that The amount of the first emulsifier is 0.01wt%-0.1wt% of the total amount of all monomers, the amount of the second emulsifier is 0.01wt%-1.0wt% of the total amount of all monomers, the amount of the first initiator is 0.01wt%-3.0wt% of the total amount of all monomers, the amount of the second initiator is 0.01wt%-0.1wt% of the total amount of all monomers, the amount of the buffer is 0.01wt%-0.1wt% of the total amount of all monomers, the amount of the first functional monomer is 0.01wt%-1.0wt% of the total amount of all monomers, and the amount of the second functional monomer is 0.01wt%-5.0wt% of the total amount of all monomers.

3. The preparation method according to claim 1, It is characterized in that The first hard monomer and the second hard monomer are independently selected from one or more of methyl methacrylate (MMA), styrene (SM), acrylonitrile (CAN) and vinyl acetate (PEVA); the first soft monomer and the second soft monomer are independently selected from one or more of ethyl acrylate (EA), butyl acrylate (BA), isooctyl acrylate (2-EHA) and hydroxyethyl acrylate (HEA); the carboxylic acid unsaturated monomer is selected from one or more of acrylic acid (AA), methacrylic acid (MAA), itaconic acid (ITA) and maleic acid (MA).

4. The preparation method according to claim 1, It is characterized in that The first functional monomer and the second functional monomer are independently selected from cross-linking monomers and / or molecular weight regulators, respectively. The cross-linking monomer is selected from one or more of diacetone acrylamide (DAAM), adipic acid dihydrazide (ADH), organic zinc salts, organic aluminum salts, diallyl phthalate (DAP) and ethylene glycol dimethacrylate (EGDMA), and the molecular weight regulator is selected from one or more of mercaptoethanol (ME), mercaptopropionic acid (3-MPA), n-butyl mercaptopropionate, α-methylstyrene dimer (AMSD), n-dodecyl mercaptan and tert-dodecyl mercaptan.

5. The preparation method according to claim 4, It is characterized in that The first functional monomer is a molecular weight regulator, and the second functional monomer is a cross-linking monomer; preferably, the second functional monomer is diacetone acrylamide (DAAM).

6. The preparation method according to claim 1, It is characterized in that The first emulsifier and the second emulsifier are independently selected from one or more of a polymerizable emulsifier, a phosphate ester, sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate and sodium benzene sulfonate; wherein the polymerizable emulsifier is selected from sodium vinyl sulfonate (SVS), sodium allyl sulfonate (SAS), allyloxy nonylphenol polyoxyethylene (10) ether (ANPEO10), allyloxy nonylphenol polyoxyethylene (10) ether monophosphate (ANPEO10-P1), allyloxy nonylphenol polyoxyethylene (10) ether ammonium sulfate (DNS-86), allyloxy hydroxypropane sulfonic acid sodium salt (HAPS), methacrylate hydroxypropane sulfonic acid sodium salt (HPMAS), 2-acrylamido-2-methylpropane sulfonate sodium Salt (AMPS-NA), sodium dioctyl sulfosuccinate (OT-75), sodium tridecanol sulfosuccinate (TR-70), disodium salt of ethoxylated nonylphenol sulfosuccinate half ester (DNS-1035), disodium salt of ethoxylated alkyl alcohol ether sulfosuccinate half ester (DNS-330), sodium salt of diisobutyl sulfosuccinate (IB-45), sodium salt of dibutyl sulfosuccinate (DBMS-45), ammonium sulfate of alkyl alcohol polyoxyethylene (3) (DNS-28A), sodium sulfate of alkyl alcohol polyoxyethylene (1-4) ether (DNS-360S), ammonium sulfate of alkyl alcohol polyoxyethylene (3) ether (DNS-18), ammonium sulfate of fatty alcohol ether (DP-70), sodium salt of succinic acid monooctadecylamide (DNS A-18), disodium salt of sulfosuccinic acid monoamide (DP-25), sodium salt of alkyl alcohol polyoxyethylene (2) ether sulfate (DNS-328), ammonium sulfate of alkyl alcohol polyoxyethylene (1-4) ether (DNS-360), sodium isobutyl methyl sulfosuccinate (DNS-80), sodium dicyclohexyl sulfosuccinate (DNS-196), sodium isodecyl sulfosuccinate (DNS-268) and disodium decyl polyoxyethylene (6) sulfosuccinate (DNS-628).

7. The preparation method according to claim 1, It is characterized in that The first initiator and the second initiator are independently selected from one or more of ammonium persulfate (APS), potassium persulfate, sodium persulfate, tert-butyl hydroperoxide (TBHP), hydrogen peroxide and sodium hyposulfite; the buffer is selected from one or more of sodium bicarbonate, ammonium bicarbonate, sodium carbonate and ammonium carbonate; the pH adjuster is selected from one or more of ammonia water, sodium hydroxide and potassium hydroxide; the reducing agent is selected from sodium bisulfite or sodium sulfite.

8. The preparation method according to any one of claims 1 to 7, It is characterized in that In step (1), the temperature is set to 70-90°C, 1%-20% of the total mass of the core monomer mixture is added to the reactor, and the mixture is kept warm for 15-30 minutes; in step (2), the mixture is kept warm for 15-60 minutes; in step (3), an alkaline solution is added at a temperature of 70-90°C; in step (5), the temperature is set to 40-90°C, a solution containing 10%-50% of the total mass of the second initiator and a reducing agent solution are added to the reactor, and the shell monomer pre-emulsion obtained in step (4) is added by continuous dropwise addition or all-in-one addition, and the continuous dropwise addition time of the shell monomer pre-emulsion obtained in step (4) is 1-3 hours, and then the temperature is raised to 70-90°C and kept warm for 1-3 hours.

9. The preparation method according to claim 8, It is characterized in that In step (5), after keeping the temperature at 70-90°C for 1-3 hours, The invention comprises the following steps: cooling to 60°C, adding the remaining solution containing 10%-50% of the total mass of the second initiator and the reducing agent solution to eliminate the residual monomers; then, cooling to 40°C, adding 0.5wt%-1.5wt% of the third functional monomer of the total monomer amount, wherein the third functional monomer is a cross-linking monomer, selected from one or more of diacetone acrylamide (DAAM), adipic acid dihydrazide (ADH), organic zinc salt, organic aluminum salt, diallyl phthalate (DAP) and ethylene glycol dimethacrylate (EGDMA), preferably, the third functional monomer is adipic acid dihydrazide (ADH), and the added amount is 0.5wt%-1.5wt% of the total amount of all monomers; further preferably, the molar ratio of the second functional monomer diacetone acrylamide (DAAM) to the third functional monomer adipic acid dihydrazide (ADH) is (2.5-3):

1.

10. A high-transparency, low-gloss, high-performance water-based acrylic wood emulsion prepared by the preparation method according to any one of claims 1 to 9, It is characterized in that The molecular weight of the aqueous acrylic wood emulsion is 10 4 -10 6 , molecular weight distribution is 1-50, emulsion particle size is 40-150nm, particle size distribution is 0.01-0.30, and glass transition temperature is 0-50℃.