Preparation method of broadband quick-response acrylate dielectric elastomer as well as product and application of broadband quick-response acrylate dielectric elastomer
By using crosslinking agent, flexible monomer and functional monomer in acrylate dielectric elastomer photocuring method, combined with chemical and physical crosslinking, the problem of low response speed and frequency of acrylate dielectric elastomer is solved, and the problem of low response speed and frequency of acrylate dielectric elastomer is achieved. Faster response speed and wider frequency range improve the application potential of software robot drivers.
Patent Information
- Application Number
- CN202411106475.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing acrylate dielectric elastomers have slow response speed and low response frequency, which affects their application effect in the field of software robot drivers.
Acrylate crosslinking agent, flexible monomer and functional monomer are used to form a crosslinking network polymer through photocuring, combining chemical and physical crosslinking to prepare acrylate dielectric elasticity with faster response speed and wider response frequency range body.
While achieving large drive strain, it reduces viscoelasticity, improves the response speed and response frequency range, and significantly improves the driving effect of acrylate dielectric elastomer in soft robot drivers.
Smart Images

Figure CN118930753A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dielectric elastomers, and in particular relates to a preparation method of a broadband fast-response acrylic dielectric elastomer and a product and application thereof. Background Art
[0002] As an electroactive polymer, dielectric elastomer will deform due to electrostatic force under external electric field stimulation. Compared with piezoelectric materials, magnetostrictive materials and shape memory alloys, dielectric elastomers have the characteristics of low density, low noise, large driving strain and high energy density, making dielectric elastomers, a kind of "artificial muscle-like" intelligent material, extremely valuable for research and application in many fields such as flexible actuators, energy harvesting, flexible sensors, vibration controllers, speakers, etc.
[0003] Common dielectric elastomer materials currently include silicone rubber, polyurethane and acrylate. Among them, acrylic dielectric elastomers have a much smaller elastic modulus than silicone rubber and polyurethane, and are more likely to produce large electro-induced deformations. However, the commonly used 3M VHB series acrylic dielectric elastomers have shortcomings such as slow response speed, obvious hysteresis, and low response frequency, which seriously affect the driving effect of acrylic dielectric elastomers in the fields of soft robots. However, there are few reports on research on improving the response speed and response frequency of acrylic dielectric elastomers.
[0004] Since the flexible and efficient movement of soft robots is highly dependent on the faster response speed and wider response frequency of flexible actuators, the preparation of a broadband and fast-response acrylic dielectric elastomer can greatly promote its application and development in soft robot actuators. Summary of the invention
[0005] In view of one or more of the above defects or improvement needs of the prior art, the present invention provides a method for preparing a broadband fast-response acrylate dielectric elastomer, and its product and application. The present invention adopts a method of photocuring an acrylate crosslinking agent and an acrylate flexible monomer and a functional monomer to form a crosslinked network polymer to prepare an acrylate dielectric elastomer, which can achieve a large driving strain while having a faster response speed and a wider response frequency range.
[0006] To achieve the above object, according to a first aspect of the present invention, a method for preparing a broadband fast-response acrylic dielectric elastomer is provided, comprising the following steps: (1) uniformly mixing an acrylate crosslinking agent, an acrylate flexible monomer, an acrylate functional monomer, and a photoinitiator to form an acrylate dielectric elastomer precursor solution; (2) After vacuuming the acrylate dielectric elastomer precursor solution to remove bubbles, the solution is injected into a dielectric elastomer mold having a groove; (3) After UV light curing, the acrylic dielectric elastomer is obtained.
[0007] As a further improvement of the present invention, the acrylate dielectric elastomer precursor solution includes the following components in percentage by mass: 40-60% of an acrylic crosslinker, 20-35% of an acrylate flexible monomer, 10-25% of an acrylate functional monomer, and 0.5-3% of a photoinitiator.
[0008] As a further improvement of the present invention, the acrylate crosslinking agent is selected from any one or more of a polyester acrylate crosslinking agent, a polyether acrylate crosslinking agent, an epoxy acrylate crosslinking agent and a polyurethane acrylate crosslinking agent.
[0009] More preferably, the acrylic crosslinking agent is a polyurethane acrylate crosslinking agent CN9021 containing two functional groups, which is purchased from Sartomer.
[0010] As a further improvement of the present invention, the acrylic ester flexible monomer is selected from any one or more of ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, isooctyl acrylate, decyl acrylate, and isodecyl acrylate; Preferably, the acrylic flexible monomer is butyl acrylate and / or isooctyl acrylate.
[0011] As a further improvement of the present invention, the acrylate functional monomer is selected from any one or more of hexafluorobutyl acrylate, lauryl acrylate, hydroxyethyl acrylate, acrylic acid, 4-hydroxybutyl acrylate, polyethylene glycol diacrylate, isobornyl acrylate, methyl methacrylate, ethyl methacrylate, hydroxyethyl methacrylate, neopentyl glycol polymethylethylene oxide diacrylate, and tripropylene glycol diacrylate; Preferably, the acrylic functional monomer is hexafluorobutyl acrylate and / or lauryl acrylate and / or hydroxyethyl acrylate.
[0012] The photoinitiator of the present invention adopts a conventional photoinitiator for acrylate photocuring. Preferably, the photoinitiator is a free radical ultraviolet photoinitiator, including but not limited to one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, and 2,2-dimethoxy-phenylacetophenone; more preferably, the initiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0013] As a further improvement of the present invention, in step (2), in order to reduce the influence of oxygen on the UV light curing reaction, the dielectric elastomer mold preferably includes a lower support plate, an intermediate cushion frame and an upper transparent cover plate arranged in sequence from bottom to top.
[0014] Preferably, the material of the lower support plate is selected from metal, plastic, and glass, and the lower support plate is a thick plate with flat upper and lower surfaces, and its thickness is preferably 5-20 mm.
[0015] Preferably, the material of the intermediate cushion frame is selected from acrylic plastic, polytetrafluoroethylene, polyimide, and rubber; the intermediate cushion frame is a square ring frame or a circular ring frame. It should be noted that since the acrylate dielectric elastomer precursor solution is filled in the middle groove of the intermediate cushion frame, the thickness of the intermediate cushion frame determines the thickness of the final acrylate dielectric elastomer, so the thickness of the obtained dielectric elastomer can be adjusted by selecting intermediate cushion frames of different thicknesses.
[0016] Preferably, the material of the upper transparent cover plate is selected from transparent plastic and glass. The upper transparent cover plate is a thin plate with flat upper and lower surfaces, and its thickness is preferably 3-15 mm.
[0017] As a further improvement of the present invention, a release film is provided between the lower support plate and the intermediate cushion frame, and a release film is provided between the intermediate cushion frame and the upper transparent cover plate. The release film can be a PET release film or other release film commonly used in the prior art. By providing the release film, not only can the utilization efficiency of the lower support plate and the upper transparent cover plate be improved, the contact between oxygen and the precursor solution during UV light curing can be further reduced, and the storage, peeling, cutting and use of the dielectric elastomer can be facilitated.
[0018] In step (2), when applying the dielectric elastomer mold, first lay a layer of release film on the lower support plate, then place the middle cushion frame, inject a sufficient amount of acrylic ester dielectric elastomer precursor solution into the groove of the middle cushion frame, then slowly lay another layer of release film on top, and then cover it with an upper transparent cover plate, compact it, and then perform UV curing.
[0019] As a further improvement of the present invention, in step (3), the power of UV light curing is 100-1500 mW / cm 2 The curing time is 0.5 to 15 minutes; the UV light can be conventional UV light in the art, and preferably, the wavelength of the UV light is 265 to 420 nm.
[0020] According to a second aspect of the present invention, there is provided a broadband fast-response acrylate dielectric elastomer, which is prepared by the method for preparing the broadband fast-response acrylate dielectric elastomer.
[0021] According to a third aspect of the present invention, there is provided a use of the broadband and fast-response acrylic dielectric elastomer in a soft robot actuator.
[0022] The present invention adopts a method of photocuring a cross-linked network polymer formed by an acrylate cross-linking agent, an acrylate flexible monomer, and a functional monomer to prepare an acrylate dielectric elastomer. The flexible monomer and the cross-linking agent are chemically cross-linked to form an elastomer network skeleton. The flexible molecular chain of the flexible monomer has good flexibility, which plays a role in reducing the Young's modulus and keeps the elastomer at a high elongation at break, thereby ensuring that the dielectric elastomer can have a greater deformation capacity; the present invention innovatively adds a small amount of functional monomers to participate in the reaction to form nanocrystalline domains as the physical cross-linking part, which increases the cross-linking density of the elastomer, reduces viscoelasticity, and thereby improves its dynamic driving performance such as response speed and response frequency range. The present invention improves the performance of the acrylate dielectric elastomer through the synergistic effect of chemical and physical cross-linking, so that it can achieve a large driving strain while having a smaller viscoelasticity, a faster response speed, and a wider response frequency range.
[0023] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art: (1) The preparation method of the acrylate dielectric elastomer of the present invention adopts a method of photocuring an acrylate crosslinking agent and an acrylate flexible monomer and a functional monomer to form a crosslinked network polymer. Through the synergistic effect of chemical and physical crosslinking, it can achieve a large driving strain while having smaller viscoelasticity, faster response speed and wider response frequency range.
[0024] (2) The method for preparing the acrylic dielectric elastomer of the present invention uses a simple UV light curing method and adopts an improved dielectric elastomer mold to achieve reaction conditions close to an oxygen-free environment, thereby reducing the inhibitory effect of oxygen on the light curing reaction and improving the reaction efficiency.
[0025] (3) The acrylate dielectric elastomer prepared by the present invention promotes the application and development of acrylate dielectric elastomers in soft robot actuators, and greatly improves the driving effect and application potential of acrylate dielectric elastomers in soft robot actuators. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the structure of a dielectric elastomer mold according to an embodiment of the present invention; Figure 2 The static electrodeformation performance test results of the embodiments of the present invention and the comparative examples are shown in FIG. Figure 3 The dynamic multi-frequency electrodeformation performance result diagram of Example 2 of the present invention; Figure 4The dynamic multi-frequency electrodeformation performance result diagram of comparative example 1 of the present invention.
[0027] In all the drawings, the same reference numerals represent the same technical features, specifically: 1. upper transparent cover plate; 2. middle cushion frame; 3. lower support plate; 4. PET release film. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0029] In the specific embodiments of the present invention, unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art, and conventional methods and conditions may be used; unless otherwise specified, the materials, reagents, etc. used in the examples are all commercially available products.
[0030] Example 1 In this embodiment, the composition of the acrylate dielectric elastomer precursor solution is shown in Table 1.
[0031] Table 1 Composition of the acrylic dielectric elastomer precursor solution in Example 1
[0032] In this embodiment, the preparation method of the acrylate dielectric elastomer is as follows: (1) Stir and mix the acrylate crosslinking agent CN9021, acrylate flexible monomer (butyl acrylate), acrylate functional monomer (lauryl acrylate, hexafluorobutyl acrylate), and photoinitiator (2-hydroxy-2-methyl-1-phenyl-1-propanone) with a glass rod to obtain an acrylate dielectric elastomer precursor solution, and store it in a light-shielded place for later use; (2) The uniformly mixed acrylate dielectric elastomer precursor solution in step (1) is placed in a vacuum barrel, and the solution is completely vacuumed to remove bubbles; at the same time, an 8 mm thick lower support plate 3 (glass plate) is prepared and placed horizontally, a 0.125 mm thick PET release film 4 is laid on it, and a 1 mm thick acrylic intermediate cushion frame 2 is placed in the middle; then the uniformly mixed and bubble-free acrylate dielectric elastomer precursor solution is injected into the groove formed by the intermediate cushion frame 2 until the precursor solution slightly overflows the groove; after the precursor solution is self-leveled, a layer of PET release film 4 is slowly laid on top to ensure that there is no gap and no bubbles between the release film and the solution; then a 5 mm thick upper transparent cover plate 1 (glass plate) is gently covered and compacted with a manual flat press to ensure that the thickness of the precursor solution is consistent with the thickness of the intermediate cushion frame.
[0033] (3) Place the mold filled with the precursor solution in step (2) into the curing box and place it under UV curing power of 900mW / cm 2 , and cured for 10 minutes under the condition of UV wavelength of 365 nm. After UV curing, the dielectric elastomer material was peeled off from the surface of the release film to obtain a dielectric elastomer film material, which was recorded as sample 1 and stored for later use.
[0034] Example 2 The preparation method of the acrylate dielectric elastomer precursor solution and the dielectric elastomer material in this embodiment is the same as that in Embodiment 1, except that the composition of the acrylate dielectric elastomer precursor solution is shown in Table 2. The dielectric elastomer film material prepared in this embodiment is recorded as Sample 2.
[0035] Table 2 Composition of the acrylic dielectric elastomer precursor solution in Example 2
[0036] Example 3 The preparation method of the acrylate dielectric elastomer precursor solution and the dielectric elastomer material in this embodiment is the same as that in Embodiment 1, except that the composition of the acrylate dielectric elastomer precursor solution is shown in Table 3. The dielectric elastomer film material prepared in this embodiment is recorded as Sample 3.
[0037] Table 3 Composition of the acrylic dielectric elastomer precursor solution in Example 3
[0038] Comparative Example 1 The comparative example is a commercial acrylic dielectric elastomer: 3M VHB4910 (purchased from 3M Company).
[0039] Test Example 1 The electrodeformability of the film samples 1 to 3 prepared in Examples 1 to 3 and the VHB 4910 in Comparative Example 1 was tested using a circular film driver. In each example and comparative example, the initial thickness of the film was 1 mm, and the film sample was pre-stretched by 300% before the test. After the pre-stretching, the film thickness was 115±10 um. The pre-stretched film was fixed on an acrylic ring with an inner diameter of 5 cm, and the upper and lower surfaces of the middle area were coated with circular black carbon paste flexible electrodes with a diameter of 2 cm, and the area coated with the flexible electrodes was connected to a Trek 610E high voltage power supply using a silver-plated copper wire.
[0040] The static electrodeformation performance test method is as follows: The voltage was slowly increased from 0 kV, and an integrated smart camera (model VS-L160MX, Keyence, Japan) was used to track the driving changes of the circular thin film actuator in real time, and the area changes of the black carbon paste flexible electrode area in the middle of the actuator under different voltages were recorded until the sample broke down. act The calculation formula is as follows: S act = ×100% In the formula, A act A0 is the area of the electrode when the electric field is applied, and A1 is the area of the electrode when the electric field is not applied.
[0041] The static electrodeformation performance test results of the film samples 1-3 prepared in Examples 1-3 and Comparative Example 1 (VHB4910) are as follows: Figure 2 As shown. It can be seen that under a driving voltage of 6 kV, the maximum electro-induced area strain of sample 2 reaches 145.1%; the maximum electro-induced area strain of sample 3 reaches 122.4%. However, the maximum electro-induced area strain of the commercially available acrylic dielectric elastomer VHB 4910 under a driving voltage of 6.5 kV only reaches 109.2%. At an operating voltage of 5.0 kV, the electro-induced area strain of sample 1 reaches 78.1%, the electro-induced area strain of sample 2 reaches 54.2%, and the electro-induced area strain of sample 3 reaches 43.3%, all of which are greater than the electro-induced area strain of 30.5% of the commercially available acrylic dielectric elastomer VHB4910.
[0042] The above results show that the advantage of the dielectric elastomer material of the embodiment of the present invention is that, under the same circular thin film actuator manufacturing process conditions, compared with the commercially available acrylic dielectric elastomer (VHB 4910), a larger electro-induced area strain can be achieved, and the maximum is 145.1%.
[0043] Test Example 2 The circular thin film driver in Experimental Example 1 was used to test the dynamic driving effect of the thin film sample 2 prepared in Example 2 and the comparative example 1 (VHB4910) at different frequencies. A signal generator was added to generate a square wave frequency signal, which was amplified 1000 times by the amplifier function of the Trek 610E high voltage power supply and acted on the circular thin film driver. The electroinduced area strain S act The calculation formula is the same as above.
[0044] The dynamic multi-frequency electrodeformation performance test results of the film sample 2 prepared in Example 2 and the comparative example 1 (VHB4910) are as follows: Figure 3 and Figure 4 As shown. It can be seen that at a frequency of 0.1 Hz, Example 2 has reached the maximum electro-induced area strain of 31.2% under this frequency cycle almost in the first cycle, and the response speed is fast; while the maximum electro-induced area strain of Comparative Example 1 has been gradually increasing in 9 cycles, and finally did not reach the steady-state value, and the response lag phenomenon is obvious. With the increase of the driving frequency, the maximum electro-induced area strain of the two materials shows different degrees of attenuation. At a frequency of 20 Hz, the maximum electro-induced area strain in the dynamic actuation cycle of Example 2 is 24.3%, and the residual area strain is 7.5%. It still has a driving range of 16.8% electro-induced area strain, which can achieve the driving effect; while the maximum electro-induced area strain of Comparative Example 1 is 12.0%, and the residual area strain is 10.0%, leaving only 2% of the electro-induced area strain driving range, which seriously affects the driving effect.
[0045] The above results show that the advantage of the dielectric elastomer material of the embodiment of the present invention is that, compared with the commercially available acrylic dielectric elastomer (VHB 4910), it has a faster response speed and a wider response frequency range.
[0046] It is easy for a person skilled in the art to understand that "comprising", "including", "having", "containing", etc. used herein are all open terms, that is, they mean including but not limited to. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper limit and the lower limit of the range is also specifically disclosed. Each smaller range between any stated value or intermediate value in the stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the range.
[0047] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a broadband fast-response acrylic dielectric elastomer, characterized in that: The steps include: (1) uniformly mixing an acrylate crosslinking agent, an acrylate flexible monomer, an acrylate functional monomer, and a photoinitiator to form an acrylate dielectric elastomer precursor solution; (2) After vacuuming the acrylate dielectric elastomer precursor solution to remove bubbles, the solution is injected into a dielectric elastomer mold having a groove; (3) The acrylic dielectric elastomer is obtained after UV light curing.
2. The method for preparing a broadband fast-response acrylic dielectric elastomer according to claim 1, characterized in that: The acrylate dielectric elastomer precursor solution includes the following components in percentage by mass: 40~60% acrylic crosslinker, 20~35% acrylate flexible monomer, 10~25% acrylate functional monomer, 0.5~3% photoinitiator.
3. The method for preparing a broadband fast-response acrylic dielectric elastomer according to claim 1, characterized in that: The acrylate crosslinking agent is selected from any one or more of a polyester acrylate crosslinking agent, a polyether acrylate crosslinking agent, an epoxy acrylate crosslinking agent, and a polyurethane acrylate crosslinking agent; Preferably, the acrylic crosslinking agent is a polyurethane acrylate crosslinking agent CN9021 containing two functional groups.
4. The method for preparing a broadband fast-response acrylic dielectric elastomer according to claim 1, characterized in that: The acrylic ester flexible monomer is selected from any one or more of ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, isooctyl acrylate, decyl acrylate, and isodecyl acrylate; and / or, The acrylate functional monomer is selected from any one or more of hexafluorobutyl acrylate, lauryl acrylate, hydroxyethyl acrylate, acrylic acid, 4-hydroxybutyl acrylate, polyethylene glycol diacrylate, isobornyl acrylate, methyl methacrylate, ethyl methacrylate, hydroxyethyl methacrylate, neopentyl glycol polymethylethylene oxide diacrylate, and tripropylene glycol diacrylate; Preferably, the acrylic flexible monomer is butyl acrylate and / or isooctyl acrylate; Preferably, the acrylic functional monomer is any one or more of hexafluorobutyl acrylate, lauryl acrylate, and hydroxyethyl acrylate.
5. The method for preparing a broadband fast-response acrylic dielectric elastomer according to claim 1, characterized in that: The photoinitiator is a free radical ultraviolet photoinitiator; Preferably, the photoinitiator is selected from any one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, and 2,2-dimethoxy-phenylacetophenone.
6. The method for preparing a broadband fast-response acrylic dielectric elastomer according to any one of claims 1 to 5, characterized in that: In step (2), the dielectric elastomer mold includes a lower support plate, an intermediate cushion frame, and an upper transparent cover plate arranged in sequence from bottom to top; The material of the lower support plate is selected from metal, plastic, and glass; and / or, The intermediate cushion frame is a square ring frame or a circular ring frame, and the material of the intermediate cushion frame is selected from acrylic plastic, polytetrafluoroethylene, polyimide, and rubber; and / or, The material of the upper transparent cover is selected from transparent plastic and glass; Preferably, the thickness of the lower support plate is 5-20 mm, and the thickness of the upper transparent cover plate is 3-15 mm.
7. The method for preparing a broadband fast-response acrylic dielectric elastomer according to claim 6, characterized in that: A release film is provided between the lower supporting plate and the middle cushion layer frame, and a release film is provided between the middle cushion layer frame and the upper transparent cover plate.
8. The method for preparing a broadband fast-response acrylic dielectric elastomer according to any one of claims 1 to 5 or 7, characterized in that: In step (3), the power of UV light curing is 100~1500mW / cm 2 The curing time is 0.5~15min, and the wavelength of UV light is 265~420nm.
9. A broadband fast-response acrylic dielectric elastomer, characterized in that: The invention is prepared by the method for preparing a broadband fast-response acrylic dielectric elastomer according to any one of claims 1 to 8.
10. Use of the broadband fast-response acrylic dielectric elastomer as claimed in claim 9 in a soft robot actuator.
Citation Information
Patent Citations
Dielectric elastomer composite material, dielectric elastomer prepolymer, preparation method and application
CN111690094A
Acrylate dielectric elastomer and preparation method thereof
CN112375183A
Thermosetting dielectric elastomer film and dielectric driver thereof
CN114181417A
Dielectric elastomeric material
US20220135711A1
Cited By
Hydrophobic elastomer as well as preparation method and application thereof
CN119463015A
Dual-network acrylate dielectric elastomer as well as preparation method and application thereof
CN119798555A
Dual-network acrylate elastomers, methods of making and using the same
CN119798555B