Preparation method and application of amino-terminated quaternary ammonium salt polymer material
By synthesizing end amino quaternary ammonium polymers and undergoing thermal curing reaction with epoxy resin, the problem of insufficient toughness and antibacterial properties of epoxy resin materials is solved, and the effect of improving material toughness and antibacterial properties is achieved.
Patent Information
- Application Number
- CN202411107248.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Epoxy resin materials have poor toughness and lack of antibacterial properties, which limit their application in the fields of antibacterial products and medical supplies.
Using a preparation method of end amino quaternary ammonium salt polymer material, the Boc aminobenzene quaternary ammonium salt compound is synthesized by etherification and quaternization reaction, and polymerized with isocyanate monomer and polyol, and trifluoroacetic acid is added to remove protection. The group is used to obtain a terminal amino quaternary ammonium salt polymer with antibacterial properties, which is then heat-cured with the epoxy resin to form a toughener to improve the toughness and antibacterial properties of the epoxy resin.
It improves the elongation and impact strength of epoxy resins, and gives them significant antibacterial properties, making them have wide application prospects in the fields of antibacterial products and medical supplies.
Smart Images

Figure BDA0004991176310000022 
Figure BDA0004991176310000032 
Figure BDA0004991176310000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a preparation method and application of an amino-terminated quaternary ammonium salt polymer material. Background Art
[0002] At present, the amino-terminated materials on the market are mainly polyetheramines, which are polymers with a polyether structure as the main chain and an amine group as the terminal active functional group. Polyetheramines are obtained by ammoniation of polyethylene glycol, polypropylene glycol or ethylene glycol / propylene glycol copolymer under high temperature and high pressure. They have been widely used in many fields such as polyurea spraying, large composite materials, epoxy resin curing agents and automotive gasoline detergents. However, polyetheramines usually require high temperature and high pressure reaction conditions, and the reaction conditions are relatively complicated.
[0003] Epoxy resin has high strength, excellent insulation performance, and good curing performance. It is widely used in adhesives, coatings, etc. However, traditional epoxy resin does not have antibacterial properties, which limits its practical application in antibacterial products, medical supplies, etc. In addition, epoxy resin has the problem of brittleness and poor toughness. Polyurethane is a type of polymer material with high elasticity and good toughness, and has broad application prospects in the toughening and modification of epoxy resin. The master's thesis "Research on Amine-Terminated Polyurethane Toughened Epoxy Resin Adhesives" discloses that the reaction of polyethylene glycol, toluene diisocyanate, and meta-phenylenediamine to obtain an amine-terminated polyurethane can improve the toughness, strength and other properties of epoxy resin. However, the paper did not give epoxy resin antibacterial properties. Summary of the invention
[0004] The invention provides a preparation method and application of an amino-terminated quaternary ammonium salt polymer material, which solves the problem that epoxy resin has poor toughness and no antibacterial property.
[0005] The technical scheme is: a preparation method of an amino-terminated quaternary ammonium salt polymer material, which comprises the following steps: adding polyol into a flask, vacuum drying and dehydration, introducing nitrogen, adding isocyanate monomer, heating to 80-90°C, stirring and reacting for 2-5h, then adding a viscosity reducer, lowering the temperature to 35-60°C, adding a Boc aminophenyl quaternary ammonium salt compound and dibutyltin dilaurate, reacting for 2-3h, rotary evaporation, then adding dichloromethane, stirring and dispersing, then adding trifluoroacetic acid, stirring and reacting at room temperature for 18-24h, rotary evaporation, washing with a sodium bicarbonate solution and ethanol in sequence, and drying to obtain the amino-terminated quaternary ammonium salt polymer material.
[0006] The general chemical formula of the amino quaternary ammonium salt compound is as shown in formula (I):
[0007] Where n=8-16.
[0008] Preferably, the molar ratio of the polyol, the isocyanate monomer, and the Boc aminophenyl quaternary ammonium salt compound is 1:(2-3):(2-2.6). The polyol is a polyether polyol, a polyester polyol, or a vegetable oil polyol; the molecular weight of the polyol is 1000-3000. The isocyanate monomer is toluene-2,4-diisocyanate, isophorone diisocyanate, diphenylmethane-4,4'-diisocyanate, or isophorone diisocyanate.
[0009] Preferably, the amount of the viscosity reducer added is 10-20% of the total mass of the polyol and the isocyanate monomer. The viscosity reducer is one or a combination of acetone, ethyl acetate, dichloromethane, 1,2-dichloroethane, benzene, toluene, and xylene.
[0010] Preferably, the preparation method of Boc aminophenyl quaternary ammonium salt compound is:
[0011] Step (1), add (4-hydroxyphenyl) carbamic acid tert-butyl ester, water, polyethylene glycol 400 to a flask, add epichlorohydrin dropwise after stirring, add potassium hydroxide aqueous solution dropwise after stirring, wherein the molar ratio of (4-hydroxyphenyl) carbamic acid tert-butyl ester, water, polyethylene glycol 400, epichlorohydrin, potassium hydroxide is 1: (0.045-0.05): (2.5-3.2): (2.5-3.2), heat to 80-95 ° C, react for 4-10 hours, cool, add hydrochloric acid solution to neutralize, then add dichloromethane to extract, collect the organic phase, dry over anhydrous sodium sulfate, rotary evaporate, wash with petroleum ether, and obtain Boc aminophenyl glycidyl ether. The reaction formula is:
[0012]
[0013] Step (2), add isopropanol, water, Boc aminophenyl glycidyl ether to a flask, add HCl aqueous solution dropwise, stir and add N,N-dimethylalkylamine, wherein the molar ratio of Boc aminophenyl glycidyl ether, HCl, and N,N-dimethylalkylamine is 1:1:(0.9-1.1), and the structural formula of N,N-dimethylalkylamine is wherein n=8-16; heating to 55-70°C, reacting for 1-2h, removing isopropanol by rotary evaporation, precipitating a precipitate, filtering, washing with petroleum ether, and recrystallizing the product in ethanol to obtain a Boc aminophenyl quaternary ammonium salt compound. The reaction formula is:
[0014]
[0015] Preferably, the amino-terminated quaternary ammonium salt polymer material is used in the epoxy resin, and the amount of the amino-terminated quaternary ammonium salt polymer material is 10-30% of the epoxy resin.
[0016] The technical effect of the present invention is that: the present invention uses potassium hydroxide as a catalyst and polyethylene glycol 400 as a phase transfer catalyst to carry out an etherification reaction on tert-butyl (4-hydroxyphenyl)carbamate and epichlorohydrin, and then carries out a quaternization reaction with N,N-dimethylalkylamine and HCl to obtain a novel Boc aminophenyl quaternary ammonium salt compound containing a hydroxyl group.
[0017] The invention uses toluene-2,4-diisocyanate, isophorone diisocyanate and the like as isocyanate monomers, and carries out polymerization reaction with polyols such as polyether polyol and polyester polyol to obtain an isocyanate-terminated polyurethane prepolymer, which is then reacted with the hydroxyl group of a Boc aminophenyl quaternary ammonium salt compound, and finally the Boc protecting group is removed by trifluoroacetic acid to obtain a polyurethane-based polymer material containing an amino group and a quaternary ammonium salt group at the terminal.
[0018] The present invention uses an amino-terminated quaternary ammonium salt polymer material as a toughening agent and adds it to the epoxy resin. The polyurethane itself has the advantages of high elasticity and good toughness, and contains amino groups at both ends, which can undergo a thermal curing reaction with the epoxy resin, thereby grafting the polyurethane flexible molecular chain into the epoxy resin to form a flexible cured cross-linking network, which has a good toughening effect and improves the elongation at break and the impact strength of the epoxy resin.
[0019] The amino-terminated quaternary ammonium salt polymer material of the present invention contains a unique quaternary ammonium salt group, which can interact with the negatively charged cell membrane of bacteria, change the permeability of the cell membrane, and allow substances inside the bacterial cell membrane to overflow, thereby killing the bacteria and making the epoxy resin material exhibit good antibacterial properties. DETAILED DESCRIPTION
[0020] In order to make the purpose, implementation mode and advantages of the present application clearer, the exemplary implementation mode of the present application will be clearly and completely described below in combination with the exemplary embodiments of the present application. Obviously, the described exemplary embodiments are only part of the embodiments of the present application, rather than all the embodiments.
[0021] Example 1
[0022] Step (1), add 40mmol (4-hydroxyphenyl) tert-butyl carbamate, 10mL water, 1.8mmol polyethylene glycol 400 into a flask, add 128mmol epichlorohydrin dropwise after stirring, add 40mL aqueous solution containing 128mmol potassium hydroxide dropwise after stirring, heat to 95°C, react for 6h, cool, add hydrochloric acid solution to neutralize, then add dichloromethane to extract, collect the organic phase, dry over anhydrous sodium sulfate, rotary evaporate, wash with petroleum ether to obtain Boc aminophenyl glycidyl ether.
[0023] Step (2), add 80mL isopropanol, 70mL water, 40mmol Boc aminophenyl glycidyl ether to a flask, dropwise add 4mL 10mol / L HCl aqueous solution, stir and add 44mmol N,N-dimethyl n-octylamine, heat to 55°C, react for 2h, remove isopropanol by rotary evaporation, precipitate, filter, wash with petroleum ether, and recrystallize the product in ethanol to obtain a Boc aminophenyl quaternary ammonium salt compound. The structural formula is:
[0024] Step (3), add 10mmol polyethylene glycol 1000 as polyether polyol to the flask, vacuum dry and dehydrate, introduce nitrogen, add 23mmol toluene-2,4-diisocyanate, heat to 85°C, stir and react for 4h, then add viscosity reducer acetone, the amount of viscosity reducer added is 20% of the total mass of polyol and isocyanate monomer; the temperature is reduced to 40°C, add 23mmol Boc aminophenyl quaternary ammonium salt compound, dibutyltin dilaurate, react for 3h, rotary evaporate, then add 300mL dichloromethane, stir and disperse, then add 120mL trifluoroacetic acid, stir and react at room temperature for 24h, rotary evaporate, wash with sodium bicarbonate solution and ethanol in turn, dry, and obtain terminal amino quaternary ammonium salt polymer material. The reaction formula is:
[0025]
[0026] Step (4), add 100g epoxy resin E44, 5g ethylenediamine curing agent, and 10g terminal amino quaternary ammonium salt polymer material into a container, stir to mix, then cast into a mold, vacuum degassing, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0027] Example 2
[0028] Step (1), add 40mmol (4-hydroxyphenyl) tert-butyl carbamate, 10mL water, 2mmol polyethylene glycol 400 into a flask, stir and dropwise add 128mmol epichlorohydrin, stir and dropwise add 40mL aqueous solution containing 128mmol potassium hydroxide, heat to 85°C, react for 10h, cool, add hydrochloric acid solution to neutralize, then add dichloromethane to extract, collect the organic phase, dry over anhydrous sodium sulfate, rotary evaporate, wash with petroleum ether to obtain Boc aminophenyl glycidyl ether.
[0029] Step (2), add 80mL isopropanol, 70mL water, 40mmol Boc aminophenyl glycidyl ether to a flask, dropwise add 4mL 10mol / L HCl aqueous solution, stir and add 36mmol dodecyldimethyl tertiary amine, heat to 70°C, react for 1h, remove isopropanol by rotary evaporation, precipitate, filter, wash with petroleum ether, and recrystallize the product in ethanol to obtain a Boc aminophenyl quaternary ammonium salt compound. The structural formula is
[0030] Step (3), add 10mmol polycarbonate diol 1000 as polyester polyol into a flask, vacuum dry and dehydrate, introduce nitrogen, add 26mmol isophorone diisocyanate, heat to 85°C, stir and react for 4h, then add dichloromethane as a viscosity reducer, the amount of the viscosity reducer added is 20% of the total mass of the polyol and isocyanate monomers; the temperature is reduced to 35°C, 26mmol Boc aminophenyl quaternary ammonium salt compound and dibutyltin dilaurate are added, react for 3h, rotary evaporate, then add 300mL dichloromethane, stir and disperse, then add 120mL trifluoroacetic acid, stir and react at room temperature for 24h, rotary evaporate, wash with sodium bicarbonate solution and ethanol in turn, and dry to obtain an amino-terminated quaternary ammonium salt polymer material.
[0031] Step (4), add 100g epoxy resin E44, 5g ethylenediamine curing agent, and 15g terminal amino quaternary ammonium salt polymer material into a container, stir and mix, then cast into a mold, vacuum degassing, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0032] Example 3
[0033] Step (1), add 40mmol (4-hydroxyphenyl) tert-butyl carbamate, 10mL water, 2mmol polyethylene glycol 400 into a flask, add 100mmol epichlorohydrin dropwise after stirring, add 40mL aqueous solution containing 100mmol potassium hydroxide dropwise after stirring, heat to 95°C, react for 4h, cool, add hydrochloric acid solution to neutralize, then add dichloromethane to extract, collect the organic phase, dry over anhydrous sodium sulfate, rotary evaporate, wash with petroleum ether to obtain Boc aminophenyl glycidyl ether.
[0034] Step (2), add 80mL of isopropanol, 70mL of water, and 40mmol of Boc aminophenyl glycidyl ether into a flask, dropwise add 4mL of 10mol / L HCl aqueous solution, stir, add 44mmol of dodecyldimethyl tertiary amine, heat to 60°C, react for 2h, remove isopropanol by rotary evaporation, precipitate, filter, wash with petroleum ether, and recrystallize the product in ethanol to obtain a Boc aminophenyl quaternary ammonium salt compound.
[0035] Step (3), adding 10mmol of polytetrahydrofuran ether diol as a polyether polyol into a flask, vacuum drying and dehydration, introducing nitrogen, adding 30mmol of diphenylmethane-4,4'-diisocyanate, heating to 90°C, stirring and reacting for 2h, then adding a viscosity reducer ethyl acetate, wherein the amount of the viscosity reducer added is 20% of the total mass of the polyol and the isocyanate monomer; the temperature is reduced to 60°C, adding 26mmol of Boc aminophenyl quaternary ammonium salt compound and dibutyltin dilaurate, reacting for 2h, rotary evaporation, then adding 300mL of dichloromethane, stirring and dispersing, and then adding 120mL of trifluoroacetic acid, stirring and reacting at room temperature for 18h, rotary evaporation, washing with sodium bicarbonate solution and ethanol in turn, and drying to obtain an amino-terminated quaternary ammonium salt polymer material.
[0036] Step (4), add 100g epoxy resin E44, 5g ethylenediamine curing agent, and 20g terminal amino quaternary ammonium salt polymer material into a container, stir and mix, then cast into a mold, vacuum degass, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0037] Example 4
[0038] Step (1), add 40mmol (4-hydroxyphenyl) tert-butyl carbamate, 10mL water, 2mmol polyethylene glycol 400 into a flask, add 110mmol epichlorohydrin dropwise after stirring, add 40mL aqueous solution containing 110mmol potassium hydroxide dropwise after stirring, heat to 80°C, react for 10h, cool, add hydrochloric acid solution to neutralize, then add dichloromethane to extract, collect the organic phase, dry over anhydrous sodium sulfate, rotary evaporate, wash with petroleum ether to obtain Boc aminophenyl glycidyl ether.
[0039] Step (2), add 80mL of isopropanol, 70mL of water, and 40mmol of Boc aminophenyl glycidyl ether into a flask, dropwise add 4mL of 10mol / L HCl aqueous solution, stir, add 40mmol of hexadecyldimethyl tertiary amine, heat to 55°C, react for 2h, remove isopropanol by rotary evaporation, precipitate, filter, wash with petroleum ether, and recrystallize the product in ethanol to obtain a Boc aminophenyl quaternary ammonium salt compound.
[0040] Step (3), adding 10mmol polyethylene glycol 1000 as a polyether polyol into a flask, vacuum drying and dehydration, introducing nitrogen, adding 23mmol toluene-2,4-diisocyanate, heating to 80°C, stirring and reacting for 5h, then adding a viscosity reducer xylene, wherein the amount of the viscosity reducer added is 10% of the total mass of the polyol and isocyanate monomers; the temperature is reduced to 60°C, 23mmol Boc aminophenyl quaternary ammonium salt compound and dibutyltin dilaurate are added, reacting for 3h, rotary evaporation, then adding 300mL dichloromethane, stirring and dispersing, and then adding 120mL trifluoroacetic acid, stirring and reacting at room temperature for 24h, rotary evaporation, washing with sodium bicarbonate solution and ethanol in turn, and drying to obtain an amino-terminated quaternary ammonium salt polymer material.
[0041] Step (4), add 100g epoxy resin E44, 5g ethylenediamine curing agent, and 25g terminal amino quaternary ammonium salt polymer material into a container, stir and mix, then cast into a mold, vacuum degassing, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0042] Example 5
[0043] Step (1), add 40mmol (4-hydroxyphenyl) tert-butyl carbamate, 10mL water, 1.8mmol polyethylene glycol 400 into a flask, stir and drop 128mmol epichlorohydrin, stir and drop 40mL aqueous solution containing 128mmol potassium hydroxide, heat to 85°C, react for 8h, cool, add hydrochloric acid solution to neutralize, then add dichloromethane to extract, collect the organic phase, dry over anhydrous sodium sulfate, rotary evaporate, wash with petroleum ether to obtain Boc aminophenyl glycidyl ether.
[0044] Step (2), add 80mL isopropanol, 70mL water, 40mmol Boc aminophenyl glycidyl ether to a flask, dropwise add 4mL 10mol / L HCl aqueous solution, stir, add 40mmol hexadecyl dimethyl tertiary amine, heat to 65°C, react for 1h, remove isopropanol by rotary evaporation, precipitate, filter, wash with petroleum ether, and recrystallize the product in ethanol to obtain a Boc aminophenyl quaternary ammonium salt compound. The structural formula is
[0045] Step (3), adding 10mmol polycaprolactone diol 1000 as polyester polyol into a flask, vacuum drying and dehydration, introducing nitrogen, adding 20mmol isophorone diisocyanate, heating to 80°C, stirring and reacting for 4h, then adding dichloromethane as a viscosity reducer, wherein the amount of the viscosity reducer added is 10% of the total mass of the polyol and isocyanate monomers; the temperature is reduced to 35°C, 20mmol Boc aminophenyl quaternary ammonium salt compound and dibutyltin dilaurate are added, reacting for 2h, rotary evaporation, then adding 300mL dichloromethane, stirring and dispersing, and then adding 120mL trifluoroacetic acid, stirring and reacting at room temperature for 24h, rotary evaporation, washing with sodium bicarbonate solution and ethanol in turn, and drying to obtain an amino-terminated quaternary ammonium salt polymer material.
[0046] Step (4), add 100g epoxy resin E44, 5g ethylenediamine curing agent, and 30g terminal amino quaternary ammonium salt polymer material into a container, stir and mix, then cast into a mold, vacuum degass, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0047] The difference between Comparative Example 1 and Example 1 is that no amino-terminated quaternary ammonium salt polymer material is added to the epoxy resin material. Specifically:
[0048] Step (1), add 100g epoxy resin E44 and 5g ethylenediamine curing agent into a container, stir to mix, then cast into a mold, vacuum degas, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0049] The difference between Comparative Example 2 and Example 1 is that when preparing the quaternary ammonium salt polymer material, trifluoroacetic acid is not used to remove the Boc protecting group. Specifically:
[0050] Step (1), adding 10mmol polyethylene glycol 1000 as a polyether polyol into a flask, vacuum drying and dehydration, introducing nitrogen, adding 23mmol toluene-2,4-diisocyanate, heating to 85°C, stirring and reacting for 4h, then adding viscosity reducer acetone, the amount of the viscosity reducer added is 20% of the total mass of the polyol and isocyanate monomers; the temperature is reduced to 40°C, adding 23mmol Boc aminophenyl quaternary ammonium salt compound and dibutyltin dilaurate, reacting for 3h, rotary evaporation, ethanol washing, and drying to obtain a quaternary ammonium salt polymer material.
[0051] Step (2), add 100g epoxy resin E44, 5g ethylenediamine curing agent, and 10g quaternary ammonium salt polymer material into a container, stir and mix, then cast into a mold, vacuum degass, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0052] The difference between Comparative Example 3 and Example 1 is that when preparing the amino-terminated polymer material, N-Boc-ethanolamine (structural formula: ) replaces the Boc aminophenyl quaternary ammonium salt compound, specifically:
[0053] Step (1), adding 10mmol polyethylene glycol 1000 as a polyether polyol into a flask, vacuum drying and dehydration, introducing nitrogen, adding 23mmol toluene-2,4-diisocyanate, heating to 85°C, stirring and reacting for 4h, then adding a viscosity reducer acetone, wherein the amount of the viscosity reducer added is 20% of the total mass of the polyol and isocyanate monomers; the temperature is reduced to 40°C, 23mmol N-Boc-ethanolamine and dibutyltin dilaurate are added, reacting for 3h, rotary evaporation, then adding 300mL dichloromethane, stirring and dispersing, and then adding 120mL trifluoroacetic acid, stirring and reacting at room temperature for 24h, rotary evaporation, washing with sodium bicarbonate solution and ethanol in turn, and drying to obtain an amino-terminated polymer material.
[0054] Step (2), add 100g epoxy resin E44, 5g ethylenediamine curing agent, and 10g terminal amino polymer material into a container, stir to mix, then cast into a mold, vacuum degas, place in a heating box, first cure at 80°C for 4h, then cure at 130°C for 5h, demold, and obtain an epoxy resin material.
[0055] The tensile properties, flexural strength and impact strength of epoxy resin materials are tested according to GB / T 2567-2021. The test results are shown in the table below.
[0056]
[0057]
[0058] As can be seen from the above table, compared with Comparative Example 1, the polyurethane-based polymer with terminal amino groups is added to the epoxy resin of Examples 1-5. The polyurethane itself has the advantages of high elasticity and good toughness, and it contains amino groups at both ends, which can react with the epoxy resin to undergo a thermal curing reaction, thereby grafting the polyurethane flexible molecular chain into the epoxy resin to form a flexible cured cross-linked network, which has a good toughening effect, and the elongation at break reaches 10.1-23.5%, and the impact strength reaches 13.6-26.4 kJ / m 2 .
[0059] In Comparative Example 2, when preparing the quaternary ammonium salt polymer material, trifluoroacetic acid is not used to remove the Boc protecting group. The obtained polyurethane-based polymer does not contain terminal amino groups and cannot undergo a curing reaction with the epoxy resin. The particle compatibility is poor, the toughening effect on the epoxy resin is poor, and the elongation at break and impact strength are low.
[0060] In Comparative Example 3, when preparing the terminal amino polymer material, N-Boc-ethanolamine is used instead of the Boc aminophenyl quaternary ammonium salt compound. The obtained polyurethane-based polymer contains a terminal amino group and can undergo a thermal curing reaction with the epoxy resin to form a flexible cured cross-linking network, which has a good toughening effect and significantly improves the elongation at break and impact strength of the epoxy resin.
[0061] The epoxy resin material was poured onto the tinplate surface, first cured at 80°C for 4 hours, then cured at 130°C for 5 hours to form an epoxy resin film, and then sterilized by ultraviolet light; Staphylococcus aureus, Escherichia coli, and Candida albicans were cultured and activated at 37°C for 24 hours to prepare bacterial suspensions (concentration of 10 6 cfu / mL); 0.1mL of bacterial suspension was spread on the surface of agar medium, and then the epoxy resin film was attached to the surface of agar medium, placed in an incubator, cultured at 37℃ for 24h, and the diameter of the inhibition zone was measured. Each group of samples was tested 3 times and the average value was taken. The test results are shown in the table below.
[0062]
[0063] It can be seen from the above table that the epoxy resin film materials of Examples 1-5 all show obvious inhibition zone diameters for Staphylococcus aureus, Escherichia coli, and Candida albicans, and have excellent antibacterial properties. This is because the added terminal amino quaternary ammonium salt polymer material contains a unique quaternary ammonium salt group, which can interact with the negatively charged cell membrane of the bacteria, change the permeability of the cell membrane, and allow the substances inside the bacterial cell membrane to overflow, thereby killing the bacteria and showing good antibacterial properties.
[0064] In Comparative Example 1, no amino-terminated quaternary ammonium salt polymer material was added, and the epoxy resin material did not show the diameter of the inhibition zone and the antibacterial property.
[0065] The quaternary ammonium salt polymer material added in Comparative Example 2 can also improve the antibacterial properties of the epoxy resin material, showing an obvious inhibition zone diameter.
[0066] In Comparative Example 3, when preparing the amino-terminated polymer material, N-Boc-ethanolamine was used instead of the Boc aminophenyl quaternary ammonium salt compound. The obtained amino-terminated polymer material did not contain antibacterial quaternary ammonium salt groups, and the epoxy resin material did not show the inhibition zone diameter and antibacterial properties.
[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an amino-terminated quaternary ammonium salt polymer material, It is characterized in that The preparation method is as follows: add polyol to a flask, vacuum dry and dehydrate, introduce nitrogen, add isocyanate monomer, heat to 80-90° C., stir and react for 2-5 hours, then add viscosity reducer, reduce the temperature to 35-60° C., add Boc aminophenyl quaternary ammonium salt compound and dibutyltin dilaurate, react for 2-3 hours, rotary evaporate, then add dichloromethane, stir and disperse, then add trifluoroacetic acid, stir and react at room temperature for 18-24 hours, rotary evaporate, wash with sodium bicarbonate solution and ethanol in sequence, and dry to obtain an amino-terminated quaternary ammonium salt polymer material; The general chemical formula of the amino quaternary ammonium salt compound is shown in formula (I): Where n=8-16.
2. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 1, It is characterized in that The molar ratio of the polyol, the isocyanate monomer and the Boc aminophenyl quaternary ammonium salt compound is 1:(2-3):(2-2.6).
3. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 1, It is characterized in that The polyol is polyether polyol, polyester polyol or vegetable oil polyol; the molecular weight of the polyol is 1000-3000.
4. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 1, It is characterized in that The isocyanate monomer is toluene-2,4-diisocyanate, isophorone diisocyanate, diphenylmethane-4,4'-diisocyanate or isophorone diisocyanate.
5. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 1, It is characterized in that The added amount of the viscosity reducer is 10-20% of the total mass of the polyol and the isocyanate monomer.
6. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 5, It is characterized in that The viscosity reducing agent is one or a combination of acetone, ethyl acetate, dichloromethane, 1,2-dichloroethane, benzene, toluene and xylene.
7. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 2, It is characterized in that The preparation method of the Boc aminophenyl quaternary ammonium salt compound is: Step (1), add tert-butyl (4-hydroxyphenyl)carbamate, water, polyethylene glycol 400 into a flask, add epichlorohydrin dropwise after stirring, add potassium hydroxide aqueous solution dropwise after stirring, heat to 80-95° C., react for 4-10 hours, cool, add hydrochloric acid solution to neutralize, then add dichloromethane to extract, collect the organic phase, dry over anhydrous sodium sulfate, rotary evaporate, wash with petroleum ether to obtain Boc aminophenyl glycidyl ether; Step (2), add isopropanol, water, Boc aminophenyl glycidyl ether into a flask, add HCl aqueous solution dropwise, add N,N-dimethylalkylamine after stirring, heat to 55-70° C., react for 1-2 hours, remove isopropanol by rotary evaporation, precipitate, filter, wash with petroleum ether, and recrystallize the product in ethanol to obtain a Boc aminophenyl quaternary ammonium salt compound.
8. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 7, It is characterized in that In the step (1), the molar ratio of tert-butyl (4-hydroxyphenyl)carbamate, water, polyethylene glycol 400, epichlorohydrin and potassium hydroxide is 1:(0.045-0.05):(2.5-3.2):(2.5-3.2).
9. The method for preparing the amino-terminated quaternary ammonium salt polymer material according to claim 7, It is characterized in that In the step (1), the molar ratio of Boc aminophenyl glycidyl ether, HCl, and N,N-dimethylalkylamine is 1:1:(0.9-1.1); the structural formula of N,N-dimethylalkylamine is Where n=8-16.
10. Use of the amino-terminated quaternary ammonium salt polymer material obtained by the preparation method according to any one of claims 1 to 9 in epoxy resin, It is characterized in that The amount of the amino-terminated quaternary ammonium salt polymer material is 10-30% of the epoxy resin.
Citation Information
Patent Citations
Cyclic carbonate group-terminated polyurethane prepolymer and preparation method and application thereof
CN112011029A
Dendritic macromolecular quaternary ammonium salt compound, preparation method and application thereof
CN112080011A
Amino-terminated polyether, preparation method of amino-terminated polyether and preparation method of polyurethane toughened epoxy resin
CN117720717A
Preparation method and application of two-component anticorrosive antibacterial adhesive