Preparation method and application of organic long-afterglow elastic film

By doping the fused ring compound into the flexible polymer, an organic long afterglow elastic film with high efficiency luminescence and excellent tensile properties is prepared, which solves the problem that materials in the prior art are difficult to take into account both luminescence and tensile properties, and achieves a large amount of Area coating and uniform luminescence, suitable for flexible display and anti-counterfeiting fields.

CN118930921APending Publication Date: 2024-11-12HEFEI HUISHI TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205006.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing long afterglow materials are difficult to balance efficient luminescence and excellent tensile properties, which limits their applications in flexible displays, wearable devices and high-end anti-counterfeiting fields.

Method used

Doping the fused ring compound such as benzophenylade or tetraphenyl into the flexible polymer styrene-ethylene-butene-styrene, an organic long afterglow elastic film is prepared by solution drop coating, utilizing the density of the polymer and oxygen Isolation ability to achieve uniform luminescence and stretchability of the material.

Benefits of technology

The prepared organic long afterglow film has good tensile properties, can be coated on a large area and emit uniformly, and the afterglow time reaches about 5 seconds, which is suitable for flexible display and anti-counterfeiting applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930921A_ABST
    Figure CN118930921A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an organic long-afterglow elastic film, in the preparation method, a fused ring compound and styrene-ethylene-butylene-styrene are used as solutes to be added into a solvent to form a mixed solution, then the mixed solution is dispensed to form a film, the film is naturally cooled, and after the solvent is naturally evaporated, the organic long-afterglow elastic film is obtained. The organic long-afterglow elastic film is obtained; the organic long-afterglow elastic film prepared by the method disclosed by the invention can be applied to electronic equipment as a flexible afterglow material and can also be used as an anti-counterfeiting marker. The organic long-afterglow thin film obtained by the preparation method disclosed by the invention has large-area coating performance, has a good stretching function and is uniform in luminescence, and the improvement of the flexibility is very beneficial to the application of an organic LPL (Liquefied Petroleum Liquefied) material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic long afterglow material preparation method, in particular to a preparation method and application of an organic long afterglow elastic film. Background Art

[0002] Organic long-persistent luminescence (OLPL) materials have the advantages of being easy to synthesize, functionally modified and processed, and being able to control persistent room-temperature phosphorescence (PRTP) through reasonable molecular design. They show potential application prospects in bioimaging, photodynamic therapy, information storage anti-counterfeiting, sensing, electroluminescent devices and security protection. However, since the intersystem crossing between singlet and triplet states of organic compounds is transition-forbidden and sensitive to temperature and air, it is difficult to achieve long-life and high-efficiency organic long-persistent luminescence. Researchers have improved the organic afterglow time, luminescence brightness and afterglow color by constructing a rigid environment, crystallization, host-guest doping, H-aggregates and other methods. However, the afterglow materials prepared by these methods are generally fragile, difficult to coat on a large area and emit light uniformly, and are not flexible and difficult to stretch, which seriously limits the commercial application of such materials in flexible displays, wearable and portable electronic devices and anti-counterfeiting applications. Therefore, developing materials with high-efficiency luminescence and excellent stretchability for application in flexible display technology, wearable devices and high-end anti-counterfeiting fields is a difficult problem that needs to be solved urgently.

[0003] Many researchers have solved this problem by adding high molecular polymers to prepare flexible films. Among them, the blending method is widely favored because of its simplicity and the lack of complex synthesis. The initial blending method for preparing such materials is to blend phosphors with polymers (such as PDMS, PVA), but hydrogen bonds will be formed after blending, which makes the structure of the phosphors and the polymers limited by the interaction requirements, and it is difficult to form a good effect; then researchers found that poly (methyl methacrylate) (PMMA) and polyvinyl pyrrolidone (PVP) showed good blending effects, but they showed limited stretchability. Another commonly used method is to dope phosphors in thermoplastic polymers, and the stretchability of polymers is easily affected by high temperatures. In addition, these methods usually rely on the inherent phosphorescence properties of phosphors. Therefore, there is still little research on polymers that can induce the RTP phenomenon of phosphors through simple processes while maintaining their superior stretchability. Therefore, it is of utmost importance to develop an afterglow material with uniform luminescence, good flexibility and stretchability. Summary of the invention

[0004] The present invention provides a preparation method and application of an organic long afterglow elastic film, so as to solve the problem that it is difficult to balance the luminescence performance and the stretching performance of the OLPL film prepared by the prior art OLPL material preparation method.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] The method for preparing an organic long afterglow elastic film comprises the following steps: adding a condensed ring compound and styrene-ethylene-butylene-styrene as solutes into a solvent, and stirring the mixture at a temperature of 60°C to 80°C to allow the solutes to be completely dispersed and dissolved in the solvent, thereby forming a mixed solution; then, drop-coating the mixed solution onto a substrate to form a film, and after the film is naturally cooled at room temperature, the solvent is naturally evaporated at room temperature, thereby obtaining an organic long afterglow elastic film.

[0007] Furthermore, in the solute, the mass ratio of the condensed ring compound to styrene-ethylene-butylene-styrene is 1:200.

[0008] Furthermore, the solvent is toluene.

[0009] Furthermore, the total mass of the solute added per 1 ml of toluene is 201 mg to 402 mg.

[0010] Furthermore, the condensed ring compound is triphenylene or tetracene.

[0011] The organic long afterglow elastic film prepared by the method for preparing the organic long afterglow elastic film is used as a flexible afterglow material in electronic devices.

[0012] The invention discloses an application of the organic long afterglow elastic film prepared by the method for preparing the organic long afterglow elastic film as an anti-counterfeiting mark.

[0013] The purpose of the present invention is to provide a method for preparing an organic long afterglow elastic film that can be coated over a large area and has stretchable properties. The preparation method is simple, the materials are cheap and readily available, the conditions are mild and do not require harsh conditions such as high temperature and high pressure.

[0014] In the present invention, from the perspective of improving the large-area coating and stretching of organic long afterglow film materials, condensed ring compounds are doped into the flexible polymer styrene ethylene butylene styrene (SEBS). The condensed ring compounds are used as luminophores because of their simple structure and easy availability. The compactness of the flexible polymer styrene ethylene butylene styrene is used to construct a rigid environment to suppress non-radiative transitions. More importantly, the flexible polymer has the ability to isolate oxygen, which greatly improves the room temperature phosphorescence of organic molecules and obtains an afterglow time of up to 5 seconds. At the same time, the elasticity of the flexible polymer is used to achieve large-area coating and stretchability of the organic long afterglow film, and the organic long afterglow film is made to emit light uniformly.

[0015] Therefore, compared with the prior art, the method for preparing an organic long afterglow film of the present invention has the performance of being able to be coated on a large area and has good stretching function, can be repeatedly stretched for many times, and has good afterglow luminescence performance, and can form a uniform, transparent, flexible and stretchable large-area film, and its stretching performance is the best among polymer long afterglow materials. The stretching performance of the long afterglow materials prepared by the polymer method in the prior art is still relatively poor, while the organic long afterglow film of the present invention that can be coated on a large area and has a stretching function has good stretching performance and uniform luminescence, and the improvement of flexibility will be very beneficial to the application of organic LPL materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the tensile stress-strain curve of BP@SEBS obtained in Example 1.

[0017] Figure 2 This is an optical photograph of the afterglow of BP@SEBS obtained in Example 1 before and after illumination.

[0018] Figure 3 This is the afterglow time decay curve of BP@SEBS obtained in Example 1.

[0019] Figure 4 This is the tensile stress-strain curve of NP@SEBS obtained in Example 2.

[0020] Figure 5 This is an optical photograph of the afterglow of NP@SEBS obtained in Example 2 before and after illumination.

[0021] Figure 6 This is the afterglow time decay curve of NP@SEBS obtained in Example 2. DETAILED DESCRIPTION

[0022] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0023] Embodiment 1:

[0024] A method for preparing an organic long afterglow elastic film BP@SEBS, the process is as follows:

[0025] The condensed ring compound phenylene (BP) and the flexible polymer styreneethylene butylene styrene (SEBS) are used as solutes and toluene is used as solvent. Due to the good solubility of SEBS and BP in toluene, they can be well mixed.

[0026] Among them, the manufacturer of triphenylene is Beijing Inokai Technology Co., Ltd. (purity: 97%), and the structural formula of triphenylene is:

[0027]

[0028] The structural formula of styrene-ethylene-butylene-styrene is:

[0029]

[0030] In the solute, the mass ratio of triphenylene to styrene-ethylene-butylene-styrene is 1:200, and the total mass of the solute added per 1 ml of toluene is 201 mg to 402 mg.

[0031] In this embodiment, 2 mg of triphenylene, 400 mg of styrene-ethylene-butylene-styrene, and 1 ml of toluene are taken. 2 mg of triphenylene and 400 mg of styrene-ethylene-butylene-styrene are added to 1 ml of toluene, and stirred at a temperature of 60°C to 80°C to make the triphenylene and styrene-ethylene-butylene-styrene completely and evenly dispersed and dissolved in toluene, thereby forming a mixed solution.

[0032] Then, a glass substrate is used as a substrate, and the mixed solution is drop-coated on the glass substrate to form a thin film. After the thin film is naturally cooled at room temperature of 20-25°C, the thin film on the glass substrate is transferred to a mold, and the solvent is naturally evaporated in the mold at room temperature of 20-25°C. The residue obtained is the organic long afterglow elastic film BP@SEBS, in which BP is uniformly dispersed in SEBS, and the obtained organic long afterglow elastic film BP@SEBS is stretchable and emits light uniformly.

[0033] The following describes the performance of the organic long afterglow elastic film BP@SEBS prepared in this embodiment in combination with the images obtained in the experiment. During the experiment, the optical performance measurement instrument used was an Ocean Optics multi-band spectrometer, and the mechanical performance measurement instrument used was an electronic universal tensile testing machine MTS CMT4000.

[0034] Figure 1 The tensile stress-strain curve of the organic long afterglow elastic film BP@SEBS with stretchable properties obtained in Example 1 is shown in FIG. Figure 1 It can be seen that at a constant strain rate of 2 mm·s -1 Under the conditions of , the long afterglow material with RTP performance showed excellent stretchability and was able to be stretched to about 420% of its original length. The tensile properties of the blended material were very similar to those of pure SEBS (about 445% of its original length), indicating that even trace amounts of phosphors do not affect the tensile properties of SEBS.

[0035] Figure 2 This is a macroscopic LPL picture of the organic long afterglow elastic film BP@SEBS with stretchable properties obtained in Example 1 at room temperature. It can be seen that the obtained organic long afterglow elastic film BP@SEBS emits light more evenly. Figure 2 It can be seen that when the film is excited by 365nm ultraviolet light, the fluorescence color emitted by the film is blue. After irradiation for 3 seconds, the excitation light source is turned off, and the organic long afterglow elastic film BP@SEBS can emit green afterglow light (such as Figure 2 a), in the first 3 seconds ( Figure 2 b represents the 1st s, Figure 2 c represents the 2nd s, Figure 2 d represents the 2nd second) the afterglow brightness of the compound is stronger, from the 4th second (such as Figure 2 e) and the afterglow gradually weakened, reaching the 5th second (as shown in Figure 2 f) has a weak afterglow, and the 6th second (as shown in Figure 2 The above results show that the afterglow time of the organic long afterglow elastic film BP@SEBS reaches about 5s, it has good afterglow performance, and the whole film emits light evenly.

[0036] The afterglow performance attenuation of the organic long afterglow elastic film BP@SEBS of Example 1 was tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 3 shown. Figure 3 In the figure, -2s to 0s is the organic long afterglow elastic film BP@SEBS of Example 1 under 365nm ultraviolet light, which shows photoluminescence characteristics; 0s to 10s is the organic long afterglow elastic film BP@SEBS of Example 1 after the ultraviolet light is removed, which shows green long afterglow light, and the afterglow time is about 5s, which is similar to the afterglow time observed by the naked eye.

[0037] The organic long afterglow elastic film BP@SEBS prepared in this embodiment can be used as a flexible afterglow material in flexible display electronic devices, wearable electronic devices, and portable electronic devices, and can also be used as an anti-counterfeiting mark.

[0038] Embodiment 2:

[0039] A method for preparing an organic long afterglow elastic film NP@SEBS, the process is as follows:

[0040] The fused ring compound naphthacene (NP) and the flexible polymer styreneethylene butylene styrene (SEBS) were used as solutes and toluene was used as solvent. Due to the good solubility of SEBS and NP in toluene, they can be well mixed.

[0041] Among them, the manufacturer of tetracene is Beijing Inokai Technology Co., Ltd. (purity: 97%), and the structural formula of tetracene is:

[0042]

[0043] The structural formula of styrene-ethylene-butylene-styrene is:

[0044]

[0045] In the solute, the mass ratio of tetracene to styrene-ethylene-butylene-styrene is 1:200, and the total mass of the solute added per 1 ml of toluene is 201 mg to 402 mg.

[0046] In this embodiment, 2 mg of tetracene, 400 mg of styrene-ethylene-butylene-styrene, and 1 ml of toluene are taken. 2 mg of tetracene and 400 mg of styrene-ethylene-butylene-styrene are added to 1 ml of toluene, and stirred at a temperature of 60°C to 80°C to make the tetracene and styrene-ethylene-butylene-styrene completely and evenly dispersed and dissolved in the toluene, thereby forming a mixed solution.

[0047] Then, a glass substrate is used as a substrate, and the mixed solution is drop-coated on the glass substrate to form a thin film. After the thin film is naturally cooled at room temperature of 20-25°C, the thin film on the glass substrate is transferred to a mold, and the solvent is naturally evaporated in the mold at room temperature of 20-25°C. The residue obtained is the organic long afterglow elastic film NP@SEBS, in which NP is uniformly dispersed in SEBS, and the obtained organic long afterglow elastic film NP@SEBS is stretchable and emits light uniformly.

[0048] The following is a description of the performance of the organic long afterglow elastic film NP@SEBS prepared in this embodiment in combination with the images obtained in the experiment. The apparatus used in the experiment is the same as that in embodiment 1.

[0049] Figure 4The tensile stress-strain curve of the organic long afterglow elastic film NP@SEBS with stretchable properties obtained in Example 2 is shown in FIG. Figure 4 It can be seen that at a constant strain rate of 2 mm·s -1 Under the conditions of , the long afterglow material with RTP performance showed excellent stretchability and was able to be stretched to about 420% of its original length. The tensile properties of the blended material were very similar to those of pure SEBS (about 445% of its original length), indicating that even trace amounts of phosphors do not affect the tensile properties of SEBS.

[0050] Figure 5 This is a macroscopic LPL picture of the organic long afterglow elastic film NP@SEBS with stretchable properties obtained in Example 2 at room temperature. It can be seen that the obtained organic long afterglow elastic film NP@SEBS emits light more evenly. Figure 5 It can be seen that when the film is excited by 365nm ultraviolet light, the fluorescent color emitted by the film is light yellow. After irradiation for 3 seconds, the excitation light source is turned off and the polymer film can emit a light yellow afterglow (such as Figure 5 a), in the first 1s( Figure 5 b represents the first second) the afterglow brightness of the compound is stronger, from the second second (such as Figure 5 c) and then the afterglow gradually weakens, from the 3rd second (as shown in Figure 5 d) and then the afterglow gradually disappears, and from the 4th second (as shown in Figure 5 The above results show that the afterglow time of the organic long afterglow elastic film NP@SEBS is about 3s, which has good afterglow performance and the whole film emits light uniformly.

[0051] The afterglow performance attenuation of the organic long afterglow elastic film NP@SEBS of Example 2 was tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 6 shown. Figure 6 In the figure, -2s to 0s is the organic long afterglow elastic material of Example 2 under 365nm ultraviolet light irradiation, which exhibits photoluminescence characteristics; 0s to 10s is the organic long afterglow elastic film NP@SEBS of Example 2 after the ultraviolet light is removed, which exhibits green long afterglow light, and the afterglow time is about 3s, which is similar to the afterglow time observed by the naked eye.

[0052] The organic long afterglow elastic film NP@SEBS prepared in this embodiment can be used as a flexible afterglow material in flexible display electronic devices, wearable electronic devices, and portable electronic devices, and can also be used as an anti-counterfeiting mark.

[0053] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. The embodiments described in the present invention are merely descriptions of the preferred embodiments of the present invention, and do not limit the concept and scope of the present invention. The various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction, and such combinations should also be regarded as the contents disclosed in the present disclosure as long as they do not violate the concept of the present invention. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0054] The present invention is not limited to the specific details of the above-mentioned embodiments. Within the technical concept of the present invention and without departing from the design concept of the present invention, various modifications and improvements made to the technical solution of the present invention by technical personnel in this field should fall within the protection scope of the present invention. The technical contents for which protection is sought in the present invention have been fully recorded in the claims.

Claims

1. A method for preparing an organic long afterglow elastic film, characterized in that: A condensed ring compound and styrene-ethylene-butylene-styrene are added as solutes to a solvent, and stirred at a temperature of 60°C to 80°C to allow the solute to be completely dispersed and dissolved in the solvent, thereby forming a mixed solution; then, the mixed solution is drop-coated on a substrate to form a thin film, and after the film is naturally cooled at room temperature, the solvent is naturally evaporated at room temperature, thereby obtaining an organic long afterglow elastic film.

2. The method for preparing an organic long afterglow elastic film according to claim 1 is characterized in that: In the solute, the mass ratio of the condensed ring compound to styrene-ethylene-butylene-styrene is 1:

200.

3. The method for preparing an organic long afterglow elastic film according to claim 2, characterized in that: The solvent is toluene.

4. The method for preparing an organic long afterglow elastic film according to claim 3, characterized in that: The total mass of solute added per 1 ml of toluene is 201 mg~402 mg.

5. The method for preparing an organic long afterglow elastic film according to any one of claims 1 to 4, characterized in that: The condensed ring compound is triphenylene or tetracene.

6. Use of the organic long afterglow elastic film prepared by the method for preparing the organic long afterglow elastic film as claimed in any one of claims 1 to 5 as a flexible afterglow material in electronic devices.

7. Use of an organic long afterglow elastic film prepared by the method for preparing an organic long afterglow elastic film as claimed in any one of claims 1 to 5 as an anti-counterfeiting mark.