High-performance plastic additive and preparation method thereof

By combining modified limestone, modified activated carbon, additives, and modified graphite powder, the problem of insufficient tensile yield strength and flexural modulus of existing high-performance plastic additives has been solved, and the performance of plastic additives has been significantly improved.

CN118930981APending Publication Date: 2024-11-12然石功能材料(江苏)有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411237215.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing high-performance plastic additives have weak tensile yield strength and low flexural modulus, which affects their performance.

Method used

High-performance plastic additives are prepared by combining modified limestone, modified activated carbon, additives, pentaerythritol and modified graphite powder, through microwave reaction, heat treatment and stirring and grinding, to enhance material compatibility and performance.

Benefits of technology

It significantly improves the tensile yield strength and flexural modulus of plastic additives, thereby enhancing the overall performance of plastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930981A_ABST
    Figure CN118930981A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of plastics, particularly relates to a high-performance plastic additive and a preparation method thereof, and provides the following scheme aiming at the problems of relatively weak tensile yield strength and relatively small bending modulus in the prior art. The high-performance plastic additive is composed of the following components in parts by weight: 35-45 parts of modified limestone, 15-25 parts of modified activated carbon, 15-20 parts of an additive, 10-15 parts of pentaerythritol and 5-15 parts of modified graphite powder, and the raw materials of the modified limestone comprise limestone, 10-30% hydrochloric acid and sulfamic acid. The additives comprise a catalyst, an antioxidant, a stiffening agent, a toughening agent, a nucleating agent, a dispersing agent and a slipping agent, the high-performance plastic additive is prepared from the modified limestone, the modified activated carbon, the additives, pentaerythritol and the modified graphite powder, and after the high-performance plastic additive is added into plastic to produce a product, the tensile yield strength is greatly improved, and the bending modulus of the product is greatly enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, and in particular to a high-performance plastic additive and a preparation method thereof. Background Art

[0002] The Chinese patent document with application number 201810144942.5 discloses a high-performance plastic additive and a preparation method thereof. The high-performance plastic additive of the present invention contains magnesium oxide nanopowder, niobium oxide nanopowder, tungsten selenide layered nanomaterials, tantalum sulfide layered nanomaterials, cobalt sulfide layered nanomaterials, graphene, calcium fluoride nanopowder, aluminum dihydrogen phosphate, 8-hydroxyquinoline aluminum, calcium chloride powder, and fumed silica. By utilizing the physical properties of the above materials and under the synergistic effect of each component, the compatibility of the plastic additive in the plastic is increased, the polymer material is plasticized, and the impact resistance, rigidity and heat resistance of the plastic are improved. The preparation method of the plastic additive of the present invention is simple and easy to produce and prepare.

[0003] However, the high-performance plastic additive and its preparation method also have some problems. For example, the performance of the plastic additive is poor, and the tensile yield strength of the product produced after adding plastic is weak and the bending modulus is small, which affects the performance of the plastic additive. Summary of the invention

[0004] Based on the fact that the background technology has the problems of weak tensile yield strength and small bending modulus, the present invention proposes a high-performance plastic additive and a preparation method thereof.

[0005] The invention provides a high-performance plastic additive, which consists of the following components in parts by weight: 35 to 45 parts of modified limestone, 15 to 25 parts of modified activated carbon, 15 to 20 parts of additives, 10 to 15 parts of pentaerythritol and 5 to 15 parts of modified graphite powder. The raw materials of the modified limestone include limestone, 10-30% hydrochloric acid and aminosulfonic acid, and the raw materials of the additive include catalysts, antioxidants, stiffening agents, toughening agents, nucleating agents, dispersants and lubricants. The high-performance plastic additive is prepared by using the modified limestone, modified activated carbon, additives, pentaerythritol and modified graphite powder. After being added into plastic to produce products, the tensile yield strength is greatly improved and the flexural modulus of the product is greatly enhanced.

[0006] Preferably, the weight ratio of limestone, 10-30% hydrochloric acid and aminosulfonic acid in the modified limestone is 4:1:1, and the limestone is selected to be granular powdery limestone, which can enhance the compatibility with other materials.

[0007] Preferably, the modification method of the modified limestone is as follows: limestone, 10-30% hydrochloric acid and aminosulfonic acid are poured into a container and stirred to obtain a mixture, the mixture is poured into a reaction container of a microwave reactor, the microwave reactor is started to perform microwave reaction on the mixture of limestone, 10-30% hydrochloric acid and aminosulfonic acid, the radiation time is controlled to be 5 minutes to 30 minutes, and the power is 50w to 200w to obtain modified limestone, thereby ensuring the modification effect of limestone and facilitating the mixing of modified limestone with other materials.

[0008] Preferably, the raw materials of the modified activated carbon include activated carbon, polyimine and polydimethylsiloxane, and the weight ratio of activated carbon, polyimine and polydimethylsiloxane in the modified activated carbon is controlled to be 20:1:2, which is convenient for modifying the activated carbon inside the modified activated carbon and for exerting the effect of the auxiliary agent.

[0009] Preferably, the preparation method of the modified activated carbon is as follows: the activated carbon to be modified is obtained, mixed with polyimine, poured into an oven for heating, the heating temperature is controlled at 250°C to 300°C, the heating time is controlled at 3 hours, after cooling, polydimethylsiloxane is added for mixing, and after mixing evenly, the material is put into an oven, sealed and heated again, the heating temperature is controlled at 150°C to 200°C, cooled naturally after 1 hour, and the raw material is taken out of the oven to obtain modified activated carbon, which can enhance the performance of the modified activated carbon.

[0010] Preferably, the additives include catalyst, antioxidant, stiffener, toughener, nucleating agent, dispersant and lubricant. The catalyst is tetrabutyl titanate, the nucleating agent is sorbitol nucleating agent, and the dispersant is carboxymethyl cellulose dispersant. The effects of various additives can be effectively exerted to achieve antioxidant and toughening effects on plastics, thereby facilitating the production and preparation of plastics.

[0011] Preferably, the preparation method of the modified graphite powder is as follows: natural spherical graphite is poured into a citric acid aqueous solution for mixing, the citric acid aqueous solution needs to completely submerge the natural spherical graphite, and then a wet grinder is used for stirring and grinding until the material passes through a 200-mesh sieve, followed by spray drying, and the dried material is carbonized again using a carbonization device, and finally ground and sieved to obtain modified graphite powder, thereby enhancing the performance of the modified graphite powder and allowing the modified graphite powder to be better compatible with other materials.

[0012] A method for preparing a high-performance plastic additive comprises the following steps: S1: Add modified limestone and modified activated carbon into a stirring device, stir them evenly, grind them repeatedly using a grinding device, sieve and filter them using a 100-mesh sieve, and grind them repeatedly until all the materials pass the sieve to obtain a primary mixed material; S2: adding pentaerythritol and modified graphite powder to the primary mixture, and continuing to stir to uniformly mix the pentaerythritol, modified graphite powder and the primary mixture to obtain a semi-mixture; S3: Add additives to the semi-mixed material, heat and mix again, and finally obtain a high-performance plastic additive.

[0013] Preferably, in S2, during mixing, the stirring speed is controlled at 120 rpm to 240 rpm, and the stirring process is performed for 15 minutes to 30 minutes, which can enhance the uniformity of the material and facilitate subsequent processing.

[0014] Preferably, in S3, during mixing, the stirring speed is controlled at 720 rpm to 880 rpm, and the stirring process is performed for 15 minutes to 30 minutes to enhance the uniformity of the high-performance plastic additive.

[0015] Beneficial effects of the present invention: High-performance plastic additives are prepared using modified limestone, modified activated carbon, additives, pentaerythritol and modified graphite powder. After being added to plastics to produce products, the tensile yield strength is greatly improved and the flexural modulus of the product is greatly enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The working flow chart proposed by the present invention. DETAILED DESCRIPTION

[0017] The present invention will be further explained below in conjunction with specific embodiments.

[0018] Reference Figure 1 , Embodiment 1 In this embodiment, a high-performance plastic additive is proposed. The high-performance plastic additive is composed of the following components in parts by weight: 38 parts of modified limestone, 22 parts of modified activated carbon, 16 parts of additives, 13 parts of pentaerythritol and 11 parts of modified graphite powder. The raw materials of the modified limestone include limestone, 10-30% hydrochloric acid and aminosulfonic acid. The raw materials of the additive include catalysts, antioxidants, stiffeners, tougheners, nucleating agents, dispersants and lubricants. The weight ratio of limestone, 10-30% hydrochloric acid and aminosulfonic acid in the modified limestone is 4:1:1. The limestone is selected in the form of granular powder to increase compatibility with other materials. The modification method of the modified limestone is as follows: limestone is added to the mixture. limestone, 10-30% hydrochloric acid and aminosulfonic acid are poured into a container for stirring and uniformly mixing to obtain a mixture, and the mixture is poured into a reaction container of a microwave reactor, and the microwave reactor is started to perform microwave reaction on the mixture of limestone, 10-30% hydrochloric acid and aminosulfonic acid, and the radiation time is controlled to be 5 minutes to 30 minutes and the power is 50w to 200w to obtain modified limestone, thereby ensuring the modification effect of the limestone and facilitating the mixing of the modified limestone with other materials. The raw materials of the modified activated carbon include activated carbon, polyimide and polydimethylsiloxane, and the weight proportion of the activated carbon, polyimide and polydimethylsiloxane in the modified activated carbon is controlled to be 20:1:2, so as to facilitate the modification of the modified activated carbon. The modified activated carbon is modified to facilitate the effect of the auxiliary agent. The preparation method of the modified activated carbon is as follows: the activated carbon to be modified is obtained, mixed with polyimide, poured into an oven for heating, the heating temperature is controlled at 250°C ~ 300°C, the heating time is controlled at 3 hours, after cooling, polydimethylsiloxane is added for mixing, and after mixing evenly, the material is put into the oven, sealed and heated again, the heating temperature is controlled at 150°C ~ 200°C, cooled naturally after 1 hour, and the raw material is taken out of the oven to obtain modified activated carbon, which can enhance the performance of the modified activated carbon. The additives include catalysts, antioxidants, stiffeners, toughening agents, nucleating agents, dispersants and lubricants, and the catalyst is tetrabutyl titanate , select sorbitol nucleating agent, select carboxymethyl cellulose dispersant as dispersant, which can effectively play the role of various additives, play an antioxidant, toughening and other effects on plastics, and facilitate the production and preparation of plastics. The preparation method of modified graphite powder is as follows: pour natural spherical graphite into citric acid aqueous solution for mixing. The citric acid aqueous solution needs to completely submerge the natural spherical graphite, and then use a wet grinder to stir and grind until the material passes the screening of a 200-mesh sieve, followed by spray drying. The dried material is carbonized again using a carbonization equipment, and finally ground and sieved to obtain modified graphite powder, enhance the performance of the modified graphite powder, and make the modified graphite powder better compatible with other materials.

[0019] A method for preparing a high-performance plastic additive comprises the following steps: S1: Add modified limestone and modified activated carbon into a stirring device, stir them evenly, grind them repeatedly using a grinding device, sieve and filter them using a 100-mesh sieve, and grind them repeatedly until all the materials pass the sieve to obtain a primary mixed material; S2: adding pentaerythritol and modified graphite powder to the primary mixture, continuing to stir, and uniformly mixing the pentaerythritol, modified graphite powder and the primary mixture. During mixing, the stirring speed is controlled at 220 rpm, and the stirring is performed for 21 minutes to obtain a semi-mixed material; S3: Add the additives to the semi-mixed material, heat and mix again. During mixing, the stirring speed is controlled at 780 rpm. The stirring process is performed for 18 minutes to finally obtain a high-performance plastic additive.

[0020] Reference Figure 1 , Embodiment 2 In this embodiment, a high-performance plastic additive is proposed. The high-performance plastic additive is composed of the following components in parts by weight: 40 parts of modified limestone, 18 parts of modified activated carbon, 17 parts of additives, 13 parts of pentaerythritol and 12 parts of modified graphite powder. The raw materials of the modified limestone include limestone, 10-30% hydrochloric acid and aminosulfonic acid. The raw materials of the additive include catalysts, antioxidants, stiffeners, tougheners, nucleating agents, dispersants and lubricants. The weight ratio of limestone, 10-30% hydrochloric acid and aminosulfonic acid in the modified limestone is 4:1:1. The limestone is selected in the form of granular powder to increase compatibility with other materials. The modification method of the modified limestone is as follows: limestone is added to the mixture. limestone, 10-30% hydrochloric acid and aminosulfonic acid are poured into a container for stirring and uniformly mixing to obtain a mixture, and the mixture is poured into a reaction container of a microwave reactor, and the microwave reactor is started to perform microwave reaction on the mixture of limestone, 10-30% hydrochloric acid and aminosulfonic acid, and the radiation time is controlled to be 5 minutes to 30 minutes and the power is 50w to 200w to obtain modified limestone, thereby ensuring the modification effect of the limestone and facilitating the mixing of the modified limestone with other materials. The raw materials of the modified activated carbon include activated carbon, polyimide and polydimethylsiloxane, and the weight proportion of the activated carbon, polyimide and polydimethylsiloxane in the modified activated carbon is controlled to be 20:1:2, so as to facilitate the modification of the modified activated carbon. The modified activated carbon is modified to facilitate the effect of the auxiliary agent. The preparation method of the modified activated carbon is as follows: the activated carbon to be modified is obtained, mixed with polyimide, poured into an oven for heating, the heating temperature is controlled at 250°C ~ 300°C, the heating time is controlled at 3 hours, after cooling, polydimethylsiloxane is added for mixing, and after mixing evenly, the material is put into the oven, sealed and heated again, the heating temperature is controlled at 150°C ~ 200°C, cooled naturally after 1 hour, and the raw material is taken out of the oven to obtain modified activated carbon, which can enhance the performance of the modified activated carbon. The additives include catalysts, antioxidants, stiffeners, toughening agents, nucleating agents, dispersants and lubricants, and the catalyst is tetrabutyl titanate , select sorbitol nucleating agent, select carboxymethyl cellulose dispersant as dispersant, which can effectively play the role of various additives, play an antioxidant, toughening and other effects on plastics, and facilitate the production and preparation of plastics. The preparation method of modified graphite powder is as follows: pour natural spherical graphite into citric acid aqueous solution for mixing. The citric acid aqueous solution needs to completely submerge the natural spherical graphite, and then use a wet grinder to stir and grind until the material passes the screening of a 200-mesh sieve, followed by spray drying. The dried material is carbonized again using a carbonization equipment, and finally ground and sieved to obtain modified graphite powder, enhance the performance of the modified graphite powder, and make the modified graphite powder better compatible with other materials.

[0021] A method for preparing a high-performance plastic additive comprises the following steps: S1: Add modified limestone and modified activated carbon into a stirring device, stir them evenly, grind them repeatedly using a grinding device, sieve and filter them using a 100-mesh sieve, and grind them repeatedly until all the materials pass the sieve to obtain a primary mixed material; S2: adding pentaerythritol and modified graphite powder to the primary mixture, continuing to stir, and uniformly mixing the pentaerythritol, modified graphite powder and the primary mixture. During mixing, the stirring speed is controlled at 220 rpm, and the stirring is performed for 21 minutes to obtain a semi-mixed material; S3: Add the additives to the semi-mixed material, heat and mix again. During mixing, the stirring speed is controlled at 780 rpm. The stirring process is performed for 18 minutes to finally obtain a high-performance plastic additive.

[0022] Reference Figure 1 , Embodiment 3 In this embodiment, a high-performance plastic additive is proposed. The high-performance plastic additive is composed of the following components in parts by weight: 39 parts of modified limestone, 21 parts of modified activated carbon, 17 parts of additives, 12 parts of pentaerythritol and 11 parts of modified graphite powder. The raw materials of the modified limestone include limestone, 10-30% hydrochloric acid and aminosulfonic acid. The raw materials of the additive include catalysts, antioxidants, stiffeners, tougheners, nucleating agents, dispersants and lubricants. The weight ratio of limestone, 10-30% hydrochloric acid and aminosulfonic acid in the modified limestone is 4:1:1. The limestone is selected in the form of granular powder to increase compatibility with other materials. The modification method of the modified limestone is as follows: limestone is added to the mixture. limestone, 10-30% hydrochloric acid and aminosulfonic acid are poured into a container for stirring and uniformly mixing to obtain a mixture, and the mixture is poured into a reaction container of a microwave reactor, and the microwave reactor is started to perform microwave reaction on the mixture of limestone, 10-30% hydrochloric acid and aminosulfonic acid, and the radiation time is controlled to be 5 minutes to 30 minutes and the power is 50w to 200w to obtain modified limestone, thereby ensuring the modification effect of the limestone and facilitating the mixing of the modified limestone with other materials. The raw materials of the modified activated carbon include activated carbon, polyimide and polydimethylsiloxane, and the weight proportion of the activated carbon, polyimide and polydimethylsiloxane in the modified activated carbon is controlled to be 20:1:2, so as to facilitate the modification of the modified activated carbon. The modified activated carbon is modified to facilitate the effect of the auxiliary agent. The preparation method of the modified activated carbon is as follows: the activated carbon to be modified is obtained, mixed with polyimide, poured into an oven for heating, the heating temperature is controlled at 250°C ~ 300°C, the heating time is controlled at 3 hours, after cooling, polydimethylsiloxane is added for mixing, and after mixing evenly, the material is put into the oven, sealed and heated again, the heating temperature is controlled at 150°C ~ 200°C, cooled naturally after 1 hour, and the raw material is taken out of the oven to obtain modified activated carbon, which can enhance the performance of the modified activated carbon. The additives include catalysts, antioxidants, stiffeners, toughening agents, nucleating agents, dispersants and lubricants, and the catalyst is tetrabutyl titanate , select sorbitol nucleating agent, select carboxymethyl cellulose dispersant as dispersant, which can effectively play the role of various additives, play an antioxidant, toughening and other effects on plastics, and facilitate the production and preparation of plastics. The preparation method of modified graphite powder is as follows: pour natural spherical graphite into citric acid aqueous solution for mixing. The citric acid aqueous solution needs to completely submerge the natural spherical graphite, and then use a wet grinder to stir and grind until the material passes the screening of a 200-mesh sieve, followed by spray drying. The dried material is carbonized again using a carbonization equipment, and finally ground and sieved to obtain modified graphite powder, enhance the performance of the modified graphite powder, and make the modified graphite powder better compatible with other materials.

[0023] A method for preparing a high-performance plastic additive comprises the following steps: S1: Add modified limestone and modified activated carbon into a stirring device, stir them evenly, grind them repeatedly using a grinding device, sieve and filter them using a 100-mesh sieve, and grind them repeatedly until all the materials pass the sieve to obtain a primary mixed material; S2: adding pentaerythritol and modified graphite powder to the primary mixture, continuing to stir, and uniformly mixing the pentaerythritol, modified graphite powder and the primary mixture. During mixing, the stirring speed is controlled at 220 rpm, and the stirring is performed for 21 minutes to obtain a semi-mixed material; S3: Add the additives to the semi-mixed material, heat and mix again. During mixing, the stirring speed is controlled at 780 rpm. The stirring process is performed for 18 minutes to finally obtain a high-performance plastic additive.

[0024] Reference Figure 1 , Embodiment 4 In this embodiment, a high-performance plastic additive is proposed. The high-performance plastic additive is composed of the following components in parts by weight: 36 parts of modified limestone, 24 parts of modified activated carbon, 18 parts of additives, 12 parts of pentaerythritol and 10 parts of modified graphite powder. The raw materials of the modified limestone include limestone, 10-30% hydrochloric acid and aminosulfonic acid. The raw materials of the additive include catalysts, antioxidants, stiffeners, tougheners, nucleating agents, dispersants and lubricants. The weight ratio of limestone, 10-30% hydrochloric acid and aminosulfonic acid in the modified limestone is 4:1:1. The limestone is selected in the form of granular powder to increase compatibility with other materials. The modification method of the modified limestone is as follows: limestone is added to the mixture. limestone, 10-30% hydrochloric acid and aminosulfonic acid are poured into a container for stirring and uniformly mixing to obtain a mixture, and the mixture is poured into a reaction container of a microwave reactor, and the microwave reactor is started to perform microwave reaction on the mixture of limestone, 10-30% hydrochloric acid and aminosulfonic acid, and the radiation time is controlled to be 5 minutes to 30 minutes and the power is 50w to 200w to obtain modified limestone, thereby ensuring the modification effect of the limestone and facilitating the mixing of the modified limestone with other materials. The raw materials of the modified activated carbon include activated carbon, polyimide and polydimethylsiloxane, and the weight proportion of the activated carbon, polyimide and polydimethylsiloxane in the modified activated carbon is controlled to be 20:1:2, so as to facilitate the modification of the modified activated carbon. The modified activated carbon is modified to facilitate the effect of the auxiliary agent. The preparation method of the modified activated carbon is as follows: the activated carbon to be modified is obtained, mixed with polyimide, poured into an oven for heating, the heating temperature is controlled at 250°C ~ 300°C, the heating time is controlled at 3 hours, after cooling, polydimethylsiloxane is added for mixing, and after mixing evenly, the material is put into the oven, sealed and heated again, the heating temperature is controlled at 150°C ~ 200°C, cooled naturally after 1 hour, and the raw material is taken out of the oven to obtain modified activated carbon, which can enhance the performance of the modified activated carbon. The additives include catalysts, antioxidants, stiffeners, toughening agents, nucleating agents, dispersants and lubricants, and the catalyst is tetrabutyl titanate , select sorbitol nucleating agent, select carboxymethyl cellulose dispersant as dispersant, which can effectively play the role of various additives, play an antioxidant, toughening and other effects on plastics, and facilitate the production and preparation of plastics. The preparation method of modified graphite powder is as follows: pour natural spherical graphite into citric acid aqueous solution for mixing. The citric acid aqueous solution needs to completely submerge the natural spherical graphite, and then use a wet grinder to stir and grind until the material passes the screening of a 200-mesh sieve, followed by spray drying. The dried material is carbonized again using a carbonization equipment, and finally ground and sieved to obtain modified graphite powder, enhance the performance of the modified graphite powder, and make the modified graphite powder better compatible with other materials.

[0025] A method for preparing a high-performance plastic additive comprises the following steps: S1: Add modified limestone and modified activated carbon into a stirring device, stir them evenly, grind them repeatedly using a grinding device, sieve and filter them using a 100-mesh sieve, and grind them repeatedly until all the materials pass the sieve to obtain a primary mixed material; S2: adding pentaerythritol and modified graphite powder to the primary mixture, continuing to stir, and uniformly mixing the pentaerythritol, modified graphite powder and the primary mixture. During mixing, the stirring speed is controlled at 220 rpm, and the stirring is performed for 21 minutes to obtain a semi-mixed material; S3: Add the additives to the semi-mixed material, heat and mix again. During mixing, the stirring speed is controlled at 780 rpm. The stirring process is performed for 18 minutes to finally obtain a high-performance plastic additive.

[0026] Reference Figure 1 Embodiment 5 In this embodiment, a high-performance plastic additive is proposed. The high-performance plastic additive is composed of the following components in parts by weight: 40 parts of modified limestone, 25 parts of modified activated carbon, 15 parts of additives, 13 parts of pentaerythritol and 7 parts of modified graphite powder. The raw materials of the modified limestone include limestone, 10-30% hydrochloric acid and aminosulfonic acid. The raw materials of the additive include catalysts, antioxidants, stiffeners, tougheners, nucleating agents, dispersants and lubricants. The weight ratio of limestone, 10-30% hydrochloric acid and aminosulfonic acid in the modified limestone is 4:1:1. The limestone is selected in the form of granular powder to increase compatibility with other materials. The modification method of the modified limestone is as follows: the limestone is , 10-30% hydrochloric acid and aminosulfonic acid are poured into a container for stirring and uniformly mixing to obtain a mixture, and the mixture is poured into the reaction container of a microwave reactor, and the microwave reactor is started to perform microwave reaction on the mixture of limestone, 10-30% hydrochloric acid and aminosulfonic acid, and the radiation time is controlled to be 5 minutes to 30 minutes and the power is 50w to 200w to obtain modified limestone, thereby ensuring the modification effect of limestone and facilitating the mixing of modified limestone with other materials. The raw materials of modified activated carbon include activated carbon, polyimide and polydimethylsiloxane, and the weight proportion of activated carbon, polyimide and polydimethylsiloxane in the modified activated carbon is controlled to be 20:1:2, so as to facilitate the modification of the internal structure of the modified activated carbon. The modified activated carbon is modified to facilitate the effect of the auxiliary agent. The preparation method of the modified activated carbon is as follows: the activated carbon to be modified is obtained, mixed with polyimide, poured into an oven for heating, the heating temperature is controlled at 250°C to 300°C, the heating time is controlled at 3 hours, and after cooling, polydimethylsiloxane is added for mixing. After mixing evenly, the material is put into the oven, sealed and heated again, the heating temperature is controlled at 150°C to 200°C, cooled naturally after 1 hour, and the raw material is taken out of the oven to obtain modified activated carbon, which can enhance the performance of the modified activated carbon. The catalyst, antioxidant, stiffener, toughener, nucleating agent, dispersant and lubricant are selected as the catalyst, tetrabutyl titanate is selected as the catalyst, Select sorbitol nucleating agent as nucleating agent and carboxymethyl cellulose dispersing agent as dispersing agent, which can effectively exert the effects of various additives, have antioxidant and toughening effects on plastics, and facilitate the production and preparation of plastics. The preparation method of modified graphite powder is as follows: natural spherical graphite is poured into citric acid aqueous solution for mixing. The citric acid aqueous solution needs to completely submerge the natural spherical graphite, and then stirred and ground using a wet grinder until the material passes the screening of a 200-mesh sieve, followed by spray drying. The dried material is carbonized again using a carbonization equipment, and finally ground and sieved to obtain modified graphite powder, thereby enhancing the performance of the modified graphite powder and making the modified graphite powder more compatible with other materials.

[0027] A method for preparing a high-performance plastic additive comprises the following steps: S1: Add modified limestone and modified activated carbon into a stirring device, stir them evenly, grind them repeatedly using a grinding device, sieve and filter them using a 100-mesh sieve, and grind them repeatedly until all the materials pass the sieve to obtain a primary mixed material; S2: adding pentaerythritol and modified graphite powder to the primary mixture, continuing to stir, and uniformly mixing the pentaerythritol, modified graphite powder and the primary mixture. During mixing, the stirring speed is controlled at 220 rpm, and the stirring is performed for 21 minutes to obtain a semi-mixed material; S3: Add the additives to the semi-mixed material, heat and mix again. During mixing, the stirring speed is controlled at 780 rpm. The stirring process is performed for 18 minutes to finally obtain a high-performance plastic additive.

[0028] Comparing conventional plastic additives with the plastic additives prepared in Examples 1 to 5, the plastic additives prepared in Examples 1 to 5 are shown in the following table: Comparative Example Embodiment 1 Embodiment 2 Embodiment 3 Embodiment 4 Embodiment 5 Tensile yield strength (MPa) 39.7 43.8 43.9 43.7 43.3 43.1 Flexural modulus (MPa) 1493 1638 1642 1632 1612 1594 It can be seen from the above table that the tensile yield strength and flexural modulus of the plastic additive prepared by the present invention are significantly improved, and implementation 2 is the best implementation example.

[0029] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high performance plastic additive, characterized in that: The high performance plastic additive comprises the following components in parts by weight: Composition: 35 to 45 parts of modified limestone, 15 to 25 parts of modified activated carbon, 15 to 20 parts of additives, 10 to 15 parts of pentaerythritol and 5 to 15 parts of modified graphite powder. The raw materials of the modified limestone include limestone, 10-30% hydrochloric acid and aminosulfonic acid. The raw materials of the additive include catalyst, antioxidant, stiffener, toughener, nucleating agent, dispersant and lubricant.

2. A high performance plastic additive according to claim 1, characterized in that: The weight ratio of limestone, 10-30% hydrochloric acid and aminosulfonic acid in the modified limestone is 4:1:1, and the limestone is granular powdery limestone.

3. A high performance plastic additive according to claim 1, characterized in that: The modified limestone modification method comprises the following steps: pouring limestone, 10-30% hydrochloric acid and aminosulfonic acid into a container for stirring and uniformly mixing to obtain a mixture, pouring all the mixture into a reaction container of a microwave reactor, starting the microwave reactor to perform microwave reaction on the mixture of limestone, 10-30% hydrochloric acid and aminosulfonic acid, controlling the radiation time to be 5 minutes to 30 minutes and the power to be 50W to 200W, and obtaining the modified limestone.

4. A high performance plastic additive according to claim 1, characterized in that: The raw materials of the modified activated carbon include activated carbon, polyimine and polydimethylsiloxane, and the weight ratio of the activated carbon, polyimine and polydimethylsiloxane in the modified activated carbon is controlled to be 20:1:

2.

5. A high performance plastic additive according to claim 4, characterized in that: The preparation method of the modified activated carbon comprises the following steps: obtaining the activated carbon to be modified, mixing it with polyimine, pouring it into an oven for heating, controlling the heating temperature at 250°C to 300°C, and controlling the heating time at 3 hours; after cooling, adding polydimethylsiloxane for mixing; after mixing evenly, putting the material into an oven, sealing it, heating it again, controlling the heating temperature at 150°C to 200°C, cooling it naturally after 1 hour, taking the raw material out of the oven, and obtaining the modified activated carbon.

6. A high performance plastic additive according to claim 1, characterized in that: The additives include catalyst, antioxidant, stiffening agent, toughening agent, nucleating agent, dispersant and lubricant. The catalyst is tetrabutyl titanate, the nucleating agent is sorbitol nucleating agent, and the dispersing agent is carboxymethyl cellulose dispersant.

7. A high performance plastic additive according to claim 1, characterized in that: The preparation method of the modified graphite powder comprises the following steps: pouring natural spherical graphite into a citric acid aqueous solution for mixing, wherein the citric acid aqueous solution needs to completely submerge the natural spherical graphite, and then stirring and grinding the material using a wet grinder until the material passes through a 200-mesh sieve, and then spray drying the material, and carbonizing the dried material again using a carbonization device, and finally grinding and sieving the material to obtain the modified graphite powder.

8. A method for preparing a high-performance plastic additive as claimed in claim 1, characterized in that: The following steps are involved: S1: Add modified limestone and modified activated carbon into a stirring device, stir them evenly, grind them repeatedly using a grinding device, sieve and filter them using a 100-mesh sieve, and grind them repeatedly until all the materials pass the sieve to obtain a primary mixed material; S2: adding pentaerythritol and modified graphite powder to the primary mixture, and continuing to stir to uniformly mix the pentaerythritol, modified graphite powder and the primary mixture to obtain a semi-mixture; S3: Add additives to the semi-mixed material, heat and mix again, and finally obtain a high-performance plastic additive.

9. A high-performance plastic additive and a preparation method thereof according to claim 8, characterized in that: In S2, during mixing, the stirring speed is controlled at 120 rpm to 240 rpm, and the stirring process is performed for 15 minutes to 30 minutes.

10. A high performance plastic additive and a preparation method thereof according to claim 8, characterized in that: In S3, during mixing, the stirring speed is controlled at 720 rpm to 880 rpm, and the stirring process is performed for 15 minutes to 30 minutes.