PC / ABS (Polycarbonate / Acrylonitrile Butadiene Styrene) alloy containing hyperbranched amide compatibilizer
By using the hyperbranched amide compatibilizer HBPA to mix with PC, ABS resin and glass fiber in a twin-screw extruder, the problem of low efficiency of existing PC/ABS alloy compatibilizers is solved, and the mechanical properties and compatibility of the alloy are significantly improved.
Patent Information
- Application Number
- CN202411211166.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-19
AI Technical Summary
Existing PC/ABS alloys use inefficient compatibilizers and are difficult to prepare, failing to meet the mechanical strength and compatibility requirements of complex applications.
Hyperbranched amide compatibilizer HBPA was prepared by synthesizing amide via the acyl chloride method using hyperbranched amide type compatibilizer. It was then mixed with PC, ABS resin and glass fiber in a twin-screw extruder to form a PC/ABS/GF/HBPA alloy.
The tensile strength, tensile modulus, flexural strength, flexural modulus and impact toughness of PC/ABS alloys were improved, significantly enhancing the overall performance of the alloys.
Smart Images

Figure CN118978801A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to a PC / ABS alloy containing a hyperbranched amide type compatibilizer. Background Art
[0002] PC / ABS alloy has excellent mechanical and thermal properties, which make PC / ABS widely used in various engineering plastic products. With the continuous development of society, the defects of PC / ABS alloy are becoming increasingly prominent: its mechanical strength is low and cannot meet various complex application scenarios; moreover, its compatibility is also poor, so it is particularly important to modify and expand its capacity. Since PC / ABS alloy can be extended to products with different properties according to different ratios and added reinforcing agents, it is of great academic and economic value to develop high-performance PC / ABS alloys and technologies and processes by studying the influence of processing parameters, types of reinforcing agents, characteristics of reinforcing agents, material surface treatment conditions and other factors on the performance of PC / ABS alloys, and to develop and prepare high-efficiency reinforcing agents suitable for PC / ABS alloys. And since PC / ABS alloy can be extended to chemical products with different properties according to different ratios and added compatibilizers, it is of great academic and economic value to study the influence of the types and addition amounts of compatibilizers on PC / ABS alloys, as well as the mechanism of action of compatibilizers on PC / ABS alloys, for the development and preparation of high-efficiency compatibilizers suitable for PC / ABS alloys.
[0003] Non-reactive compatibilizers have become the preferred compatibilizers for various complex polymer materials. They can effectively improve the performance of materials and make them compatible with other materials, thereby achieving better performance. There are many varieties of these compatibilizers, from block copolymers to graft copolymers to random copolymers, all of which can meet various complex application requirements.
[0004] Reactive compatibilizers are polymers composed of a non-polar polymer main chain and active groups (such as hydroxyl groups and epoxy groups, which are mostly random). Since its non-polar polymer main body is compatible with the non-polar polymer in the blend, and its polar groups can react or bond with the active groups of the polar polymer in the blend, it can play a good compatibilizing role
[47] . It is generally a macromolecular type, and its active functional groups can be at the end of the molecule or on the side chain of the molecule. Its macromolecular main chain can be the same as or different from at least one polymer matrix in the blend system. However, in different cases, its macromolecular main chain should have good compatibility with at least one polymer matrix in the blend system. After adding the compatibilizer, the PC / PP blend can have a more uniform two-phase structure, and the particle size of the dispersed phase PP becomes smaller; the dynamic mechanical properties test (DMR) results show that the addition of the compatibilizer makes the Tg peaks of PC and PP tend to approach each other; the DSC results show that the addition of the compatibilizer reduces the crystallinity of the dispersed phase PP and changes the crystal morphology from homogeneous nucleation to heterogeneous nucleation. The melt flow rate (MFR) test shows that the MFR of the PC / PP blend increases with the addition of the compatibilizer, and the processing fluidity becomes better.
[0005] However, the existing PC / ABS alloys use mostly non-reactive compatibilizers, which have low efficiency and high preparation difficulty. Therefore, it is necessary to develop a PC / ABS alloy with a new compatibilizer. Summary of the invention
[0006] The purpose of the present invention is to solve the above-mentioned problems and to propose a PC / ABS alloy containing a hyperbranched amide type compatibilizer.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A PC / ABS alloy containing a hyperbranched amide type compatibilizer comprises the PC / ABS alloy, wherein the components thereof are expressed by weight as follows: 146 parts of a reinforcing agent GF, 30 parts of a hyperbranched amide compatibilizer (HBPA), 577 parts of a PC resin, and 247 parts of an ABS resin.
[0009] Furthermore, the hyperbranched amide compatibilizer uses trimethyl acyl chloride and p-phenylenediamine as monomers, and adopts the acyl chloride method to synthesize amide to prepare the hyperbranched amide.
[0010] Further, the preparation of the hyperbranched amide compatibilizer comprises the following steps:
[0011] (1) Preparation of tools: 500 mL three-necked flask, separatory funnel, stirring paddle, beaker, etc. were cleaned with deionized water and placed in a drying oven for drying before use.
[0012] (2) Use a 100 mL measuring cylinder to measure 300 mL of acetone in a three-necked flask, weigh 6.64 g of trimethylol chloride and add it to the acetone, then turn on the stirring paddle to quickly dissolve the trimethylol chloride; weigh 3.18 g of anhydrous sodium carbonate and 5.41 g of p-phenylenediamine, and add them to 100 mL of 80°C deionized water. When they are completely dissolved, the solution will turn reddish brown; slowly add the reddish brown liquid dropwise into the three-necked flask through a separatory funnel, and the solution in the three-necked flask quickly turns into a green turbid solution, and then heat the mixture in 20°C water for 6 hours; after the reaction is completed, the green suspension is filtered by suction, and the obtained green solid is washed with acetone 3 times, and then washed with deionized water above 80°C 3 times, and filtered by suction several times to remove small molecular substances; finally, it is placed in a vacuum drying oven at 80°C and dried for 12 hours.
[0013] (3) The prepared compatibilizer HBPA was analyzed by Fourier transform infrared spectroscopy using KBr pellet method. The compatibilizer HBPA was analyzed by nuclear magnetic resonance spectrometer at 25°C. 1 H-NMR analysis.
[0014] Furthermore, the preparation of the PC / ABS / GF / HBPA alloy comprises the following steps:
[0015] (1) Drying of PC and ABS masterbatch: Use a glass petri dish to hold the resin particles. The particle stacking depth should not exceed 2 cm. Place the PC resin particles and ABS resin particles in a drying oven at 120°C overnight.
[0016] (2) Preparation of PC / ABS alloy by twin-screw extrusion: Weigh the corresponding weight ratio of PC resin particles and ABS resin particles respectively, mix them evenly and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C and the lower cavity plate of the twin-screw extruder is 260°C. Then the material is cooled and granulated.
[0017] (3) Preparation of PC / ABS / GF alloy by twin-screw extrusion: Weigh the corresponding weight of PC particles, ABS particles and chopped glass fibers respectively, mix them evenly and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C and the lower cavity plate of the twin-screw extruder is 260°C. Then the materials are cooled and granulated.
[0018] (4) Preparation of PC / ABS / GF / HBPA alloy by twin-screw extrusion method: Weigh the corresponding weight of PC resin particles, ABS resin particles, short glass fibers, and HBPA particles respectively, mix them evenly, and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C, and the lower cavity plate of the twin-screw extruder is 260°C. Then, the materials are cooled and granulated.
[0019] (5) Plastic alloy injection molding: Use a micro-injection molding machine to mold the obtained small piece of plastic alloy into a standard test specimen. The injection temperature and mold temperature of the micro-injection molding machine are set to 280°C and 80°C respectively; the holding pressure of the micro-injection molding machine is 450 bar, and the holding time is 5 seconds; the injection pressure of the micro-injection molding machine is 500 bar, and the injection time is 6 seconds. The obtained plastic alloy injection molding specimen is quickly removed from the mold to prevent cooling and adhesion.
[0020] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0021] The hyperbranched amide structure compatibilizer prepared in the present invention is a reactive compatibilizer. Compared with other compatibilizers, the hyperbranched amide structure compatibilizer has high action efficiency and is easy to prepare, so a small amount of addition can bring excellent effects on the performance of the alloy;
[0022] Moreover, the PC / ABS alloy prepared by adding the hyperbranched amide structure compatibilizer has significantly improved tensile strength, tensile modulus, flexural strength, flexural modulus and impact toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of the synthesis process of the hyperbranched amide compatibilizer provided by the present invention is shown;
[0024] Figure 2 A schematic diagram showing the preparation of a hyperbranched amide compatibilizer by a twin-screw extruder and an injection molding machine provided by the present invention;
[0025] Figure 3 A schematic diagram showing the results of nuclear magnetic resonance hydrogen spectrum detection of HBPA provided by the present invention is shown;
[0026] Figure 4 Schematic diagram showing the test results of (a) tensile strength (b) tensile modulus (c) elongation at break of the PC / ABS alloy provided by the present invention;
[0027] Figure 5 Schematic diagram showing the test results of (a) tensile strength (b) tensile modulus (c) elongation at break of the PC / ABS / GF alloy provided by the present invention;
[0028] Figure 6 A schematic diagram showing the test results of (a) tensile strength, (b) tensile modulus and (c) elongation at break of the PC / ABS / GF / HBPA alloy provided by the present invention;
[0029] Figure 7 A schematic diagram showing the test results of (a) flexural strength and (b) flexural modulus of a PC / ABS alloy provided by the present invention;
[0030] Figure 8 A schematic diagram showing the test results of (a) flexural strength and (b) flexural modulus of a PC / ABS / GF alloy provided by the present invention;
[0031] Fig. 9 A schematic diagram showing the test results of the impact performance test of the PC / ABS alloy provided by the present invention is shown;
[0032] Fig.10 A schematic diagram showing the test results of the impact performance test of the PC / ABS / GF alloy provided by the present invention is shown;
[0033] Fig.11 A schematic diagram of SEM characterization of a PC / ABS alloy provided according to the present invention is shown;
[0034] Fig.12 A schematic diagram of SEM characterization of a PC / ABS / GF alloy provided according to the present invention is shown;
[0035] Fig.13 A schematic diagram of SEM characterization of the PC / ABS / GF / HBPA alloy provided according to the present invention is shown. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] See also Figure 1-13 The present invention provides a technical solution: a PC / ABS alloy containing a hyperbranched amide type compatibilizer, wherein the components thereof are expressed by weight as follows: 146 parts of reinforcing agent GF, 30 parts of hyperbranched amide compatibilizer (HBPA), 577 parts of PC resin, and 247 parts of ABS resin.
[0038] The hyperbranched amide compatibilizer uses trimethyl acyl chloride and p-phenylenediamine as monomers and adopts the acyl chloride method to synthesize amide to prepare the hyperbranched amide.
[0039] 1. The preparation of the hyperbranched amide compatibilizer comprises the following steps:
[0040] (1) Preparation of tools: 500 mL three-necked flask, separatory funnel, stirring paddle, beaker, etc. were cleaned with deionized water and placed in a drying oven for drying before use.
[0041] (2) Use a 100 mL measuring cylinder to measure 300 mL of acetone in a three-necked flask, weigh 6.64 g of trimethylol chloride and add it to the acetone, then turn on the stirring paddle to quickly dissolve the trimethylol chloride; weigh 3.18 g of anhydrous sodium carbonate and 5.41 g of p-phenylenediamine, and add them to 100 mL of 80°C deionized water. When they are completely dissolved, the solution will turn reddish brown; slowly add the reddish brown liquid dropwise into the three-necked flask through a separatory funnel, and the solution in the three-necked flask quickly turns into a green turbid solution, and then heat the mixture in 20°C water for 6 hours; after the reaction is completed, the green suspension is filtered by suction, and the obtained green solid is washed with acetone 3 times, and then washed with deionized water above 80°C 3 times, and filtered by suction several times to remove small molecular substances; finally, it is placed in a vacuum drying oven at 80°C and dried for 12 hours.
[0042] (3) The prepared compatibilizer HBPA was analyzed by Fourier transform infrared spectroscopy using KBr pellet method. The compatibilizer HBPA was analyzed by nuclear magnetic resonance spectrometer at 25°C. 1 H-NMR analysis.
[0043] 2. The preparation of PC / ABS / GF / HBPA alloy includes the following steps:
[0044] (1) Drying of PC and ABS masterbatch: Use a glass petri dish to hold the resin particles. The particle stacking depth should not exceed 2 cm. Place the PC resin particles and ABS resin particles in a drying oven at 120°C overnight.
[0045] (2) Preparation of PC / ABS alloy by twin-screw extrusion: Weigh the corresponding weight ratio of PC resin particles and ABS resin particles respectively, mix them evenly and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C and the lower cavity plate of the twin-screw extruder is 260°C. Then the material is cooled and granulated.
[0046] (3) Preparation of PC / ABS / GF alloy by twin-screw extrusion: Weigh the corresponding weight of PC particles, ABS particles and chopped glass fibers respectively, mix them evenly and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C and the lower cavity plate of the twin-screw extruder is 260°C. Then the materials are cooled and granulated.
[0047] (4) Preparation of PC / ABS / GF / HBPA alloy by twin-screw extrusion method: Weigh the corresponding weight of PC resin particles, ABS resin particles, short glass fibers, and HBPA particles respectively, mix them evenly, and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C, and the lower cavity plate of the twin-screw extruder is 260°C. Then, the materials are cooled and granulated.
[0048] (5) Plastic alloy injection molding: Use a micro-injection molding machine to mold the obtained small piece of plastic alloy into a standard test specimen. The injection temperature and mold temperature of the micro-injection molding machine are set to 280°C and 80°C respectively; the holding pressure of the micro-injection molding machine is 450 bar, and the holding time is 5 seconds; the injection pressure of the micro-injection molding machine is 500 bar, and the injection time is 6 seconds. The obtained plastic alloy injection molding specimen is quickly removed from the mold to prevent cooling and adhesion.
[0049] 3. Detection of the H NMR spectrum of the prepared HBPA
[0050] HBPA 1 H-NMR spectrum Figure 3 As shown. It can be seen that there are at least 7 different types of hydrogen atoms, among which δ10.70 and 10.06 ppm are characteristic peaks of protons on amide bonds, δ8.71, 7.87, 7.48, and 6.58 ppm are characteristic peaks of different hydrogen atoms on benzene rings, and the characteristic peak at δ2.52 ppm is the characteristic peak of hydrogen atoms on the terminal amino group (NH2) of HBPA. Generally, the water peak appears at δ3.30 ppm
[67] , but this impurity peak appears at δ3.56 ppm because of the difference between instruments, which is consistent with the results studied by Sun et al.
[68] . Therefore, various types of hydrogen atoms also confirm the successful synthesis of HBPA.
[0051] 4. Testing of the morphology, structure and performance of the prepared PC / ABS / GF / HBPA alloy
[0052] The structures of PC / ABS alloy, PC / ABS / GF alloy and PC / ABS / GF / HBPA alloy were characterized by solid infrared method using Fourier transform infrared spectrometer. The structure of compatibilizer HBPA was characterized by nuclear magnetic resonance spectrometer. The fracture surfaces of tensile specimens of PC / ABS alloy, PC / ABS / GF alloy and PC / ABS / GF / HBPA alloy were observed by scanning electron microscope at 500μm, 200μm, 100μm and 50μm. The mechanical properties of samples were tested by microcomputer-controlled electronic universal testing machine, bending testing machine and impact testing machine. The thermal properties of samples were tested by thermogravimetric analyzer and differential scanning calorimeter.
[0053] 5. Tensile performance test of the prepared PC / ABS / GF / HBPA alloy
[0054] Tensile test: According to GB / T 1040.2-2022 standard
[49] , the tensile strength and elongation at break of the blends were determined by a computer-controlled electronic universal testing machine. The tensile rate was selected as 50 mm / min, the size of the spline was a dumbbell-shaped spline, and the dumbbell-shaped sample type was 1BA type.
[0055] The tensile properties of PC / ABS alloy are tested as follows: Figure 4 As shown. Figure 4 From the data of (a) and 6(b), it can be seen that the tensile properties of PC / ABS alloy are affected by its PC component. When PC:ABS=7:3, the tensile strength of PC / ABS alloy is 71.20MPa, while the tensile modulus shows a trend of first increasing and then decreasing. When PC:ABS=7:3, the tensile modulus reaches the maximum value, and the tensile modulus of PC / ABS alloy is 525.32MPa. The elongation at break is as follows: Figure 4 As shown in (c), with the increase of PC content, the elongation at break will show a trend of first increasing and then decreasing, and when PC:ABS=7:3, the elongation at break can be as high as 100.67%. Compared with PC and ABS, the mechanical properties of PC / ABS alloy are better than those of single PC and ABS, and the ratio of PC / ABS alloy with excellent tensile properties can also be obtained as PC:ABS=7:3. From the tensile property test of PC / ABS alloy, it can be obtained that the ratio of PC to ABS in the PC / ABS alloy with excellent comprehensive performance is PC:ABS=7:3. Based on PC:ABS=7:3, the reinforcing agent GF is added in proportion.
[0056] Tensile test of PC / ABS / GF alloy Figure 5 shown. Figure 5 (a) shows the tensile strength of PC / ABS / GF alloy. With the increase of GF addition, its tensile strength shows a trend of first increasing and then decreasing. When the reinforcing agent GF addition amount is 15%, the tensile strength of PC / ABS / GF alloy reaches the maximum value of 84.31MPa; Figure 5 (b) shows the tensile modulus of PC / ABS / GF alloy. As the amount of reinforcing agent GF added increases, the tensile modulus increases accordingly. When the amount of reinforcing agent GF added is 15%, the tensile modulus of PC / ABS / GF alloy is 931.10MPa. Figure 5 (c) shows the elongation at break of PC / ABS / GF alloy. With the increase of the amount of reinforcing agent GF added, the elongation at break first decreases, starts to increase when the GF addition amount is 10%, reaches the maximum value when the GF addition amount is 20%, and then decreases. When the reinforcing agent GF addition amount is 15%, the elongation at break of PC / ABS / GF alloy is 23.98%. Compared with the single PC / ABS alloy, the mechanical stability of PC / ABS / GF alloy is significantly improved, and when the content of reinforcing agent GF reaches 15%, it has excellent performance.
[0057] From the tensile performance test of PC / ABS alloy, it can be obtained that the ratio of PC to ABS in PC / ABS alloy with relatively excellent comprehensive performance is PC:ABS=7:3. Based on PC:ABS=7:3, the reinforcing agent GF is added in proportion. After the tensile performance test of PC / ABS / GF alloy, the optimal addition amount of reinforcing agent GF is 15%. Based on the ratio of PC:ABS=7:3, the addition amount of reinforcing agent GF is 15% as the standard, and the compatibilizer HBPA is added in proportion.
[0058] The tensile properties of the alloy blended with PC resin particles, ABS resin particles, reinforcing agent GF and compatibilizer HBPA are tested as follows: Figure 6 shown. Figure 6 (a) shows the tensile strength of the alloy blended with PC / ABS / GF alloy and compatibilizer HBPA. With the increase of the amount of compatibilizer HBPA added, the tensile strength first increases and then decreases. When the amount of compatibilizer HBPA added is 3%, the tensile strength of the alloy blended with PC / ABS / GF alloy and compatibilizer HBPA reaches the maximum value of 95.51MPa. Figure 6 (b) shows the tensile modulus of the alloy blended with PC / ABS / GF alloy and compatibilizer HBPA. As the amount of compatibilizer HBPA added increases, the tensile modulus curve first increases and then decreases. When the amount of compatibilizer HBPA added is 3%, the tensile modulus of the alloy blended with PC / ABS / GF alloy and compatibilizer HBPA reaches a maximum value of 1799.77MPa. Figure 6 (c) shows the tensile strength of the alloy blended with PC / ABS / GF and HBPA. With the increase of HBPA addition, the elongation at break curve first increases and then decreases. When the HBPA addition is 3%, the elongation at break of PC / ABS / GF / HBPA reaches a maximum value of 7.37%. Compared with the mechanical properties of PC / ABS / GF alloy, the mechanical properties of the alloy blended with PC resin particles, ABS resin particles, reinforcing agent GF and HBPA are more excellent, with good comprehensive performance, and the best HBPA addition can be obtained at 3%.
[0059] 6. Analysis of the bending properties of the prepared PC / ABS / GF / HBPA alloy
[0060] The flexural strength and flexural modulus of PC / ABS alloy are as follows Figure 7 As shown. Among them, Figure 7 (a) shows that as the PC content decreases, the flexural strength will also decrease accordingly. When PC:ABS=7:3, its flexural strength is 97.26MPa; Figure 7(b) shows the bending modulus. As the PC content decreases, its bending modulus first increases and then decreases, reaching a maximum value when PC:ABS = 7:3. When PC:ABS = 7:3, the bending modulus E of the PC / ABS alloy is 2337.33 MPa.
[0061] The flexural strength and flexural modulus of PC / ABS / GF alloy are as follows Figure 8 shown. Figure 8 (a) shows the bending strength of PC / ABS / GF alloy. With the increase of the amount of reinforcing agent GF added, the bending strength curve shows an upward trend. When the GF addition amount is 15%, the bending strength value is 115.80MPa. Figure 8 (b) shows the flexural modulus of PC / ABS / GF alloy. As the amount of reinforcing agent GF added increases, the tensile modulus increases accordingly. When the amount of reinforcing agent GF added is 15%, the flexural modulus of PC / ABS / GF alloy is 4738.60 MPa.
[0062] The bending and impact performance tests of PC / ABS / GF / HBPA alloy are shown in Table 5. It can be seen that the PC / ABS / GF alloy with the addition of compatibilizer HBPA is better than the original in all aspects. The bending strength of the PC / ABS / GF alloy without the addition of compatibilizer HBPA is 115.80MPa, while the bending strength of the PC / ABS / GF alloy with the addition of 3% compatibilizer HBPA is 128.67MPa, and the performance is improved by 11.11%; the bending modulus of the PC / ABS / GF alloy with the addition of compatibilizer HBPA is 4738.60MPa, while the bending strength of the PC / ABS / GF alloy with the addition of 3% compatibilizer HBPA is 5653.00MPa, and the performance is improved by 19.30%.
[0063] Table 5 Bending performance test of PC / ABS / GF / HBPA alloy
[0064]
[0065]
[0066] 7. Impact toughness analysis of the prepared PC / ABS / GF / HBPA alloy
[0067] The impact toughness of PC / ABS alloy is as follows Fig. 9As shown in the figure, with the decrease of PC content, the impact toughness first increases until it reaches the highest point, and then falls back. When the ratio of PC to ABS in PC / ABS alloy is 7:3, the impact toughness of PC / ABS alloy reaches the maximum value. When PC:ABS=7:3, its impact toughness is 14.40kJ / m2. It can be obtained that PC / ABS alloy has better mechanical properties than single material PC and ABS resin.
[0068] Impact toughness of PC / ABS / GF alloy Fig.10 As shown. As the amount of reinforcing agent GF added increases, the impact toughness decreases. When the amount of reinforcing agent GF added is 15%, the impact toughness value of PC / ABS / GF alloy is 6.48kJ / m2. The reason for the decrease is that due to the large amount of fiber added, the friction between the fiber itself and the fiber and the matrix resin during the twin-screw mixing process produces a cutting effect. When subjected to external impact loads, the shorter fiber length cannot form a network in the resin group to absorb the load. In addition, because the distribution of short-cut fibers in the resin matrix will form agglomerations at the interface of the PC / ABS resin alloy, the existence of defects will affect the fracture behavior of the resin alloy and thus affect the mechanical properties of the material.
[0069] The impact toughness of PC / ABS / GF / HBPA alloy is shown in Table 6. The impact toughness of PC / ABS / GF alloy with compatibilizer HBPA is 6.48 kJ / m2, while the flexural strength of PC / ABS / GF alloy with 3% compatibilizer HBPA is 15.57 kJ / m2, which is 140.28% higher.
[0070] Table 6 Impact performance test of PC / ABS / GF / HBPA alloy
[0071]
[0072] 8. Scanning Electron Microscope Analysis of PC / ABS / GF / HBPA Alloy
[0073] SEM characterization of PC / ABS alloy Fig.11 As shown. The fracture surface of PC / ABS alloy is smooth, indicating that PC and ABS have good compatibility; SEM characterization of PC / ABS / GF alloy is shown Fig.12 As shown in the figure, it can be seen that GF is mixed in the middle of the PC / ABS alloy. The fracture surface of the PC / ABS / GF alloy is relatively rough and has many wrinkles, such as Fig.12 As shown in (c), the compatibility of PC / ABS / GF alloy is poor; the SEM characterization of the alloy mixed with PC / ABS / GF alloy and compatibilizer HBPA is as follows Fig.13As shown in the figure, the fracture surface of the PC / ABS / GF alloy mixed with the compatibilizer HBPA is relatively smooth, without a large number of bubbles or wrinkles. Fig.13 As shown in (c), it shows that the interfacial tension of PC / ABS / GF alloy and HBPA alloy is low so that the fracture surface is relatively smooth. The addition of reinforcing agent GF makes the compatibility of PC / ABS / GF alloy worse, but the addition of HBPA improves the poor compatibility of PC / ABS / GF alloy, making its interfacial compatibility better and having better comprehensive performance. The reason why the compatibility of the alloy is improved by adding HBPA is that in the structure of HBPA, there are a large number of functional groups at the end, and the presence of a large number of functional groups at the end helps to form a large number of hydrogen bonds or chemical crosslinking with other polymers.
[0074] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A PC / ABS alloy containing a hyperbranched amide type compatibilizer, characterized in that: The PC / ABS alloy comprises, by weight, 146 parts of reinforcing agent GF, 30 parts of hyperbranched amide compatibilizer (HBPA), 577 parts of PC resin, and 247 parts of ABS resin.
2. A PC / ABS alloy containing a hyperbranched amide type compatibilizer according to claim 1, characterized in that: The hyperbranched amide compatibilizer uses trimethyl acyl chloride and p-phenylenediamine as monomers and adopts the acyl chloride method to synthesize amide to prepare the hyperbranched amide.
3. A PC / ABS alloy containing a hyperbranched amide type compatibilizer according to claim 2, characterized in that: The preparation of the hyperbranched amide compatibilizer comprises the following steps: (1) Prepare tools: 500 mL three-necked flask, separatory funnel, stirring paddle, beaker, etc., clean with deionized water and place in a drying oven for drying before use; (2) Use a 100 mL measuring cylinder to measure 300 mL of acetone in a three-necked flask, weigh 6.64 g of trimethylol chloride and add it to the acetone, then turn on the stirring paddle to quickly dissolve the trimethylol chloride; weigh 3.18 g of anhydrous sodium carbonate and 5.41 g of p-phenylenediamine, and add them to 100 mL of 80°C deionized water. When they are completely dissolved, the solution will turn reddish brown; slowly add the reddish brown liquid dropwise into the three-necked flask through a separatory funnel, and the solution in the three-necked flask quickly turns into a green turbid solution, and then heat the mixture in 20°C water for 6 hours; after the reaction is completed, the green suspension is filtered by suction, and the obtained green solid is washed with acetone 3 times, and then washed with deionized water above 80°C 3 times, and filtered by suction several times to remove small molecules; finally, it is placed in a vacuum drying oven at 80°C and dried for 12 hours; (3) The prepared compatibilizer HBPA was analyzed by infrared spectroscopy using a KBr pellet method using a Fourier transform infrared spectroscopy, and the compatibilizer HBPA was analyzed by a nuclear magnetic resonance spectrometer at 25°C. 1 H-NMR analysis.
4. A PC / ABS alloy containing a hyperbranched amide type compatibilizer according to claim 1, characterized in that: The preparation of the PC / ABS / GF / HBPA alloy comprises the following steps: (1) Drying of PC and ABS masterbatch: Use a glass petri dish to hold the resin particles. The particle stacking depth should not exceed 2 cm. Place the PC resin particles and ABS resin particles in a drying oven at 120°C overnight. (2) Preparation of PC / ABS alloy by twin-screw extrusion: Weigh the PC resin particles and ABS resin particles of corresponding weights respectively, mix them evenly and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C and the lower cavity plate of the twin-screw extruder is 260°C. Then the materials are cooled and granulated. (3) Preparation of PC / ABS / GF alloy by twin-screw extrusion: Weigh the corresponding weight of PC particles, ABS particles, and chopped glass fibers respectively, mix them evenly, and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C, and the lower cavity plate of the twin-screw extruder is 260°C. Then the materials are cooled and granulated. (4) Preparation of PC / ABS / GF / HBPA alloy by twin-screw extrusion: Weigh the corresponding weight of PC resin particles, ABS resin particles, chopped glass fibers, and HBPA particles, mix them evenly, and add them into a twin-screw extruder. The upper cavity plate of the twin-screw extruder is 230°C, and the lower cavity plate of the twin-screw extruder is 260°C. Then the materials are cooled and granulated. (5) Plastic alloy injection molding: Use a micro injection molding machine to injection mold the obtained small piece of plastic alloy into a standard test specimen. The injection temperature and mold temperature of the micro injection molding machine are set to 280°C and 80°C respectively; the holding pressure of the micro injection molding machine is 450 bar, and the holding time is 5 seconds; the injection pressure of the micro injection molding machine is 500 bar, and the injection time is 6 seconds. The obtained plastic alloy injection molded specimen is quickly removed from the mold to prevent cooling and adhesion.