Preparation method and application of iron-based heteronuclear diatomic active site oxygen reduction catalyst
By loading iron salts and second metal salts with liquid-phase electrostatic adsorption technology on nitrogen-doped carbon, an iron-based heteronuclear diatomic catalyst with clear active sites was prepared, which solved the poor activity of single-atom catalysts and the double-dual catalysts. The problem of unclear active sites of atomic catalysts significantly improves the oxygen reduction performance and stability of fuel cells, reduces costs, and is suitable for a variety of fuel cell applications.
Patent Information
- Application Number
- CN202310620021.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
The catalytic activity of existing iron-based single-atom catalysts is not ideal in oxygen reduction reaction, resulting in limited performance of fuel cells, and metal agglomeration in diatomic catalysts leads to unclear active sites, affecting catalytic performance.
Using liquid-phase electrostatic adsorption technology to upload iron salts and second metal salts to nitrogen-doped carbons, iron-based heteronuclear diatomic catalysts with clear active sites were prepared through high-temperature calcination, and nitrogen-doped carbons were used as support to expose rich ones. Active site.
The high oxygen reduction activity and stability of the catalyst is achieved, the cost is reduced, and the performance of the fuel cell is improved. It is especially effective in acid oxygen reduction reaction, and is suitable for hydrogen-oxygen fuel cells and hydrogen air fuels. Cathode catalyst for the battery.
Smart Images

Figure CN119050385A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy materials and electrochemical catalysis, and specifically relates to a preparation method and application of an oxygen reduction catalyst with an iron-based heteronuclear diatomic active site. Background Art
[0002] Fuel cells are energy conversion devices that convert the chemical energy of fuel into electrical energy. They have important applications in the automotive and energy storage fields. At present, the commercialization process of fuel cells is seriously hindered by the high cost of their cathode catalysts. In order to further reduce the cost of fuel cells, the key lies in the development of cathode oxygen reduction catalysts. Single-atom iron catalysts have attracted extensive research and attention because they show excellent electrocatalytic performance in oxygen reduction. In order to further improve the catalytic activity and stability of single-atom iron catalysts, a second metal atom is introduced to form a diatomic catalyst, especially an iron-based heteronuclear diatomic catalyst. The synergistic effect between the two metal atoms can significantly improve the catalytic activity and stability. At present, there are still few reports on iron-based heteronuclear diatomic catalysts. Under actual working conditions, the catalytic activity of single-atom iron catalysts is not ideal due to various reasons. Therefore, it is necessary to rationally design and synthesize catalysts with clear iron-based heteronuclear diatomic active sites to improve the oxygen reduction performance of the catalyst, thereby improving the performance of fuel cells. The design and synthesis of oxygen reduction catalysts with iron-based heteronuclear diatoms have extremely important research significance and practical application value, but they have not yet attracted the attention of researchers. Summary of the invention
[0003] The present invention provides a preparation method and application of an iron-based heteronuclear diatomic catalyst with high catalytic activity that is precisely constructed. The method is to anchor an iron pre-salt and a second metal body salt in nitrogen-doped carbon with a diameter of 100-200nm by liquid-phase electrostatic adsorption, and after pyrolysis, the topological conversion is to an iron-based heteronuclear diatomic catalyst with high catalytic activity. The present invention solves the problem of unclear active sites of the catalyst caused by metal agglomeration in diatomic catalysts in the prior art, and the problem of a small proportion of diatomic active sites. These problems all lead to the oxygen reduction performance of the catalyst being hindered, which is not conducive to the development of fuel cells.
[0004] The catalytically active iron-based heteronuclear diatomic catalyst is an active component of iron-based heteronuclear diatomic atoms uniformly loaded on nitrogen-doped carbon, the diameter of the nitrogen-doped carbon is 100-200nm, the iron metal loading is 1.0-1.5wt%, and the loading of another metal is consistent with the amount of iron substance.
[0005] The preparation method of the ultra-thin two-dimensional iron single-atom catalyst with high active site density is as follows: after the nitrogen-doped carbon is evenly ground, it is fully dispersed in ethanol, and an iron salt with a positive charge is loaded by liquid-phase electrostatic adsorption, and then a second metal salt with a negative charge is loaded by electrostatic adsorption; finally, high-temperature calcination is performed in nitrogen or an inert gas, and naturally cooled to room temperature to obtain an iron-based heteronuclear diatomic catalyst with high catalytic activity.
[0006] The diameter of the nitrogen-doped carbon is 100-200 nm.
[0007] The iron salt is ferrous sulfate, and the second metal salt is ammonium chlorostannate, potassium cobalt cyanide and potassium nickel cyanide.
[0008] The mass ratio of the nitrogen-doped carbon to the iron salt is 20:1-1.5, and the atomic ratio of the iron salt to the second metal salt is 1:1.
[0009] The flow rate of the argon or inert gas is 10-100 mL min -1 .
[0010] The high temperature calcination is 2-10℃min -1 Heat to 900-1100°C at a heating rate and maintain for 30-300 min.
[0011] The iron-based heteronuclear diatomic catalyst with clear active sites prepared above is used in catalyzing oxygen reduction reactions.
[0012] The application of the iron-based heteronuclear diatomic catalyst with clear active sites prepared above in the preparation of fuel cells.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] (1) The present invention uses a nitrogen-doped carbon as the carbon substrate, which saves the cost of raw materials. The synthesis is simple through one-step calcination synthesis. The yield is large, the preparation is easy, and it is conducive to industrialization.
[0015] (2) The present invention innovatively adopts an electrostatic adsorption self-assembly strategy to prepare an iron-based heteronuclear diatomic catalyst with clear active sites. The catalyst can obtain ultra-high oxygen reduction catalytic activity without secondary loading. The preparation method is simple, highly reproducible, high in yield, cost-saving, easy to industrialize on a large scale, and the prepared iron-based heteronuclear diatomic catalyst is green and environmentally friendly.
[0016] (3) The active sites of the iron-based heteronuclear diatomic catalyst prepared by the present invention are non-precious metals such as iron, tin, cobalt and krypton. The earth's reserves are abundant and environmentally friendly. Compared with traditional platinum-based catalysts, it is cheap and has outstanding performance.
[0017] (4) The iron-based heteronuclear diatomic catalyst prepared by the present invention has clear diatomic active sites. The catalyst uses nitrogen-doped carbon as a carrier, which is conducive to exposing abundant active sites. The liquid-phase electrostatic adsorption technology proposed and used for the first time obtained an iron-based heteronuclear diatomic catalyst with clear active sites, so that the catalyst exhibits excellent catalytic activity and stability in the acidic oxygen reduction reaction (ORR).
[0018] (5) The iron-based heteronuclear diatomic catalyst prepared by the present invention can be used as a cathode catalyst for hydrogen-oxygen fuel cells and hydrogen-air fuel cells and has excellent performance, which is conducive to promoting the development of high energy storage systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a transmission electron microscopy (TEM) image of the Fe1Sn1-NC catalyst prepared in Example 1.
[0020] Figure 2 is an aberration-corrected high-angle annular dark field scanning transmission electron microscopy image (AC-HAADF-STEM) of the Fe1Sn1-NC catalyst prepared in Example 1.
[0021] Figure 3 is an aberration-corrected high-angle annular dark field scanning transmission electron microscopy image (AC-HAADF-STEM) of the Fe1Co1-NC catalyst prepared in Example 2.
[0022] Figure 4 is an aberration-corrected high-angle annular dark field scanning transmission electron microscopy image (AC-HAADF-STEM) of the Fe1Ni1-NC catalyst prepared in Example 3.
[0023] Figure 5 This is the energy dispersive X-ray spectroscopy (EDX) elemental map of the Fe1Sn1-NC catalyst prepared in Example 1.
[0024] Figure 6 This is the energy dispersive X-ray spectroscopy (EDX) elemental map of the Fe1Co1-NC catalyst prepared in Example 1.
[0025] Figure 7 This is the energy dispersive X-ray spectroscopy (EDX) elemental map of the Fe1Ni1-NC catalyst prepared in Example 1.
[0026] Figure 8It is a linear voltammogram of oxygen reduction of the Fe1Sn1-NC catalyst obtained in Example 1, the Fe1Co1-NC catalyst obtained in Example 2, the Fe1Ni1-NC catalyst obtained in Example 3, the Fe-NC catalyst obtained in Comparative Example 1 and 20 wt % of commercial Pt / C in 0.1 M HClO4 as the electrolyte.
[0027] Fig. 9 It is a graph of hydrogen peroxide yield and transferred electron number of the Fe1Sn1-NC catalyst obtained in Example 1, the Fe1Co1-NC catalyst obtained in Example 2, the Fe1Ni1-NC catalyst obtained in Example 3, the Fe-NC catalyst obtained in Comparative Example 1 and 20 wt % of commercial Pt / C in 0.1 M HClO4 as electrolyte.
[0028] Fig.10 It is the oxygen reduction linear voltammetry curve of the Fe1Sn1-NC catalyst obtained in Example 1 before and after 10,000 cycles in 0.1M HClO4 as the electrolyte.
[0029] Fig.11 This is a linear voltammogram of oxygen reduction of the Fe-NC catalyst obtained in Comparative Example 1 before and after 10,000 cycles in 0.1M HClO4 as an electrolyte.
[0030] Fig.12 It is a polarization curve and power density curve diagram of the Fe1Sn1-NC catalyst obtained in Example 1, the Fe1Co1-NC catalyst obtained in Example 2, the Fe1Ni1-NC catalyst obtained in Example 3, the Fe-NC catalyst obtained in Comparative Example 1 and commercial Pt / C when polarized as cathode catalysts for hydrogen and oxygen fuel cells.
[0031] Fig.13 It is a polarization curve and power density curve diagram of the Fe1Sn1-NC catalyst obtained in Example 1, the Fe-NC catalyst obtained in Comparative Example 1 and commercial Pt / C when polarized as cathode catalysts for hydrogen-air fuel cells. DETAILED DESCRIPTION
[0032] To further explain the present invention, the present invention is further described below in conjunction with the accompanying drawings and examples. The following embodiments are merely exemplary embodiments adopted to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be the scope of protection of the present invention.
[0033] Example 1
[0034] (a) Preparation of ZIF-8-NC
[0035] First, 793 mg of zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 2.67 mmol) was dissolved in 20 mL of methanol and ultrasonicated for 10 min, which was marked as solution A. Then, 875 mg of 2-methylimidazole (10.66 mmol) was dissolved in 10 mL of methanol and ultrasonicated for 10 min, which was marked as solution B. Solution A was quickly poured into solution B under vigorous stirring. Subsequently, the solution was stirred at room temperature for 0.5 h; transferred to a hydrothermal reactor and kept warm at 120°C for 4 h. The resulting white precipitate was collected by centrifugation at 8,500 rpm for 3 min and washed three times with ethanol. Finally, it was dried at 60°C for 12 h to obtain ZIF-8 with a diameter of 100-200 nm. ZIF-8 was placed in a tubular furnace with argon as the protective gas. Under argon protection, the reaction mixture was heated at 5°C min -1 The temperature was raised to 950°C at a heating rate of 1.5°C and kept at this temperature for 300 min. After cooling to room temperature in the tube furnace, black powder ZIF-8-NC was obtained.
[0036] (b) Preparation of Fe-Sn heteronuclear diatomic catalysts with clear active sites
[0037] 50 mg of ZIF-8-NC obtained in step (a) was ground evenly, dispersed in 50 mL of ethanol, and ultrasonicated for 10 min. 3.72 mg of ferrous sulfate heptahydrate (FeSO4·7H2O, 0.0133 mmol) was added, and liquid phase electrostatic adsorption was performed for 2 h. Then 4.67 mg of ammonium chlorostannate hydrate ((NH4)2SnCl6, 0.0133 mmol) was added, and liquid phase electrostatic adsorption was performed for 2 h. Fe 2+ [SnCl6] 2+ @ZIF-8-NC. Fe 2+ [SnCl6] 2+ @ZIF-8-NC was placed in the middle of the quartz tube for calcination. Argon was used as the protective gas in the tube furnace with a gas flow rate of 50 mL min -1 , Heating program: start heating at 30℃, 5℃min -1 The temperature was raised to 950°C at a heating rate and kept for 90 min and then cooled naturally to obtain the iron-tin heteronuclear diatomic catalyst Fe1Sn1-NC with clear active sites.
[0038] The iron-tin heteronuclear diatomic catalyst in Example 1 has a rhombic dodecahedral three-dimensional structure ( Figure 1 ), the diameter remains 100-200nm.
[0039] In the aberration-corrected high-angle annular dark-field scanning transmission electron microscopy image (AC-HAADF-STEM), two adjacent bright spots ( Figure 2In addition, the energy dispersive X-ray spectroscopy (EDX) elemental map of Fe1Sn1-NC showed that Fe, Sn and N elements were uniformly distributed throughout the support ( Figure 5 ).
[0040] The Fe1Sn1-NC catalyst was tested for its electrocatalytic oxygen reduction performance, and it was also used as a fuel cell cathode catalyst for fuel cell performance testing.
[0041] Example 2
[0042] According to the operation method of Example 1, the second metal salt was replaced with potassium cobalt cyanide (K3[Co(CN)6]) to obtain Fe1Co1-NC catalyst for electrocatalytic oxygen reduction performance test, and it was used as a fuel cell cathode catalyst for fuel cell performance test.
[0043] Example 3
[0044] According to the operation method of Example 1, the second metal salt was replaced with potassium cobalt cyanide (K2[Ni(CN)6]) to obtain Fe1Ni1-NC catalyst for electrocatalytic oxygen reduction performance test, and it was used as a fuel cell cathode catalyst for fuel cell performance test.
[0045] Comparative Example 1
[0046] The operation method of Example 1 was followed, but without adding the second metal salt, to obtain a Fe-NC catalyst for electrocatalytic oxygen reduction performance test, and the catalyst was used as a fuel cell cathode catalyst for fuel cell performance test.
[0047] Application Example 1
[0048] 4 mg of the catalysts obtained in Example 1, Example 2 and Example 3 were respectively dispersed in a mixture of 685 μL of anhydrous ethanol, 295 μL of deionized water and 20 μL of 5 wt% Nafion. After ultrasonic mixing, 14.4 μL of the dispersed liquid was dropwise applied on a rotating disk electrode. After drying, its oxygen reduction electrocatalytic performance was measured on a Chenhua CHI660E electrochemical workstation.
[0049] In the electrochemical test, a saturated silver-silver chloride electrode was used as the reference electrode, a graphite rod was used as the counter electrode, and 0.1M HClO4 was used as the acidic electrolyte. Before the test, the electrolyte was purged with oxygen for 20 min to obtain an oxygen-saturated acidic electrolyte, and then the electrolyte was charged at 50 mV s -1 The catalyst was activated by cyclic voltammetry scanning at a scan rate of 10 mV s -1 Linear voltammetric scans were performed at a scan rate of 1.
[0050] The ORR test results of Example 1, Example 2, Example 3, Comparative Example 1 and commercial Pt / C in 0.1M HClO4 are as follows Figure 8 As shown. It shows that the ORR performance of the iron-based heteronuclear diatomic catalysts synthesized by the liquid-phase electrostatic adsorption self-assembly strategy is higher than that of the single-atom iron catalyst, and the Fe1Sn1-NC catalyst has the best ORR performance, with a half-wave potential of 0.850V vs RHE, which is 30mV higher than the single-atom iron catalyst and only 10mV lower than the commercial Pt / C. It can be seen from the figure that the ORR activity of the iron-based heteronuclear diatomic catalysts is higher than that of the single-atom iron catalyst, indicating that the active sites are FeSn, FeCo and FeNi diatomic active sites. It shows that the iron-based heteronuclear diatomic active sites clearly defined in the present invention have outstanding advantages.
[0051] The results of the hydrogen peroxide yield test of Example 1, Example 2, Example 3, Comparative Example 1 and 20 wt% commercial Pt / C in 0.1 M HClO4 electrolyte are as follows: Fig. 9 As shown. It shows that the hydrogen peroxide yields of the iron-based heteronuclear diatomic catalysts synthesized by the liquid-phase electrostatic adsorption self-assembly strategy are all less than 3%, among which the hydrogen peroxide yield of the Fe1Sn1-NC catalyst is less than 0.6%, which is much lower than that of the Fe-NC catalyst and the 20wt% commercial Pt / C catalyst. This shows that the clear iron-based heteronuclear diatomic active sites in the present invention have lower hydrogen peroxide yields and higher four-electron process selectivity advantages.
[0052] The stability of the Fe1Sn1-NC catalyst obtained in Example 1 in the oxygen reduction electrocatalytic reaction in 0.1M HClO4 electrolyte is as follows Fig.10 The half-wave potential of the Fe1Sn1-NC catalyst only dropped by 10mV after 10,000 cycles; the limiting current did not drop significantly before and after 10,000 cycles, indicating that it has good cycle stability. The stability of the Fe-NC catalyst obtained in Comparative Example 1 in the oxygen reduction electrocatalytic reaction in 0.1M HClO4 electrolyte is shown in Fig.11 The half-wave potential of the Fe1Sn1-NC catalyst only dropped by 30 mV after 10,000 cycles; the limiting current did not drop significantly before and after 10,000 cycles, indicating that the FeSn-NC catalyst with Fe / Sn diatomic active sites as the main active sites has better stability.
[0053] Application Example 2
[0054] 30 mg of the catalysts prepared in Example 1, Example 2, Example 3, and Comparative Example 1 were dispersed in a mixed solution containing 3000 μL of isopropanol, 50 μL of H2O, and 300 μL of 5% Nafion to form a uniform "ink" as a cathode catalyst. 1.7 mg of 60 wt% commercial Pt / C was dispersed in a mixed solution containing 1000 μL of isopropanol, 50 μL of H2O, and 300 μL of 5% Nafion to form a uniform "ink" as an anode catalyst. Then, the cathode catalyst "ink" was prepared at 3 mg cm -2 The concentration of 0.1 mg was uniformly sprayed on the cathode side of the N211 membrane; the anode catalyst "ink" was sprayed at 0.1 mg Pt cm -2 The concentration of 2000 g was evenly sprayed on the anode side of the N211 membrane. After the catalyst was dried, two 5 cm 2 Carbon paper (28BC, SGL) is pressed onto both sides of the PEM sprayed with the catalyst as a gas diffusion layer. Fuel cell test conditions: single cell temperature: 80°C, cathode and anode humidification tank temperature: 80°C; fuel: H2 / O2 or H2 / Air gas flow rate: 500sccm; humidity: 100%; back pressure: 2.0bar; and polarization curve test using current step mode.
[0055] Comparative Example 2
[0056] The anode catalyst "ink" in Application Example 2 was prepared with 0.1 mg Pt cm -2 The concentration of 0.1 mg Pt cm -2 The concentration of is uniformly sprayed on the cathode side of the N211 membrane. The rest is exactly the same as in Application Example 2.
[0057] like Fig.12 As shown in Figure 2, the peak power density of the hydrogen-oxygen fuel cell based on Fe1Sn1-NC catalyst as the cathode catalyst reached 1.021 W cm -2 , far exceeding the hydrogen-oxygen fuel cell with Fe-NC catalyst as cathode catalyst (0.514 mW cm -2 ), which is closest to the performance of commercial Pt / C as cathode catalyst in hydrogen-oxygen fuel cells (1.275 W cm -2 In addition, the peak power densities of hydrogen-oxygen fuel cells using Fe1Co1-NC and Fe1Ni1-NC as cathode catalysts were 0.685 and 0.680 W cm, respectively. -2The peak power density of hydrogen-air fuel cells based on Fe1Sn1-NC catalyst as cathode catalyst reached 0.594 W cm -2 , far exceeding the hydrogen-air fuel cell with Fe-NC catalyst as cathode catalyst (0.258 mW cm -2 ), once again demonstrating the advantages of iron-based heteronuclear diatomic catalysts in fuel cells.
Claims
1. An iron-based heteronuclear diatomic active site oxygen reduction catalyst, characterized in that: The catalyst is an active component of iron-based heteronuclear diatomic atoms uniformly loaded on nitrogen-doped carbon, the diameter of the nitrogen-doped carbon is 100-200nm, the iron metal loading is 1.0-1.5wt%, and the loading of another metal is consistent with the amount of iron substance.
2. A method for preparing an iron-based heteronuclear diatomic active site oxygen reduction catalyst, characterized in that: The specific operation of the preparation method is: after the nitrogen-doped carbon is evenly ground, it is fully dispersed in ethanol, and an iron salt with a positive charge is loaded by liquid-phase electrostatic adsorption, and then a second metal salt with a negative charge is loaded by electrostatic adsorption; finally, high-temperature calcination is performed in nitrogen or an inert gas, and naturally cooled to room temperature to obtain an iron-based heteronuclear diatomic catalyst with high catalytic activity.
3. The preparation method according to claim 2, characterized in that: The iron salt is ferrous sulfate, and the second metal salt is ammonium chlorostannate, potassium cobalt cyanide and potassium nickel cyanide.
4. The preparation method according to claim 2, characterized in that: The mass ratio of the nitrogen-doped carbon to the iron salt is 20:1-1.5, and the atomic ratio of the iron salt to the second metal salt is 1:
1.
5. The preparation method according to claim 2, characterized in that: The flow rate of the argon or inert gas is 20-100 mL min -1 .
6. The preparation method according to claim 2, characterized in that: The high temperature calcination is 2-10℃min -1 Heat to 900-1100°C at a heating rate and maintain for 30-300 min.
7. Use of the highly catalytically active iron-based heteronuclear diatomic catalyst prepared by the method according to any one of claims 2 to 6 in electrocatalytic oxygen reduction reaction.
8. Use of the iron-based heteronuclear diatomic catalyst with high catalytic activity prepared by the method according to any one of claims 2 to 6 in the preparation of fuel cells.
Citation Information
Cited By
Diatomic metal electrocatalyst as well as preparation method and application thereof
CN119433590A
A diatomic metal electrocatalyst, and a preparation method and application thereof
CN119433590B
Fe-Sn-N-C cathode oxygen reduction catalyst as well as preparation method and application thereof
CN119742380A
Heteronuclear Fe-Zn diatomic catalyst for zinc-air battery and preparation method of heteronuclear Fe-Zn diatomic catalyst