Preparation method of chlorinated polyethylene modified nitrile rubber
By adding functional additives to chlorinated polyethylene modified nitrile rubber and using intelligent kneading and segmented vulcanization technology, the limitations of traditional materials in terms of mechanical properties, chemical resistance and processability are solved, and the further development is achieved. High compatibility and performance improvements, suitable for high-end applications.
Patent Information
- Application Number
- CN202411421387.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional chlorinated polyethylene modified nitrile rubber has limitations in terms of mechanical properties, chemical resistance and processability. The filler is unevenly dispersed, insufficient functionality, and high processing energy consumption, which cannot meet the needs of high-end application scenarios.
Use chlorinated polyethylene, nitrile rubber, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizing agent, accelerator, plasticizer, anti-aging agent and other components, and add graphene microsheets and nanomontmorillonite , thermally conductive graphite, shape memory polymer and multi-wall carbon nanotubes, through intelligent kneading and segmented vulcanization technology, ensure the uniform dispersion of the materials and the formation of cross-linked structures.
It significantly improves the compatibility, mechanical properties, electrical conductivity, thermal conductivity and self-repairing properties of materials, reduces energy consumption, and is suitable for high-functional and multi-purpose industrial scenarios.
Smart Images

Figure CN118930994A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber production, in particular to a method for preparing chlorinated polyethylene modified nitrile rubber. Background Art
[0002] The modified combination of chlorinated polyethylene (CPE) and nitrile rubber (NBR) has been widely used in the field of rubber materials, especially in automobiles, mechanical seals and industrial products. However, traditional chlorinated polyethylene modified nitrile rubber materials usually have limitations in mechanical properties, chemical resistance and processability. For example, the material has poor dispersibility and compatibility, which leads to uneven distribution during mixing and vulcanization, affecting the final product performance. In addition, the existing technology is limited to traditional fillers, such as carbon black, in the application of functional additives, and cannot give the material a wider range of functionality, such as electrical conductivity, thermal conductivity, self-healing, etc., which limits its potential in high-end application scenarios.
[0003] The existing chlorinated polyethylene modified nitrile rubber still faces the following major problems: Uneven dispersion of fillers: Conventional mixing methods make it difficult to effectively disperse fillers and additives evenly in the rubber matrix, affecting the mechanical properties and service life of the product.
[0004] Insufficient functionality: Although common additives such as carbon black can enhance the strength of materials, they lack multifunctional properties such as electrical and thermal conductivity and cannot meet the needs of modern industry for high-functional materials.
[0005] High processing energy consumption: Traditional processing technology consumes a lot of energy, and the control of temperature and shear force is not precise, which can easily lead to material degradation or poor performance. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing chlorinated polyethylene modified nitrile rubber to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical scheme: a method for preparing chlorinated polyethylene modified nitrile rubber, wherein the chlorinated polyethylene modified nitrile rubber comprises the following specific components: chlorinated polyethylene, nitrile rubber, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizing agent, accelerator, plasticizer and antioxidant, and forms a rubber matrix; The mass fractions of the above ingredients are as follows: Chlorinated polyethylene is 25%; Nitrile rubber is 30%; Zinc oxide is 4%; magnesium oxide is 5.7%; Stearic acid is 1%; Carbon black is 10%; The vulcanizing agent is 1.8%; The accelerator is 1.5%; Plasticizer is 7%; Anti-aging agent is 2.5%; The chlorinated polyethylene modified nitrile rubber also includes additives, which include graphene microsheets, nano-montmorillonite, thermal conductive graphite, shape memory polymer and multi-walled carbon nanotubes; The mass fraction of the additives is as follows: Graphene microplatelets are 1.2%; Nano-montmorillonite is 0.6%; Thermal conductive graphite is 1.8%; Shape memory polymers: 1.3%; Multi-walled carbon nanotubes are 6.6%.
[0008] The preparation method of the chlorinated polyethylene modified nitrile rubber is based on the above-mentioned components and additives, and comprises the following steps: S1. Raw material preparation Prepare the required materials, including chlorinated polyethylene, nitrile rubber, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizer, accelerator, plasticizer, antioxidant and additives; S2. Raw material pretreatment The chlorinated polyethylene and the nitrile rubber are pretreated respectively, and the chlorinated polyethylene particles after the pretreatment are uniform, thereby improving the flexibility and plasticity of the nitrile rubber; S3, high speed mixing The pretreated chlorinated polyethylene and nitrile rubber are placed in an internal mixer for high-speed mixing. During the mixing process, plasticizers and antioxidants are added to ensure the uniformity of the mixture and the anti-aging performance of the rubber. S4. Add fillers and additives During high-speed mixing, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizer, and accelerator are gradually added, and a constant temperature is maintained to ensure adequate dispersion between the filler and the rubber matrix and to avoid uneven mixing due to excessively high or low temperatures; S5, first vulcanization The mixed materials need to be vulcanized for the first time. The mixed materials are placed in a mold and subjected to hot pressing to make the vulcanizer in the rubber matrix react with the rubber chain to initially form a cross-linked structure and maintain plasticity. S6, cooling and demoulding After vulcanization is completed, the rubber in the mold is cooled to room temperature and then demolded; S7. Add additives Adding additives, namely graphene microplatelets, nano-montmorillonite, thermally conductive graphite, shape memory polymer and multi-walled carbon nanotubes, to the cooled material; S8, second high-speed mixing The additives and the vulcanized rubber matrix are put into the internal mixer again for high-speed mixing to ensure that the additives are evenly distributed in the rubber; S9, final vulcanization After the second mixing, the second vulcanization process is carried out, the additives are firmly embedded in the rubber matrix, and the shape and performance of the rubber are finally fixed and optimized; S10, Inspection and Post-processing Vulcanized rubber products need to undergo strict quality inspections, including tests of various performance indicators such as tensile strength, hardness, wear resistance, electrical conductivity, and thermal conductivity.
[0009] To further optimize the technical solution, the additives include: Graphene microplatelets, used to enhance the conductivity and mechanical strength of materials; Nano-montmorillonite, as a nano-filler, is used to improve the thermal stability and anti-aging properties of materials; Thermal conductive graphite, as a thermal conductive filler, is used to improve the thermal conductivity of rubber; Shape memory polymers give the material the ability to self-heal. After being deformed by external forces, the polymer returns to its original shape through the memory effect; Multi-walled carbon nanotubes are used to enhance the tensile strength and electromagnetic shielding properties of materials.
[0010] Further optimizing the technical solution, the graphene microsheets are reinforced with the rubber matrix through π-π stacking or hydrogen bonding, and are physically embedded with the matrix through their high surface area. At the same time, the two-dimensional structure of the graphene forms a supporting framework in the rubber matrix, thereby improving the tensile strength, tear resistance and wear resistance of the rubber. The ultrafine particles of the nano-montmorillonite are evenly distributed in the rubber matrix to form a nano-scale barrier structure. The nano-montmorillonite reacts with the chemical groups in the rubber matrix through ion exchange, and the reaction formula is as follows:
[0011] In the formula, nano-montmorillonite interacts with the active groups in the rubber molecules through cation exchange, making it uniformly dispersed in the rubber matrix, thereby enhancing the mechanical and thermal properties.
[0012] To further optimize the technical solution, the thermally conductive graphite is distributed in the rubber matrix to form a thermally conductive channel, which quickly conducts heat from a local area to the whole, enhances the heat dissipation performance of the rubber through its high thermal conductivity, and maintains the mechanical properties of the rubber in a high temperature environment to prevent the rubber from being degraded due to overheating; The shape memory polymer embeds a memory shape in the rubber through chemical cross-linking and molecular chain arrangement. When the material is subjected to external force or deformation, the molecular chain of the polymer will be stretched or compressed; when an external stimulus is applied, the polymer returns to its original shape; the cross-linking reaction of the shape memory polymer is as follows:
[0013] A cross-linked network is generated by the above reaction, and when the shape memory polymer is heated, the cross-linked structure releases strain and restores the shape; The multi-walled carbon nanotubes form a three-dimensional network structure in the rubber matrix, which is used to improve the tensile strength and toughness of the rubber. Its high specific surface area provides a larger contact interface for the rubber matrix, enhancing the mechanical properties of the rubber. At the same time, the multi-walled carbon nanotubes form a conductive channel to absorb or shield electromagnetic waves, thereby reducing the impact of external electromagnetic interference.
[0014] To further optimize the technical solution, in step S2, when pre-treating the chlorinated polyethylene and the nitrile rubber, the pre-treatment is assisted by ultrasonic technology, and the high-frequency vibration of the ultrasonic wave improves the uniformity of the chlorinated polyethylene particles and quickly decomposes the chain structure of the nitrile rubber; When ultrasonic treatment is used, the frequency of the ultrasonic equipment is 20kHz, the power is 600W, the treatment time is 10-15 minutes, and the temperature is controlled at 60°C to avoid overheating of the raw materials and affecting performance; A shearing processor is used to perform plasticization pretreatment of the nitrile rubber. The shearing processor has a shearing rate of 3000 rpm, a temperature of 50° C.-60° C., and a processing time of 5 minutes.
[0015] Further optimizing the technical solution, in step S4, during the adding process, fillers with different particle sizes are evenly dispersed in the rubber matrix based on a double dispersion system to form a multi-scale reinforcement structure; The double dispersion system uses large particle size fillers to enhance the tear resistance of rubber, while small particle size fillers enhance its hardness and wear resistance, forming a multi-reinforced composite structure.
[0016] To further optimize the technical solution, in step S3, a first high-speed mixing is performed using an internal mixer; The parameters of the internal mixer are as follows: Rotor speed: 40-60rpm, use low speed in the initial stage of mixing, and increase the speed to 60rpm in the later stage; Temperature: 110℃-120℃; Mixing time: 8-10 minutes.
[0017] To further optimize the technical solution, in step S8, the second high-speed mixing is performed using the same internal mixer as in step S3, and the shear force of the internal mixer is increased to ensure uniform dispersion of the additives; The parameters of the internal mixer are as follows: Rotor speed: 60-80rpm; Temperature: controlled at 85℃-95℃; Mixing time: 12-15 minutes; During the vulcanization process, the viscosity change of the material is monitored to ensure the consistency of the mixture.
[0018] Further optimizing the technical solution, in the steps S5 and S9, a flat vulcanizing machine is used for the first vulcanization, the vulcanization temperature is 160° C., the pressure is 5 MPa, and the vulcanization time is 5-8 minutes for preliminary crosslinking; The final vulcanization treatment adopts a segmented vulcanization process, which is divided into the following stages: The first stage: the vulcanization temperature is 140°C, the vulcanization time is 5 minutes, and the pressure is 3MPa; The second stage: the vulcanization temperature is 170°C, the vulcanization time is 15 minutes, and the pressure is 6MPa; The third stage: cooling treatment, cooling to room temperature of 25°C, the cooling time is 10 minutes.
[0019] To further optimize the technical solution, in step S10, after the detection, the rubber is post-processed according to different uses, such as cutting, punching or surface modification; If the test results do not meet the requirements, the mixing or vulcanization steps are adjusted to ensure that the final product quality meets the standards.
[0020] Compared with the prior art, the present invention provides a method for preparing chlorinated polyethylene modified nitrile rubber, which has the following beneficial effects: The preparation method of chlorinated polyethylene modified nitrile rubber, by setting up the application of intelligent mixing and segmented vulcanization technology, not only effectively improves the compatibility of chlorinated polyethylene and nitrile rubber, reduces energy consumption and optimizes the mechanical properties of the material, so that the product has significant improvements in anti-aging, corrosion resistance, thermal conductivity and electrical conductivity, and solves the problems existing in the prior art; it also significantly enhances the electrical conductivity, thermal conductivity and self-healing performance of the material by adding functional additives such as graphene microsheets, nano-montmorillonite, and thermal conductive graphite. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of the composition of a chlorinated polyethylene modified nitrile rubber proposed in the present invention; Figure 2The present invention provides a schematic flow chart of a method for preparing chlorinated polyethylene modified nitrile rubber. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1: Please refer to Figure 1 A chlorinated polyethylene modified nitrile rubber includes the following specific components: chlorinated polyethylene, nitrile rubber, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizer, accelerator, plasticizer and antioxidant, and forms a rubber matrix.
[0024] The mass fractions of the above ingredients are as follows: Chlorinated polyethylene is 25%; Nitrile rubber is 30%; Zinc oxide is 4%; magnesium oxide is 5.7%; Stearic acid is 1%; Carbon black is 10%; The vulcanizing agent is 1.8%; The accelerator is 1.5%; Plasticizer is 7%; The antioxidant is 2.5%.
[0025] The chlorinated polyethylene modified nitrile rubber also includes additives, which include graphene microsheets, nano-montmorillonite, thermal conductive graphite, shape memory polymer and multi-walled carbon nanotubes.
[0026] The mass fraction of the additives is as follows: Graphene microplatelets are 1.2%; Nano-montmorillonite is 0.6%; Thermal conductive graphite is 1.8%; Shape memory polymers: 1.3%; Multi-walled carbon nanotubes are 6.6%.
[0027] In this embodiment, the additives include: Graphene microplatelets, used to enhance the conductivity and mechanical strength of materials; Nano-montmorillonite, as a nano-filler, is used to improve the thermal stability and anti-aging properties of materials; Thermal conductive graphite, as a thermal conductive filler, is used to improve the thermal conductivity of rubber; Shape memory polymers give the material the ability to self-heal. After being deformed by external forces, the polymer returns to its original shape through the memory effect; Multi-walled carbon nanotubes are used to enhance the tensile strength and electromagnetic shielding properties of materials.
[0028] Furthermore, the graphene microsheets are reinforced with the rubber matrix through π-π stacking or hydrogen bonding, and are physically embedded with the matrix through their high surface area. At the same time, the two-dimensional structure of the graphene forms a supporting framework in the rubber matrix, thereby improving the tensile strength, tear resistance and wear resistance of the rubber.
[0029] Ordinary chlorinated polyethylene modified nitrile rubber generally does not have excellent conductivity and wear resistance. However, by introducing graphene microsheets, not only the conductivity of the material is improved, but also its wear resistance and mechanical strength are enhanced, which makes the rubber more competitive in application scenarios requiring high strength and durability.
[0030] The ultrafine particles of the nano-montmorillonite are evenly distributed in the rubber matrix to form a nano-scale barrier structure. The nano-montmorillonite reacts with the chemical groups in the rubber matrix through ion exchange, and the reaction formula is as follows:
[0031] In the formula, nano-montmorillonite interacts with the active groups in the rubber molecules through cation exchange, making it uniformly dispersed in the rubber matrix, thereby enhancing the mechanical and thermal properties.
[0032] Compared with traditional formulas, the modification of nano-montmorillonite increases the tear resistance and thermal stability of rubber, and effectively improves its anti-aging properties, allowing it to maintain a longer service life in extreme environments.
[0033] The thermally conductive graphite is distributed in the rubber matrix to form a thermally conductive channel, which quickly conducts heat from a local area to the whole, enhances the heat dissipation performance of the rubber through its high thermal conductivity, maintains the mechanical properties of the rubber in a high temperature environment, and prevents the rubber from being degraded due to overheating.
[0034] Traditional chlorinated polyethylene modified nitrile rubber has low thermal conductivity, but after adding thermal conductive graphite, the material can remain stable in high temperature environments and is suitable for scenarios with special requirements for heat dissipation, such as high-temperature industrial equipment seals.
[0035] The shape memory polymer embeds a memory shape in the rubber through chemical cross-linking and molecular chain arrangement. When the material is subjected to external force or deformation, the molecular chain of the polymer will be stretched or compressed; when an external stimulus is applied, the polymer returns to its original shape; the cross-linking reaction of the shape memory polymer is as follows:
[0036] Through the above reaction, a cross-linked network is generated, and when the shape memory polymer is heated, the cross-linked structure releases strain and restores the shape.
[0037] The addition of shape memory polymers gives rubber certain self-healing properties, allowing it to return to its original shape after being deformed, extending the service life of the material, and is particularly suitable for applications with large dynamic loads.
[0038] The multi-walled carbon nanotubes form a three-dimensional network structure in the rubber matrix, which is used to improve the tensile strength and toughness of the rubber. Its high specific surface area provides a larger contact interface for the rubber matrix, enhancing the mechanical properties of the rubber. At the same time, the multi-walled carbon nanotubes form a conductive channel to absorb or shield electromagnetic waves, thereby reducing the impact of external electromagnetic interference.
[0039] Carbon nanotubes are not used in traditional formulas. The addition of this material greatly improves the tensile strength and toughness of the material, and further enhances the electromagnetic shielding performance, making the rubber not only strong but also having excellent protection properties in electromagnetic interference applications.
[0040] Example 2: Please refer to Figure 2 A method for preparing chlorinated polyethylene modified nitrile rubber is based on the chlorinated polyethylene modified nitrile rubber components and additives described in Example 1, comprising the following steps: S1. Raw material preparation Prepare the required materials, including chlorinated polyethylene, nitrile rubber, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizer, accelerator, plasticizer, antioxidant and additives.
[0041] The mass ratio of chlorinated polyethylene to nitrile rubber needs to be adjusted according to the use environment of the final product in order to ensure the chemical resistance and aging resistance of the rubber while maintaining excellent mechanical properties.
[0042] S2. Raw material pretreatment The chlorinated polyethylene and the nitrile rubber are pretreated respectively, and the chlorinated polyethylene particles after the pretreatment are uniform, thereby improving the flexibility and plasticity of the nitrile rubber.
[0043] In this embodiment, when chlorinated polyethylene and nitrile rubber are pretreated, the pretreatment is assisted by ultrasonic technology. The high-frequency vibration of ultrasonic waves improves the uniformity of chlorinated polyethylene particles and quickly decomposes the chain structure of nitrile rubber.
[0044] When ultrasonic treatment is used, the frequency of the ultrasonic equipment is 20kHz, the power is 600W, the treatment time is 10-15 minutes, and the temperature is controlled at 60°C to avoid overheating of the raw materials and affecting performance; A shearing processor is used to perform plasticization pretreatment of the nitrile rubber. The shearing processor has a shearing rate of 3000 rpm, a temperature of 50° C.-60° C., and a processing time of 5 minutes.
[0045] S3, high speed mixing The pretreated chlorinated polyethylene and nitrile rubber are placed in an internal mixer for high-speed mixing. During the mixing process, plasticizers and antioxidants are added to ensure the uniformity of the mixture and the anti-aging properties of the rubber.
[0046] In this embodiment, an internal mixer is used for the first high-speed mixing; The parameters of the internal mixer are as follows: Rotor speed: 40-60rpm, use low speed in the initial stage of mixing, and increase the speed to 60rpm in the later stage; Temperature: 110℃-120℃; Mixing time: 8-10 minutes.
[0047] S4. Add fillers and additives During the high-speed mixing process, zinc oxide, stearic acid, carbon black, vulcanizer and accelerator are gradually added, and a constant temperature is maintained to ensure sufficient dispersion between the filler and the rubber matrix and avoid uneven mixing caused by too high or too low temperature.
[0048] In this embodiment, during the addition process, fillers of different particle sizes are uniformly dispersed in the rubber matrix based on a double dispersion system to form a multi-scale reinforcement structure; The double dispersion system uses large particle size fillers to enhance the tear resistance of rubber, while small particle size fillers enhance its hardness and wear resistance, forming a multi-reinforced composite structure.
[0049] The addition of fillers can significantly improve the mechanical properties of rubber, such as tensile strength, hardness and wear resistance, while vulcanizers and accelerators are used in the subsequent vulcanization process.
[0050] S5, first vulcanization The mixed material needs to undergo the first vulcanization treatment. The mixed material is placed in a mold and subjected to hot pressing treatment so that the vulcanizer in the rubber matrix reacts with the rubber chain to initially form a cross-linked structure and maintain plasticity.
[0051] The first vulcanization time is short and is only used to initially form a cross-linked network of the rubber, thereby improving the stability and shape retention of the material, so that the material can still be adjusted or mixed to a certain extent in subsequent processing, so as not to be too hardened or lose fluidity. The temperature and time should be strictly controlled during the vulcanization process to ensure that the degree of vulcanization is moderate and avoid over-vulcanization or under-vulcanization problems.
[0052] S6, cooling and demoulding After vulcanization is completed, the rubber in the mold is cooled to room temperature and then demolded.
[0053] During the cooling process, the cross-linking network of the rubber gradually stabilizes and the physical properties are further enhanced. When demolding, pay attention to ensure that the surface of the product is smooth to avoid surface damage or bubbles caused by improper operation.
[0054] S7. Add additives Additives, namely graphene microplatelets, nano-montmorillonite, thermal conductive graphite, shape memory polymer and multi-walled carbon nanotubes, are added to the cooled material.
[0055] S8, second high-speed mixing The additives and the vulcanized rubber matrix are put into the internal mixer again for high-speed mixing to ensure that the additives are evenly distributed in the rubber.
[0056] In this embodiment, the second high-speed mixing uses the same internal mixer as in step S3 to increase the shear force of the internal mixer to ensure that the additives are evenly dispersed; The parameters of the internal mixer are as follows: Rotor speed: 60-80rpm; Temperature: controlled at 85℃-95℃; Mixing time: 12-15 minutes; During the vulcanization process, the viscosity change of the material is monitored to ensure the consistency of the mixture.
[0057] S9, final vulcanization After the second mixing, the second vulcanization process is carried out, and the additives are firmly embedded in the rubber matrix. At the same time, the shape and performance of the rubber are finally fixed and optimized. In order to further enhance the cross-linking density of the rubber, it has better high temperature resistance, chemical resistance and shape stability. The vulcanization temperature and time need to be adjusted according to the final use of the material to ensure maximum product performance.
[0058] S10, Inspection and Post-processing Vulcanized rubber products need to undergo strict quality inspections, including tests of various performance indicators such as tensile strength, hardness, wear resistance, electrical conductivity, and thermal conductivity.
[0059] In this embodiment, after passing the test, the rubber is post-processed according to different uses, such as cutting, punching or surface modification; If the test results do not meet the requirements, the mixing or vulcanization steps are adjusted to ensure that the final product quality meets the standards.
[0060] In this embodiment, in the steps S5 and S9, a flat vulcanizing machine is used for the first vulcanization, the vulcanization temperature is 160° C., the pressure is 5 MPa, and the vulcanization time is 5-8 minutes for preliminary crosslinking; The final vulcanization treatment adopts a segmented vulcanization process, which is divided into the following stages: The first stage: the vulcanization temperature is 140°C, the vulcanization time is 5 minutes, and the pressure is 3MPa; The second stage: the vulcanization temperature is 170°C, the vulcanization time is 15 minutes, and the pressure is 6MPa; The third stage: cooling treatment, cooling to room temperature of 25°C, the cooling time is 10 minutes.
[0061] Through staged vulcanization, the first stage uses lower temperature and pressure to form a preliminary cross-linking network and increase the flexibility of the material; the second stage is deep vulcanization at higher temperature and pressure to ensure that the cross-linking density and strength reach the optimal level. This multi-stage vulcanization process can improve the chemical resistance, high temperature resistance and overall mechanical properties of the material, and extend the life of the material in harsh environments. Example
[0062] Based on the chlorinated polyethylene modified nitrile rubber and the preparation method thereof described in Examples 1 and 2, a number of performance tests were conducted, covering key parameters such as the mechanical properties, electrical conductivity, thermal conductivity, wear resistance and self-healing ability of the material. The test results are shown in the following table.
[0063] Test results of properties of chlorinated polyethylene modified nitrile rubber Test Project Test Standards Test Results unit Tensile Strength GB / T 528-2009 18.5 MPa Elongation at break GB / T 528-2009 350 % Hardness (Shore A) GB / T 531-1999 78 Shore A Tear Strength GB / T 529-2008 35 kN / m Electrical conductivity ASTM D257-99 1.2×10^3 Ω·cm Thermal conductivity ASTM E1530-11 0.95 W / (m·K) Abrasion resistance (weight loss) DIN 53516 85 mm³ Self-healing efficiency Self-repairing volume ratio 87 % Tensile strength after aging GB / T 3512-2001 16.2 MPa Elongation at break after aging GB / T 3512-2001 320 % Oil resistance (quality change) ASTM D471-06 3.5 % Acid and alkali resistance (volume change) Volume change in acid-base environment 1.8 % Test results explanation Tensile strength and elongation at break: The tensile strength reaches 18.5MPa and the elongation at break is 350%, indicating that the material has good tensile properties and toughness under high stress conditions. After aging testing, the tensile strength decreases slightly, but still remains at a high level of 16.2MPa.
[0064] Hardness: Shore A hardness is 78, suitable for applications with good wear resistance and impact resistance.
[0065] Tear strength: The tear strength of 35kN / m proves that the material has strong tear resistance and is suitable for seals and sheath materials in harsh environments.
[0066] Conductivity: Conductivity tests show that the resistivity of the material is 1.2×10^3Ω·cm. Thanks to the addition of graphene and multi-walled carbon nanotubes, it has good conductivity and is suitable for fields that require antistatic or conductive functions.
[0067] Thermal conductivity: The thermal conductivity of the material is 0.95W / (m·K), showing excellent thermal conductivity and is suitable for use in equipment and structures with high heat dissipation requirements.
[0068] Wear resistance: The wear test according to DIN standard shows that the weight loss of the material is 85mm³, which means that it has good wear resistance and can maintain a long service life under mechanical friction and wear conditions.
[0069] Self-healing ability: Through testing, the self-healing efficiency of the material is 87%, indicating that after the material is slightly damaged, it can achieve efficient self-healing through the action of shape memory polymers, which helps to extend the service life of the material.
[0070] Oil resistance and acid and alkali resistance: The mass change of the material in an oily environment is 3.5%, showing good oil resistance; the volume change in an acid and alkali environment is 1.8%, indicating that the material has good chemical stability.
[0071] Through these test results, chlorinated polyethylene modified nitrile rubber has excellent performance in mechanical properties, electrical and thermal conductivity, self-healing and chemical resistance, and is suitable for highly functional and multi-purpose industrial scenarios.
[0072] The beneficial effects of the present invention are: The preparation method of chlorinated polyethylene modified nitrile rubber, by setting up the application of intelligent mixing and segmented vulcanization technology, not only effectively improves the compatibility of chlorinated polyethylene and nitrile rubber, reduces energy consumption and optimizes the mechanical properties of the material, so that the product has significant improvements in anti-aging, corrosion resistance, thermal conductivity and electrical conductivity, and solves the problems existing in the prior art; it also significantly enhances the electrical conductivity, thermal conductivity and self-healing performance of the material by adding functional additives such as graphene microsheets, nano-montmorillonite, and thermal conductive graphite.
[0073] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing chlorinated polyethylene modified nitrile rubber, characterized in that: The chlorinated polyethylene modified nitrile rubber comprises the following specific components: chlorinated polyethylene, nitrile rubber, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizing agent, accelerator, plasticizer and antioxidant, and forms a rubber matrix; The mass fractions of the above ingredients are as follows: Chlorinated polyethylene is 25%; Nitrile rubber is 30%; Zinc oxide is 4%; magnesium oxide is 5.7%; Stearic acid is 1%; Carbon black is 10%; The vulcanizing agent is 1.8%; The accelerator is 1.5%; Plasticizer is 7%; Anti-aging agent is 2.5%; The chlorinated polyethylene modified nitrile rubber also includes additives, which include graphene microsheets, nano-montmorillonite, thermal conductive graphite, shape memory polymer and multi-walled carbon nanotubes; The mass fraction of the additives is as follows: Graphene microplatelets are 1.2%; Nano-montmorillonite is 0.6%; Thermal conductive graphite is 1.8%; Shape memory polymer is 1.3%; Multi-walled carbon nanotubes are 6.6%; The preparation method of the chlorinated polyethylene modified nitrile rubber is based on the above-mentioned components and additives, and comprises the following steps: S1. Raw material preparation Prepare the required materials, including chlorinated polyethylene, nitrile rubber, zinc oxide, stearic acid, carbon black, vulcanizer, accelerator, plasticizer, antioxidant and additives; S2. Raw material pretreatment The chlorinated polyethylene and the nitrile rubber are pretreated respectively, and the chlorinated polyethylene particles after the pretreatment are uniform, thereby improving the flexibility and plasticity of the nitrile rubber; S3, high speed mixing The pretreated chlorinated polyethylene and nitrile rubber are placed in an internal mixer for high-speed mixing. During the mixing process, plasticizers and antioxidants are added to ensure the uniformity of the mixture and the anti-aging performance of the rubber. S4. Add fillers and additives During high-speed mixing, zinc oxide, magnesium oxide, stearic acid, carbon black, vulcanizer, and accelerator are gradually added, and a constant temperature is maintained to ensure adequate dispersion between the filler and the rubber matrix and to avoid uneven mixing due to excessively high or low temperatures; S5, first vulcanization The mixed materials need to be vulcanized for the first time. The mixed materials are placed in a mold and subjected to hot pressing to make the vulcanizer in the rubber matrix react with the rubber chain to initially form a cross-linked structure and maintain plasticity. S6, cooling and demoulding After vulcanization is completed, the rubber in the mold is cooled to room temperature and then demolded; S7. Add additives Adding additives, namely graphene microplatelets, nano-montmorillonite, thermally conductive graphite, shape memory polymer and multi-walled carbon nanotubes, to the cooled material; S8, second high-speed mixing The additives and the vulcanized rubber matrix are put into the internal mixer again for high-speed mixing to ensure that the additives are evenly distributed in the rubber; S9, final vulcanization After the second mixing, the second vulcanization process is carried out, the additives are firmly embedded in the rubber matrix, and the shape and performance of the rubber are finally fixed and optimized; S10, Inspection and Post-processing Vulcanized rubber products need to undergo strict quality inspections, including tests of various performance indicators such as tensile strength, hardness, wear resistance, electrical conductivity, and thermal conductivity.
2. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: Among the additives: Graphene microplatelets, used to enhance the conductivity and mechanical strength of materials; Nano-montmorillonite, as a nano-filler, is used to improve the thermal stability and anti-aging properties of materials; Thermal conductive graphite, as a thermal conductive filler, is used to improve the thermal conductivity of rubber; Shape memory polymers give the material the ability to self-heal. After being deformed by external forces, the polymer returns to its original shape through the memory effect; Multi-walled carbon nanotubes are used to enhance the tensile strength and electromagnetic shielding properties of materials.
3. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: The graphene microsheets are reinforced with the rubber matrix through π-π stacking or hydrogen bonding, and are physically embedded with the matrix through their high surface area. At the same time, the two-dimensional structure of the graphene forms a support framework in the rubber matrix, thereby improving the tensile strength, tear resistance and wear resistance of the rubber. The ultrafine particles of the nano-montmorillonite are evenly distributed in the rubber matrix to form a nano-scale barrier structure. The nano-montmorillonite reacts with the chemical groups in the rubber matrix through ion exchange, and the reaction formula is as follows: ; In the formula, nano-montmorillonite interacts with the active groups in the rubber molecules through cation exchange, making it uniformly dispersed in the rubber matrix, thereby enhancing the mechanical and thermal properties.
4. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: The thermally conductive graphite is distributed in the rubber matrix to form a thermally conductive channel, which quickly conducts heat from a local area to the whole, enhances the heat dissipation performance of the rubber through its high thermal conductivity, and maintains the mechanical properties of the rubber in a high temperature environment to prevent the rubber from being degraded due to overheating; The shape memory polymer embeds a memory shape in the rubber through chemical cross-linking and molecular chain arrangement. When the material is subjected to external force or deformation, the molecular chain of the polymer will be stretched or compressed; when an external stimulus is applied, the polymer returns to its original shape; the cross-linking reaction of the shape memory polymer is as follows: ; A cross-linked network is generated by the above reaction, and when the shape memory polymer is heated, the cross-linked structure releases strain and restores the shape; The multi-walled carbon nanotubes form a three-dimensional network structure in the rubber matrix, which is used to improve the tensile strength and toughness of the rubber. Its high specific surface area provides a larger contact interface for the rubber matrix, enhancing the mechanical properties of the rubber. At the same time, the multi-walled carbon nanotubes form a conductive channel to absorb or shield electromagnetic waves, thereby reducing the impact of external electromagnetic interference.
5. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: In the step S2, when the chlorinated polyethylene and the nitrile rubber are pretreated, the pretreatment is assisted by ultrasonic technology, and the high-frequency vibration of the ultrasonic wave improves the uniformity of the chlorinated polyethylene particles and quickly decomposes the chain structure of the nitrile rubber; When ultrasonic treatment is used, the frequency of the ultrasonic equipment is 20kHz, the power is 600W, the treatment time is 10-15 minutes, and the temperature is controlled at 60°C to avoid overheating of the raw materials and affecting performance; A shearing processor is used to perform plasticization pretreatment of the nitrile rubber. The shearing rate of the shearing processor is 3000 rpm, the temperature is 50° C.-60° C., and the processing time is 5 minutes.
6. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: In the step S4, during the adding process, fillers of different particle sizes are uniformly dispersed in the rubber matrix based on a double dispersion system to form a multi-scale reinforcement structure; The double dispersion system uses large particle size fillers to enhance the tear resistance of rubber, while small particle size fillers enhance its hardness and wear resistance, forming a multi-reinforced composite structure.
7. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: In the step S3, a first high-speed mixing is performed using an internal mixer; The parameters of the internal mixer are as follows: Rotor speed: 40-60rpm, use low speed in the initial stage of mixing, and increase the speed to 60rpm in the later stage; Temperature: 110℃-120℃; Mixing time: 8-10 minutes.
8. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: In step S8, the second high-speed mixing is performed using the same internal mixer as in step S3, and the shear force of the internal mixer is increased to ensure uniform dispersion of the additives; The parameters of the internal mixer are as follows: Rotor speed: 60-80rpm; Temperature: controlled at 85℃-95℃; Mixing time: 12-15 minutes; During the vulcanization process, the viscosity change of the material is monitored to ensure the consistency of the mixture.
9. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: In the steps S5 and S9, a flat vulcanizing machine is used for the first vulcanization, the vulcanization temperature is 160° C., the pressure is 5 MPa, and the vulcanization time is 5-8 minutes for preliminary crosslinking; The final vulcanization treatment adopts a segmented vulcanization process, which is divided into the following stages: The first stage: the vulcanization temperature is 140°C, the vulcanization time is 5 minutes, and the pressure is 3MPa; The second stage: the vulcanization temperature is 170°C, the vulcanization time is 15 minutes, and the pressure is 6MPa; The third stage: cooling treatment, cooling to room temperature of 25°C, the cooling time is 10 minutes.
10. The method for preparing chlorinated polyethylene modified nitrile rubber according to claim 1, characterized in that: In the step S10, after the detection, the rubber is post-processed according to different uses, such as cutting, punching or surface modification; If the test results do not meet the requirements, the mixing or vulcanization steps are adjusted to ensure that the final product quality meets the standards.
Citation Information
Patent Citations
Chlorinated polyethylene elastomer modified with carbon black and preparation method of chlorinated polyethylene elastomer
CN107033475A
Water stimulation response rubber composite material and preparation method thereof
CN110591328A
Composite rubber material and preparation method thereof
CN114634658A
High-temperature-resistant and oil-resistant flexible rubber sound insulation material and preparation method thereof
CN115368650A
Cited By
Rubber composition and rubber product
CN119591947A
Low-temperature-resistant material for trailer connector and preparation method of low-temperature-resistant material
CN121064566A