Composition and method for regenerating aged rubber asphalt

By using a composition of liquid rubber and crosslinking agent in aged rubber asphalt, the problem that the prior art cannot restore the viscoelastic properties of aged rubber asphalt is solved, effective regeneration and performance recovery of aged rubber asphalt is achieved, and the flexibility of the road surface is improved and low temperature crack resistance.

CN118930997APending Publication Date: 2024-11-12CHONGQING JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411184018.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing regenerators cannot effectively restore the viscoelastic properties of waste rubber powder modified asphalt in aged rubber asphalt pavement, resulting in cracks, pits, looses and other diseases after the service life of the aged rubber asphalt pavement, which cannot achieve effective regeneration.

Method used

Using a composition including liquid rubber and crosslinking agent, the liquid rubber accounts for 5 to 20 wt% of the mass fraction of the aged rubber bitumen, and the crosslinking agent accounts for 3 to 20 wt% of the mass fraction of the liquid rubber. The aged rubber bitumen is restored by stirring and mixing and curing. viscoelastic properties and compatibility.

Benefits of technology

It effectively restores the viscoelastic characteristics and compatibility of aged rubber asphalt, improves its performance, realizes the regeneration of aged rubber asphalt, and improves the flexibility and low-temperature crack resistance of the road surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930997A_ABST
    Figure CN118930997A_ABST
Patent Text Reader

Abstract

The invention discloses a composition for regeneration of aged rubber asphalt and a regeneration method, the composition for regeneration of aged rubber asphalt comprises liquid rubber and a cross-linking agent; wherein the liquid rubber accounts for 5-20wt% of the aged rubber asphalt in percentage by mass; and the cross-linking agent accounts for 3-20wt% of the mass of the liquid rubber. The composition can realize effective regeneration of aged rubber asphalt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composition for regenerating aged rubber asphalt and a regeneration method, and in particular to a composition for regenerating aged rubber asphalt and a regeneration method for aged rubber asphalt. Background Art

[0002] Rubber asphalt is made by using rubber materials such as waste tires as modifiers and mixing them with base asphalt at high temperature. It not only realizes the recycling of waste resources, but also gives asphalt stronger anti-aging properties, higher viscoelasticity and better noise reduction performance. It is particularly suitable for heavy-load traffic, cold areas or road construction that requires a low-noise environment, and presents a more environmentally friendly and efficient pavement material solution.

[0003] As the service life of rubber asphalt pavement increases, cracks, potholes, looseness, rutting and other defects appear on the pavement due to aging of rubber asphalt and vehicle load. The recycling of rubber asphalt pavement is imminent, and the effective recycling of waste rubber powder modified asphalt is the key. The aging process of waste rubber powder modified asphalt not only involves the aging of the asphalt itself, but also is accompanied by the depolymerization of rubber powder particles and the decay of viscoelastic properties, which causes the destruction of the phase equilibrium of the original system and the failure of the waste rubber powder modification function.

[0004] At present, the existing regeneration agents are basically only used for regeneration of base asphalt and SBS modified asphalt, but these regeneration agents cannot restore the viscoelastic properties of waste rubber powder modified asphalt in aged rubber asphalt pavement. Therefore, it is urgent to find an effective method for regenerating aged rubber asphalt. Summary of the invention

[0005] In view of this, one object of the present invention is to provide a composition for regenerating aged rubber asphalt. The composition of the present invention can achieve effective regeneration of aged rubber asphalt. Another object of the present invention is to provide a method for regenerating aged rubber asphalt.

[0006] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.

[0007] In one aspect, the present invention provides a composition for regenerating aged rubber asphalt, the composition comprising liquid rubber and a cross-linking agent;

[0008] The mass fraction of the liquid rubber in the aged rubber asphalt is 5-20wt%; the mass fraction of the cross-linking agent in the liquid rubber is 3-20wt%. This is conducive to improving the compatibility and flexibility of the aged rubber asphalt, restoring the viscoelastic properties of the aged rubber asphalt, and realizing the effective regeneration of the aged rubber asphalt.

[0009] As mentioned above, the existing regeneration agents are basically only used for regeneration of base asphalt and SBS modified asphalt, and are not suitable for aged rubber asphalt. This is because, compared with base asphalt and SBS modified asphalt, rubber asphalt has significant differences in material composition and performance. As the original unmodified petroleum asphalt, base asphalt has relatively basic performance and is suitable for general road paving. SBS modified asphalt is modified by adding SBS (styrene-butadiene-styrene) polymer to base asphalt, which improves the high temperature stability, low temperature crack resistance and elastic recovery ability of asphalt, and is suitable for occasions with high requirements for road performance. Therefore, base asphalt and SBS modified asphalt are different from rubber asphalt. Therefore, it is necessary to seek a regeneration agent and regeneration method suitable for aged rubber asphalt.

[0010] The present invention has been found through extensive research that the use of a composition comprising liquid rubber and a cross-linking agent for the regeneration of aged rubber asphalt is significantly effective.

[0011] In certain embodiments, the composition for regeneration of aged rubber asphalt of the present invention consists only of liquid rubber and a cross-linking agent.

[0012] In the present invention, the liquid rubber can be selected from those known in the art, for example, it can be carboxylated liquid nitrile rubber, liquid silicone rubber, liquid EPDM rubber, liquid chloroprene rubber, etc. It is preferably carboxylated liquid rubber. According to a specific embodiment of the present invention, the liquid rubber is carboxylated liquid nitrile rubber.

[0013] In the present invention, the crosslinking agent is selected from one of sulfur, peroxide and epoxy vegetable oil, preferably epoxy vegetable oil. Peroxides include but are not limited to dicumyl peroxide (DCP), benzoyl peroxide, sodium peroxide, ethylene glycol diacrylate (EGDA). Preferably, the peroxide is selected from at least one of dicumyl peroxide, benzoyl peroxide, sodium peroxide and ethylene glycol diacrylate, more preferably dicumyl peroxide.

[0014] In the present invention, the amount of the liquid rubber added is 5-20wt% of the mass of the aged rubber asphalt, preferably 9-18wt%, more preferably 10-14wt%. For example, it can be 5wt%, 8wt%, 9wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%.

[0015] In the present invention, the mass fraction of the crosslinking agent in the liquid rubber is 3-20wt%, preferably 5-18wt%, for example, 5wt%, 8wt%, 9wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%.

[0016] According to the composition for regeneration of aged rubber asphalt of the present invention, preferably, the liquid rubber is carboxylated liquid rubber.

[0017] According to the composition for regeneration of aged rubber asphalt of the present invention, preferably, the liquid rubber is carboxylated liquid nitrile rubber.

[0018] According to the composition for regenerating aged rubber asphalt of the present invention, preferably, the crosslinking agent is selected from one of sulfur, peroxide and epoxy vegetable oil. More preferably, the crosslinking agent is epoxy vegetable oil.

[0019] According to the composition for regeneration of aged rubber asphalt of the present invention, preferably, the peroxide is selected from at least one of dicumyl peroxide, benzoyl peroxide, sodium peroxide and ethylene glycol diacrylate.

[0020] On the other hand, the present invention also provides a method for regenerating aged rubber asphalt, comprising the step of regenerating the aged rubber asphalt using the composition as described above, which is conducive to achieving effective regeneration of the aged rubber asphalt.

[0021] In certain embodiments, liquid rubber is first added to aged rubber asphalt, stirred and mixed at a set temperature, then a cross-linking agent is added thereto, stirred and mixed at a set temperature, and then cured to obtain recycled rubber asphalt.

[0022] In other embodiments, a cross-linking agent is first added to the aged rubber asphalt, and stirred and mixed uniformly at a set temperature, and then liquid rubber is added thereto, and stirred and mixed uniformly at a set temperature, and then cured to obtain recycled rubber asphalt.

[0023] The regeneration method according to the present invention preferably comprises the following steps:

[0024] Liquid rubber is added to aged rubber asphalt, and stirred at 160-200°C to obtain a first mixture; a crosslinking agent is then added to the first mixture, and stirring is continued at 160-200°C to obtain a second mixture; the second mixture is solidified to obtain regenerated rubber asphalt. Such a regeneration method can be conducive to the effective regeneration of aged rubber asphalt and is simple to operate.

[0025] In the present invention, liquid rubber is added to aged rubber asphalt for stirring, and the stirring temperature may be 160-200° C., preferably 180-190° C. The stirring speed may be 3000-5000 rpm, preferably 4000-5000 rpm. The stirring time may be 10-30 min, preferably 15-20 min.

[0026] In the present invention, a crosslinking agent is added to the first mixture and stirred, and the stirring temperature may be 160 to 200° C., preferably 180 to 190° C. The stirring speed may be 1000 to 3000 rpm, preferably 1500 to 2500 rpm. The stirring time may be 5 to 9 min, preferably 6 to 8 min.

[0027] According to the regeneration method of the present invention, preferably, the following specific steps are included: adding liquid rubber to aged rubber asphalt, stirring at 160-200°C and 3000-5000rpm for 10-30min to obtain a first mixture; then adding a crosslinking agent to the first mixture, continuing stirring at 160-200°C and 1000-3000rpm for 5-9min to obtain a second mixture; stirring and curing the second mixture at 50-300rpm to obtain recycled rubber asphalt. In the present invention, the curing time can be more than 50min, preferably 50-120min, and more preferably 60-100min.

[0028] According to the regeneration method of the present invention, preferably, the steps include: adding a crosslinking agent to the aged rubber asphalt, stirring at 160-200°C to obtain a third mixture; then adding liquid rubber to the third mixture, continuing stirring at 160-200°C to obtain a fourth mixture; curing the fourth mixture for 50-120 minutes to obtain regenerated rubber asphalt. Such a regeneration method can be conducive to the effective regeneration of aged rubber asphalt and is simple to operate.

[0029] In the present invention, the crosslinking agent is added to the aged rubber asphalt and stirred. The stirring temperature may be 160-200° C., preferably 180-190° C. The stirring speed may be 1000-3000 rpm, preferably 1500-2500 rpm. The stirring time may be 5-9 min, preferably 6-8 min.

[0030] In the present invention, liquid rubber is added to the third mixture for stirring, and the stirring temperature may be 160-200° C., preferably 180-190° C. The stirring speed may be 3000-5000 rpm, preferably 4000-5000 rpm. The stirring time may be 10-30 min, preferably 15-20 min.

[0031] According to the regeneration method of the present invention, preferably, it includes the following specific steps: adding a cross-linking agent to the aged rubber asphalt, stirring at 160-200°C and 1000-3000rpm for 5-9min to obtain a third mixture; then adding liquid rubber to the third mixture, continuing to stir at 160-200°C and 3000-5000rpm for 10-30min to obtain a fourth mixture; stirring the fourth mixture at 50-300rpm and curing for 50-120min to obtain regenerated rubber asphalt.

[0032] The composition of the present invention can better restore the viscoelastic properties of aged rubber asphalt and improve its compatibility, thereby restoring the performance of aged rubber asphalt and achieving effective regeneration of aged rubber asphalt. According to the preferred technical solution of the present invention, the present invention uses functionalized liquid rubber as a reactive polymer plasticizer, and solidifies through a crosslinking reaction of a crosslinking agent to reconstruct the internal crosslinked network structure of the aged rubber asphalt, thereby achieving effective regeneration of the performance of the aged rubber asphalt. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 These are the results of the needle penetration, softening point and ductility of the regenerated rubber asphalt obtained in Examples 1 to 3, as well as the aged rubber asphalt and the unaged rubber asphalt.

[0034] Figure 2 These are the test results of the complex shear modulus of the regenerated rubber asphalt obtained in Examples 4 to 9, as well as the aged rubber asphalt and the unaged rubber asphalt.

[0035] Figure 3 These are the test results of the phase angles of the regenerated rubber asphalt obtained in Examples 4 to 9, as well as the aged rubber asphalt and the unaged rubber asphalt.

[0036] Figure 4 These are the test results of the stiffness modulus of the regenerated rubber asphalt obtained in Examples 4 to 9, as well as the aged rubber asphalt and the unaged rubber asphalt.

[0037] Figure 5 These are the test results of the creep rates of the regenerated rubber asphalt obtained in Examples 4 to 9, as well as the aged rubber asphalt and the unaged rubber asphalt. DETAILED DESCRIPTION

[0038] The following are the raw materials used in the examples:

[0039] Carboxylated liquid nitrile rubber was purchased from Dongguan Shenghao Plastic Raw Materials Co., Ltd. Sulfur and dicumyl peroxide (DCP) were provided by Sigma-Aldrich (Shanghai) Trading Co., Ltd. Epoxy vegetable oil was purchased from Shandong Wushuang Chemical Group Co., Ltd.

[0040] Examples 1 to 3

[0041] Add the crosslinking agent to the aged rubber asphalt, stir at 180°C and 2500rpm for 6 minutes to obtain the third mixture; then add the carboxylated liquid nitrile rubber to the third mixture, continue stirring at 180°C and 3500rpm for 15 minutes to obtain the fourth mixture; stir the fourth mixture at 100rpm and slowly cure for 65 minutes to obtain the recycled rubber asphalt. Among them, the added amount of carboxylated liquid nitrile rubber is 10wt% of the aged rubber asphalt, and the crosslinking agent accounts for 20wt% of the carboxylated liquid nitrile rubber. The feed is shown in Table 1. The test results of the needle penetration, softening point and ductility of the obtained recycled rubber asphalt are shown in Figure 1 .

[0042] Table 1

[0043]

[0044] Embodiments 4 to 9

[0045] Carboxylated liquid nitrile rubber was added to the aged rubber asphalt, and stirred at 180°C and 4000 rpm for 15 minutes to obtain a first mixture; then a crosslinking agent was added to the first mixture, and the mixture was stirred at 180°C and 1500 rpm for 6 minutes to obtain a second mixture; the second mixture was stirred at 100 rpm and slowly cured for 80 minutes to obtain recycled rubber asphalt. The materials are shown in Table 2.

[0046] Table 2

[0047]

[0048] Note: In Table 2, the liquid rubber is carboxylated liquid nitrile rubber.

[0049] Performance Testing

[0050] (I) The penetration, softening point and ductility of the regenerated rubber asphalt obtained in Examples 1 to 3, as well as the aged rubber asphalt and the unaged rubber asphalt were tested. The results are shown in Figure 1 .

[0051] Figure 1 Among them, sulfur crosslinking represents Example 1, peroxide crosslinking represents Example 2, epoxy carboxylation crosslinking represents Example 3, unaged represents unaged rubber asphalt, and long-term aging represents aged rubber asphalt.

[0052] Depend on Figure 1It can be seen that compared with the aged rubber asphalt, the needle penetration and ductility of the regenerated rubber asphalt are increased, and the softening point is also close to the unaged rubber asphalt to varying degrees, indicating that the composition of the present invention helps to improve the flexibility of the aged rubber asphalt and has a good regeneration effect on the aged rubber asphalt. The present invention believes that the composition of the present invention improves the flexibility of the aged rubber asphalt through liquid rubber plasticization and cross-linking curing.

[0053] (ii) The complex shear modulus and phase angle of the regenerated rubber asphalt obtained in Examples 4 to 9 were tested respectively. The results are shown in Table 2. Figure 2 and Figure 3 .

[0054] The test instrument and test conditions are as follows: The rheological properties (including complex shear modulus and phase angle) of recycled rubber asphalt, aged rubber asphalt and unaged rubber asphalt are tested by SYD-0628 asphalt dynamic shear rheometer. The test is carried out in temperature scanning mode. The scanning conditions are as follows: temperature 58-76°C, temperature interval 6°C, strain 12%, and angular frequency 10rad / s.

[0055] Figure 2 and Figure 3 In the embodiment, 5%, 8%, 12% and 20% respectively represent the mass proportion of carboxylated liquid nitrile rubber (liquid rubber) in aged rubber asphalt. ECCR regeneration represents the regeneration of aged rubber asphalt by a composition of epoxy vegetable oil and carboxylated liquid nitrile rubber. For example, 5% ECCR regeneration represents Example 4. SCR regeneration represents the regeneration of aged rubber asphalt by a composition of sulfur and carboxylated liquid nitrile rubber. PCR regeneration represents the regeneration of aged rubber asphalt by a composition of diisopropylbenzene peroxide and carboxylated liquid nitrile rubber.

[0056] Depend on Figure 2 It can be seen that the complex modulus of aged rubber asphalt is the largest, the rigidity increases, the flexibility deteriorates, and the asphalt material becomes hard and brittle, while the complex modulus of recycled rubber asphalt decreases and the flexibility is restored to a certain extent.

[0057] Depend on Figure 3 It can be seen that when the temperature is constant, the phase angle of almost all regenerated rubber asphalt is greater than that of aged rubber asphalt (except 8% ECCR regeneration), which also shows that the composition and regeneration method of the present invention can improve the flexibility of aged rubber asphalt and help to improve low-temperature crack resistance.

[0058] (III) The stiffness modulus S and creep rate m of the regenerated rubber asphalt obtained in Examples 3 to 8 were tested respectively. The results are shown in Table 1. Figure 4 and Figure 5 .

[0059] The test instrument and test conditions are as follows: The low temperature crack resistance of the recycled rubber asphalt is evaluated by using a bending beam creep test (BBR), which is a static load three-point bending creep test. The stiffness modulus S and creep rate m of different rubber asphalts at -18°C are tested in the present invention.

[0060] Depend on Figure 4 It can be seen that the S values ​​of different recycled rubber asphalts are all smaller than the S value of long-term aged rubber asphalt. Among them, 12% ECCR is the best. Figure 5 It can be seen that the m values ​​of different regenerated rubber asphalts are basically greater than the m value of long-term aged rubber asphalt. This shows that the present invention uses the composition to regenerate aged rubber asphalt to restore the elasticity and plasticity of rubber asphalt, improve the deformation capacity of aged rubber asphalt under low-temperature loading, improve low-temperature crack resistance, and has a good regeneration effect.

[0061] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be thought of by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A composition for regenerating aged rubber asphalt, It is characterized in that The composition includes a liquid rubber and a cross-linking agent; The mass fraction of the liquid rubber in the aged rubber asphalt is 5 to 20 wt %; the mass fraction of the cross-linking agent in the liquid rubber is 3 to 20 wt %.

2. The composition according to claim 1, It is characterized in that The liquid rubber is carboxylated liquid rubber.

3. The composition according to claim 1, It is characterized in that The liquid rubber is carboxylated liquid nitrile rubber.

4. The composition according to claim 1, It is characterized in that The cross-linking agent is selected from one of sulfur, peroxide and epoxy vegetable oil.

5. The composition according to claim 4, It is characterized in that The peroxide is selected from at least one of dicumyl peroxide, benzoyl peroxide, sodium peroxide and ethylene glycol diacrylate.

6. A method for regenerating aged rubber asphalt, It is characterized in that The method comprises the step of regenerating aged rubber asphalt by using the composition described in any one of claims 1 to 5.

7. The regeneration method according to claim 6, It is characterized in that The following steps are involved: Liquid rubber is added to aged rubber asphalt, and stirred at 160-200° C. to obtain a first mixture; a crosslinking agent is then added to the first mixture, and stirring is continued at 160-200° C. to obtain a second mixture; and the second mixture is solidified to obtain recycled rubber asphalt.

8. The regeneration method according to claim 7, It is characterized in that The method comprises the following specific steps: adding liquid rubber into aged rubber asphalt, stirring at 160-200° C. and 3000-5000 rpm for 10-30 minutes to obtain a first mixture; then adding a crosslinking agent into the first mixture, stirring at 160-200° C. and 1000-3000 rpm for 5-9 minutes to obtain a second mixture; stirring and curing the second mixture at 50-300 rpm to obtain recycled rubber asphalt.

9. The regeneration method according to claim 6, It is characterized in that The method comprises the following steps: adding a crosslinking agent to aged rubber asphalt, stirring at 160-200° C. to obtain a third mixture; then adding liquid rubber to the third mixture, continuing stirring at 160-200° C. to obtain a fourth mixture; and curing the fourth mixture for 50-120 minutes to obtain recycled rubber asphalt.

10. The regeneration method according to claim 9, It is characterized in that The method comprises the following specific steps: adding a crosslinking agent to aged rubber asphalt, stirring at 160-200° C. and 1000-3000 rpm for 5-9 minutes to obtain a third mixture; then adding liquid rubber to the third mixture, stirring at 160-200° C. and 3000-5000 rpm for 10-30 minutes to obtain a fourth mixture; stirring and curing the fourth mixture at 50-300 rpm for 50-120 minutes to obtain recycled rubber asphalt.