Preparation method of semi-conductive shielding material for crosslinked polyethylene insulated cable

By preparing a semi-conductive shielding material for cross-linked polyethylene insulated cables, the problem of partial discharge caused by cable interface defects was solved, achieving the effect of smooth cable surface, excellent electrical performance and stable physical properties.

CN118931023APending Publication Date: 2024-11-12ANHUI SIHUI CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075230.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively eliminate cable interface defects, leading to partial discharge and uneven electric field, which affect the electrical and physical properties of the cable.

Method used

A semi-conductive shielding material for cross-linked polyethylene insulated cables is prepared by using ethylene-butyl acrylate copolymer resin, conductive carbon black, conductive carbon fiber powder, and paraffin wax through melt extrusion and disc granulation processes. Dicumyl peroxide is added and the material is dried to form a black granular product.

Benefits of technology

The prepared semiconductive shielding material has good color, stability and processability, eliminates cable interface defects, achieves a uniform electric field and avoids partial discharge, and improves the electrical and physical properties of the cable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a preparation method of a semi-conductive shielding material for a crosslinked polyethylene insulated cable, and belongs to the technical field of crosslinked polyethylene, the semi-conductive shielding material is prepared through extrusion granulation of ethylene-butyl acrylate copolymer resin, conductive carbon black and conductive carbon fiber powder, the color and quality performance is uniform, the product stability is high, and the service life is long. The cable has the advantages of being high in cleanliness, resistant to scorching, good in machinability and the like, cable interface defects can be eliminated, an electric field is uniform, partial discharge is avoided, and produced cables are smooth in surface, excellent in electrical performance and physical performance and suitable for CCV and VCV crosslinking production lines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cross-linked polyethylene materials, in particular to a method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable. Background Art

[0002] The so-called "shielding" in the cable structure is essentially a measure to improve the distribution of the electric field. The cable conductor is made of multiple strands of conductor wires twisted together, and it is easy to form an air gap between it and the insulation layer. The surface of the conductor is not smooth, which will cause electric field concentration. A shielding layer of semi-conductive material is added to the surface of the conductor. It is at the same potential as the shielded conductor and has good contact with the insulation layer, thereby avoiding local discharge between the conductor and the insulation layer. This layer of shielding is also called the inner shielding layer. There may also be gaps at the contact point between the insulation surface and the sheath. When the cable is bent, cracks are easily caused on the insulation surface of the oil-paper cable. These are factors that cause local discharge. A shielding layer of semi-conductive material is added to the surface of the insulation layer. It has good contact with the shielded insulation layer and is at the same potential as the metal sheath, thereby avoiding local discharge between the insulation layer and the sheath. Those skilled in the art are in urgent need of developing a method for preparing a semi-conductive shielding material for cross-linked polyethylene insulated cables to meet existing usage needs and performance requirements. Summary of the invention

[0003] In view of the above problems, the present invention aims to provide a method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable.

[0004] The present invention is achieved through the following technical solutions: A method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable, characterized in that it comprises the following steps: (1) uniformly mixing 100-110 parts of ethylene-butyl acrylate copolymer resin, conductive carbon black, conductive carbon fiber powder, 0.8-1 part of antioxidant and 6-8 parts of paraffin wax to obtain a mixture, conveying the mixture to a forced feeder, forcing the mixture into an extruder for melt extrusion granulation, the extruder temperature being 150-160°C, and then entering a storage bin after underwater pelletizing and centrifugal dehydration to obtain shielding material premixed particles; (2) The premixed particles of the shielding material in the storage bin are transported to the disc granulator, the disc granulator is started, and a xylene solution of dicumyl peroxide with a mass fraction of 3% to 4% is sprayed under the rotation of the disc. The disc granulator is rotated for 10 to 15 minutes and then enters the drying bin. After drying for 10 to 12 hours, the disc granulator is obtained. The inclination angle of the disc granulator is 45 to 60 degrees and the rotation speed is 22 to 24 rpm.

[0005] Furthermore, the conductive carbon fiber powder is added in an amount of 5% to 10% of the mixture mass.

[0006] Furthermore, the conductive carbon fiber powder is added in an amount of 20% to 25% of the mixture mass.

[0007] Furthermore, the particle size of the conductive carbon fiber powder is 400-500 mesh.

[0008] Furthermore, the ethylene-butyl acrylate copolymer resin is one of AEB560D and R3427AC.

[0009] Furthermore, the paraffin wax is No. 54 fully refined paraffin wax or No. 58 fully refined paraffin wax.

[0010] Furthermore, the first step antioxidant is one or more of the antioxidant 330 , the antioxidant 300 , or the antioxidant 1010 .

[0011] Furthermore, the drying temperature in step (3) is 65-75° C., and the amount of dicumyl peroxide used is 1.6%-2.4% of the mass of the premixed particles of the shielding material.

[0012] Beneficial effects of the present invention: The invention discloses a method for preparing a semi-conductive shielding material for cross-linked polyethylene insulated cables. The semi-conductive shielding material is in black granular form and is prepared by extruding and granulating ethylene-butyl acrylate copolymer resin, conductive carbon black and conductive carbon fiber powder. The semi-conductive shielding material has uniform color and quality, strong product stability, high cleanliness, scorch resistance, good processability and the like. The semi-conductive shielding material can eliminate cable interface defects, uniform electric field and avoid partial discharge. The produced cable has a smooth surface, excellent electrical and physical properties and is suitable for CCV and VCV cross-linking production lines. DETAILED DESCRIPTION

[0013] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1

[0014] Raw materials and equipment: BUSSPLK46 extruder, Hitech conductive carbon fiber powder particle size is 400 mesh; ethylene-butyl acrylate copolymer resin is AEB560D; black jade pigment CT-4 conductive carbon black; Kunlun No. 54 fully refined paraffin wax; antioxidant 330; ZL10 disc granulator with an inclination angle of 60° and a speed of 24rpm.

[0015] The preparation method of semi-conductive shielding material for cross-linked polyethylene insulated cable comprises the following steps: (1) 100 parts of ethylene-butyl acrylate copolymer resin, conductive carbon black, conductive carbon fiber powder, 0.8 parts of antioxidant and 6 parts of paraffin are uniformly mixed to obtain a mixture, wherein the conductive carbon fiber powder is added in an amount of 10% by mass of the mixture and the conductive carbon fiber powder is added in an amount of 20% by mass of the mixture, and the mixture is transported to a forced feeder, and the forced feed enters a BUSS extruder for melt extrusion granulation; the mixed raw materials in the extruder are melt co-extruded at 150° C. to prepare shielding material premixed particles, which are then entered into a storage bin after underwater pelletizing and centrifugal dehydration; (2) the shielding material premixed particles in the storage bin are transported to a disc granulator, the disc granulator is started, and a xylene solution of diisopropyl peroxide with a mass fraction of 4% is sprayed under the rotation of the disc, and the disc is rotated for 10 minutes before entering a drying bin, the drying temperature is 65° C., and the amount of diisopropyl peroxide is 1.6% by mass of the shielding material premixed particles. After drying for 10 hours, the shielding material premixed particles are obtained. Example 2

[0016] Raw materials and equipment: BUSSPLK46 extruder, Hitech conductive carbon fiber powder with a particle size of 500 mesh; ethylene-butyl acrylate copolymer resin R3427AC; black jade pigment CT-8 conductive carbon black; Kunlun No. 58 fully refined paraffin wax; a mixture of antioxidant 300 and antioxidant 1010 in a mass ratio of 1:1, ZL15 disc granulator, inclination angle 45°, rotation speed 22rpm.

[0017] The preparation method of semi-conductive shielding material for cross-linked polyethylene insulated cable comprises the following steps: (1) 110 parts of ethylene-butyl acrylate copolymer resin, conductive carbon black, conductive carbon fiber powder, 1 part of antioxidant and 8 parts of paraffin are uniformly mixed to obtain a mixture, wherein the conductive carbon fiber powder is added in an amount of 5% by mass of the mixture and the conductive carbon fiber powder is added in an amount of 25% by mass of the mixture, and the mixture is conveyed to a forced feeder, and the mixture is forced to be fed into a BUSS extruder for melt extrusion granulation; the mixed raw materials in the extruder are melt co-extruded at 160° C. to prepare shielding material premixed particles, which are then entered into a storage bin after underwater pelletizing and centrifugal dehydration; (2) the shielding material premixed particles in the storage bin are conveyed to a disc granulator, the disc granulator is started, and a xylene solution of 3% by mass of diisopropyl peroxide is sprayed under the rotation of the disc, and the disc is rotated for 15 minutes before entering a drying bin, the drying temperature is 75° C., and the amount of diisopropyl peroxide is 2.4% by mass of the shielding material premixed particles. The finished products are packaged after drying for 12 hours.

[0018] The performance of the semi-conductive shielding material for cross-linked polyethylene insulated cables of Examples 1 and 2 was tested. The test results are shown in Table 1. Table 1 Performance test results of cross-linked polyethylene insulated cables with semi-conductive shielding materials in Examples 1 to 2

[0019] Note: The specimens are prepared by the particle molding method. The semi-conductive shielding material particles are preheated in the press plate of a hydraulic press at 120°C without pressure for 6 minutes, and then pressurized and heated for 4 minutes to form. The cross-linking conditions of the sample are 180°C × 15min, and the pressure of the hydraulic press should be greater than 15MPa, and then pressurized and cooled to room temperature and demolded. The molding method should be used for arbitration testing: the particles of the semi-conductive shielding material are plasticized and filmed on a plasticizer at 90°C and a roller gap of 2.5mm for 5 minutes, and then the specimens are prepared according to the above regulations. The specimens should be kept flat and smooth, with uniform thickness and no bubbles. The thickness of the specimens should meet the requirements of each test item. The tensile strength and elongation at break tests should be carried out in accordance with the provisions of GB / T1040.1-2018 and GB / T1040.3-2006. The specimen is a type 5 dumbbell sheet with a thickness of 1.0mm and a tensile speed of 250mm / min. Air heat aging test The air heat aging test conditions shall comply with the provisions of Table 1, the thickness is 1.0mm, and there shall be no less than five valid specimens. The air heat aging oven adopts a naturally ventilated electric heat aging oven, which shall comply with the requirements of 8.1 in GB / T2951.12-2008. The tensile strength and elongation at break tests after heat aging shall be carried out in accordance with the provisions of 6.3. The specimen shall be conditioned for no less than 16h in an environment with a temperature of 23°C and a relative humidity of 55%. The impact embrittlement temperature test shall be carried out in accordance with the provisions of GB / T5470-2008, with a specimen thickness of 2.0mm; the thermal extension test shall be carried out in accordance with the provisions of Chapter 9 of GB / T2951.21-2008, with a thickness of 1.0mm. The volume resistivity test determines the volume resistivity at 20°C. The test shall be carried out in accordance with the provisions of GB / T3048.3-2007, and the specimen shall be conditioned for no less than 24h in an environment with a temperature of 23°C and a relative humidity of 45%. Determine the volume resistivity at 90°C. The volume resistivity test shall be carried out in accordance with the provisions of Appendix A of JB / T10738. Determine the volume resistivity at 90°C after heat aging. After heat aging, the volume resistivity at 90°C shall be carried out within 1h. The test shall be carried out in accordance with the provisions of Appendix A of JB / T10738, and the heat aging conditions shall be in accordance with the provisions of Table 1. The preparation of the hot pressing specimens of the insulating material is as follows: The preparation of the hot pressing specimens of the peroxide cross-linked polyethylene insulating material is prepared by the particle molding method. The insulating material particles are preheated in the press plate of the hydraulic press at 120°C without pressure for 6 minutes, and then pressurized and heated for 4 minutes to form. Sample size: 200mm long, 150mm wide, and 2mm thick. The pressure of the hydraulic press should be greater than 15MPa, and the sample is pressurized and cooled to room temperature and removed from the mold. The sample should be flat and smooth, with uniform thickness and no bubbles. Sample cross-linking: Preparation of peroxide cross-linking insulation material and semi-conductive shielding material for easy-to-strip extruded insulated cable. Two hot-pressed peroxide cross-linking insulation material and semi-conductive shielding material for easy-to-strip extruded insulated cable samples are overlapped together. The dimensions of the overlapped samples are: 200mm long, 150mm wide and 4.4mm thick.When the insulating material and semi-conductive shielding material of the sample need to be isolated, an isolation material can be placed. The size of the isolated part of the sample is 210mm long, 30mm wide, and the thickness is not more than 0.1mm. The cross-linking conditions of the sample are 180℃×15min. The pressure of the hydraulic press should be greater than 15MPa. The sample is pressurized and cooled to room temperature and removed from the mold. After cross-linking, the sample should be flat and smooth, with uniform thickness and no bubbles.

Claims

1. A method for preparing a semiconductive shielding material for a cross-linked polyethylene insulated cable, characterized in that: The following steps are involved: (1) 100-110 parts of ethylene-butyl acrylate copolymer resin, conductive carbon black, conductive carbon fiber powder, 0.8-1 part of antioxidant and 6-8 parts of paraffin wax are uniformly mixed to obtain a mixture, which is then conveyed to a forced feeder, and forced fed into an extruder for melt extrusion granulation at an extruder temperature of 150-160° C. After underwater pelletizing and centrifugal dehydration, the mixture enters a storage bin to obtain shielding material premixed particles; (2) The premixed particles of the shielding material in the storage bin are transported to the disc granulator, and the disc granulator is started. The dicumyl peroxide solution is sprayed under the rotation of the disc. The disc rotates for 10 to 15 minutes and then enters the drying bin. After drying for 10 to 12 hours, the disc granulator is obtained. The inclination angle of the disc granulator is 45 to 60 degrees and the rotation speed is 22 to 24 rpm.

2. The method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable according to claim 1, characterized in that: The conductive carbon fiber powder is added in an amount of 5% to 10% of the mixture mass.

3. The method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable according to claim 1, characterized in that: The conductive carbon fiber powder is added in an amount of 20% to 25% of the mixture mass.

4. The method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable according to claim 1, characterized in that: The particle size of the conductive carbon fiber powder is 400-500 meshes.

5. The method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable according to claim 1, characterized in that: The ethylene-butyl acrylate copolymer resin is one of AEB560D and R3427AC.

6. The method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable according to claim 1, characterized in that: The paraffin wax is No. 54 fully refined paraffin wax or No. 58 fully refined paraffin wax.

7. The method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable according to claim 1, characterized in that: The first step antioxidant is one or more of the antioxidant 330 , the antioxidant 300 , or the antioxidant 1010 .

8. The method for preparing a semi-conductive shielding material for a cross-linked polyethylene insulated cable according to claim 1, characterized in that: The drying temperature in step (3) is 65-75° C., and the amount of dicumyl peroxide used is 1.6%-2.4% of the mass of the premixed particles of the shielding material.