Polycarbonate resin composition

By adding specific benzotriazole-based ultraviolet absorber and phosphorus-based stabilizer to the polycarbonate resin, the problem of blocking light at wavelengths of 400 to 420 nm and reducing the generation of forming gas is solved, thus achieving high efficiency light blocking and good forming performance.

CN118931147APending Publication Date: 2024-11-12MITSUBISHI ENG PLASTICS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411188447.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-08-16
Filing Date
2017-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polycarbonate resin compositions are difficult to effectively block ultraviolet light at wavelengths of 400 to 420 nm, and at the same time, a large amount of gas is generated during the forming process, affecting product quality.

Method used

By adding a specific amount of benzotriazole-based ultraviolet absorber and a phosphorus-based stabilizer with a maximum absorption wavelength of 375 nm or more to the polycarbonate resin, combined with an appropriate amount of stabilizer, the formed composition can effectively block 400 to 420 nm from 400 nm to the polycarbonate resin, and combining with an appropriate amount of stabilizer. Light at wavelengths and reduces gas production during forming.

Benefits of technology

Effective blocking of wavelength light from 400 to 420 nm is achieved, avoiding gas generation problems during forming, while maintaining excellent mechanical properties and transparency of polycarbonate resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931147A_ABST
    Figure CN118931147A_ABST
Patent Text Reader

Abstract

The present invention relates to a polycarbonate resin composition, and provides a polycarbonate resin composition which can block ultraviolet light and light having a wavelength of 400 to 420 nm on the visible light side thereof, and does not have a gas generation problem at the time of molding. The polycarbonate resin composition is characterized by comprising, per 100 parts by mass of a polycarbonate resin (A): (i) 0.02 to 1 part by mass of a sesamol group-containing benzotriazole-based ultraviolet absorber (B1) having an absorption curve determined using the following formula in accordance with JIS K7105 and a maximum absorption wavelength of 375 nm or more; or (ii) 0.08 to 1 part by mass of a sesamol group-containing ultraviolet absorber (B2) having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the following formula in accordance with JIS K7105; and 0.01 to 0.5 parts by mass of a stabilizer (C).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application filed on September 4, 2017, with application number 201780073319.9 and invention name “Polycarbonate resin composition”. Technical Field

[0002] The present invention relates to a polycarbonate resin composition, and more particularly to a polycarbonate resin composition that can block light having a wavelength of 400 to 420 nm on the visible light side of ultraviolet light and does not cause a problem of gas generation during molding. Background Art

[0003] Eyes are often exposed to damage from sunlight, so it is important to protect the eyes from ultraviolet light with a wavelength extending to 400nm. In addition, recent studies have shown that wavelength bands close to the visible light side of ultraviolet light can also damage eye tissues and are the cause of diseases such as cataracts. In addition, as machines or lighting using LEDs as light sources become more common, blue light that is present in large quantities in LED light sources has also been reported as a cause of eye diseases.

[0004] Therefore, a material that blocks ultraviolet light and light with a wavelength of 400 to 420 nm on the visible light side thereof is required.

[0005] Generally, polycarbonate resins exhibit excellent mechanical properties, weather resistance, and transparency, and polycarbonate resin compositions incorporating ultraviolet absorbers are used as transparent ultraviolet absorbing materials such as glasses, sunglasses, goggles, various lighting covers, etc. For example, benzophenone-based, benzotriazole-based, triazine-based, salicylate-based, etc. are used as ultraviolet absorbers (e.g., Patent Documents 1 to 2).

[0006] However, there is no known polycarbonate resin composition that can actually effectively absorb and block wavelengths of 400 to 420 nm.

[0007] In addition, when the use of conventional ultraviolet absorbers such as those described above has been achieved to block light of 420 nm wavelength, a large compounding amount thereof causes a problem of large amount of gas generation at the time of molding.

[0008] Resin compositions including polycarbonate resins and such ultraviolet absorbers are known, but polycarbonate resin compositions that can effectively absorb and block wavelengths of 400 to 420 nm while having no problem of gas generation during molding are not known.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 09-291205

[0012] Patent Document 2: Japanese Patent Publication No. 06-51840 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] The present invention has been made in view of the above circumstances, and an object (problem) of the present invention is to provide a polycarbonate resin composition which can block ultraviolet light and light of 400 to 420 nm wavelength on its visible light side and has no problem of gas generation during molding.

[0015] Solutions for solving problems

[0016] As a result of extensive and intensive investigations conducted to solve the above-mentioned problems, the present inventors have found that by mixing an ultraviolet absorber having a specific maximum absorption wavelength and a phosphorus-based stabilizer in specific amounts in each case, a polycarbonate resin composition that can block light having a wavelength of 400 to 420 nm and has no problem of gas generation during molding is obtained.

[0017] The present invention relates to a polycarbonate resin composition, which comprises, relative to 100 parts by mass of a polycarbonate resin (A),

[0018] (i) 0.02 to 1 parts by mass of a benzotriazole ultraviolet absorber (B1) containing a sesamol group having a maximum absorption wavelength of 375 nm or more in an absorption curve determined using the following formula according to JIS K7105, or

[0019] (ii) 0.08 to 1 parts by mass of a sesamol group-containing benzotriazole ultraviolet absorber (B2) having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the following formula in accordance with JIS K7105; and

[0020] 0.01 to 0.5 parts by mass of a stabilizer (C).

[0021] [Absorbance of polycarbonate resin containing 0.005 mass% of ultraviolet absorber] - [Absorbance of polycarbonate resin alone]

[0022] Effects of the Invention

[0023] The polycarbonate resin composition according to the present invention can block ultraviolet light and light with a wavelength of 400 to 420 nm on its visible light side, and has no problem of gas generation during molding. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a plan view of a drop-shaped mold used for evaluating mold contamination in Examples. DETAILED DESCRIPTION

[0025] The present invention will be described in detail below using embodiments, examples and the like.

[0026] In the present specification, “to” in describing a numerical range means that the numerical values ​​described before and after “to” serving as the lower limit value and the upper limit value are included unless otherwise specified.

[0027] The present invention is as described above and constitutes a first invention, which comprises (i) 0.02 to 1 parts by mass of a sesamol group-containing benzotriazole ultraviolet absorber (B1) having a maximum absorption wavelength of 375 nm or more, and a second invention, which comprises (ii) 0.08 to 1 parts by mass of a sesamol group-containing benzotriazole ultraviolet absorber (B2) having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the following formula according to JIS K7105.

[0028] The first invention will be described first, and then the second invention will be described.

[0029] <First Invention>

[0030] Hereinafter, the first invention will be described first.

[0031] The first invention relates to a polycarbonate resin composition and a molded article described below.

[0032] [1] A polycarbonate resin composition comprising, relative to 100 parts by mass of a polycarbonate resin (A), 0.02 to 1 part by mass of an ultraviolet absorber (B1) having a maximum absorption wavelength of 375 nm or more in an absorption curve determined using the following formula in accordance with JIS K7105, and 0.01 to 0.5 part by mass of a stabilizer (C).

[0033] [Absorbance of polycarbonate resin containing 0.005 mass% of ultraviolet absorber] - [Absorbance of polycarbonate resin alone]

[0034] [2] The polycarbonate resin composition according to [1], wherein the ultraviolet absorber (B1) is a sesamol group-containing benzotriazole-based ultraviolet absorber.

[0035] [3] The polycarbonate resin composition according to [1] or [2], wherein the ultraviolet absorber (B1) is an ultraviolet absorber represented by the following general formula (1).

[0036]

[0037] (Wherein, X represents a halogen atom.)

[0038] [4] The polycarbonate resin composition according to any one of [1] to [3], further comprising, relative to 100 parts by mass of the polycarbonate resin (A), 0.01 parts by mass or more and less than 0.08 parts by mass of a sesamol group-containing benzotriazole ultraviolet absorber (B2) having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the above formula in accordance with JIS K7105.

[0039] [5] The polycarbonate resin composition according to any one of [1] to [4], further comprising, relative to 100 parts by mass of the polycarbonate resin (A), 0.01 to 0.2 parts by mass of an ultraviolet absorber (B2) having a maximum absorption wavelength of less than 360 nm in an absorption curve determined using the above formula in accordance with JIS K7105.

[0040] [6] The polycarbonate resin composition according to [5], wherein the ultraviolet absorber (B2) is at least one selected from a benzotriazole ultraviolet absorber without a sesamol group, a triazine ultraviolet absorber, a malonate ultraviolet absorber, and a benzoxazine ultraviolet absorber.

[0041] [7] The polycarbonate resin composition according to any one of [1] to [6], wherein the transmittance measured at a wavelength of 420 nm with respect to a 2 mm thick molded article in accordance with JIS K7105 is 25% or less.

[0042] [8] A molded article, which is a molded article of the polycarbonate resin composition according to any one of [1] to [7].

[0043] The components constituting the polycarbonate resin composition of the first invention are described in detail below.

[0044] [Polycarbonate resin (A)]

[0045] The polycarbonate resin is a polymer having a basic structure of a carbonate bond represented by the formula -[-OXOC(=O)-]-. X in the formula is generally a hydrocarbon, but X incorporating a heteroatom or a hetero bond may be used to impart different properties.

[0046] Polycarbonate resins can be divided into aromatic polycarbonate resins in which each carbon atom directly bonded to a carbonate bond is an aromatic carbon, and aliphatic polycarbonate resins in which each carbon atom is an aliphatic carbon atom, and either of these two types can be used. From viewpoints such as heat resistance, mechanical properties, and electrical characteristics, aromatic polycarbonate resins are preferred.

[0047] The specific type of polycarbonate resin is not limited, and examples here are polycarbonate polymers provided by reacting dihydroxy compounds with carbonate precursors. Here, in addition to dihydroxy compounds and carbonate precursors, polyhydroxy compounds and the like may also be reacted. Carbon dioxide may also be used as a method for reacting carbonate precursors with cyclic ethers. The polycarbonate polymer may be linear or branched. In addition, the polycarbonate polymer may be a homopolymer consisting of one repeating unit, or may be a copolymer having more than two repeating units. Various copolymerization modes may be selected for such copolymers such as random copolymers, block copolymers, etc. Typically, the polycarbonate polymer described herein is a thermoplastic resin.

[0048] Among the monomers serving as the raw materials of the aromatic polycarbonate resin, the aromatic dihydroxy compounds may be exemplified by the following:

[0049] Dihydroxybenzenes, such as 1,2-dihydroxybenzene, 1,3-dihydroxybenzene (i.e., resorcinol), and 1,4-dihydroxybenzene;

[0050] Dihydroxybiphenyls, such as 2,5-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, and 4,4'-dihydroxybiphenyl;

[0051] dihydroxynaphthalenes, such as 2,2'-dihydroxy-1,1'-binaphthyl, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, and 2,7-dihydroxynaphthalene;

[0052] dihydroxydiaryl ethers, such as 2,2'-dihydroxydiphenyl ether, 3,3'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 1,4-bis(3-hydroxyphenoxy)benzene, and 1,3-bis(4-hydroxyphenoxy)benzene;

[0053] Bis(hydroxyaryl)alkanes, e.g.

[0054] 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A),

[0055] 1,1-Bis(4-hydroxyphenyl)propane,

[0056] 2,2-Bis(3-methyl-4-hydroxyphenyl)propane,

[0057] 2,2-bis(3-methoxy-4-hydroxyphenyl)propane, 2-(4-hydroxyphenyl)-2-(3-methoxy-4-hydroxyphenyl)propane, 1,1-bis(3-tert-butyl-4-hydroxyphenyl)propane,

[0058] 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane,

[0059] 2,2-Bis(3-cyclohexyl-4-hydroxyphenyl)propane,

[0060] 2-(4-hydroxyphenyl)-2-(3-cyclohexyl-4-hydroxyphenyl)propane, α,α′-bis(4-hydroxyphenyl)-1,4-diisopropylbenzene, 1,3-bis[2-(4-hydroxyphenyl)-2-propyl]benzene, bis(4-hydroxyphenyl)methane,

[0061] Bis(4-hydroxyphenyl)cyclohexylmethane, bis(4-hydroxyphenyl)phenylmethane, bis(4-hydroxyphenyl)(4-propenylphenyl)methane, bis(4-hydroxyphenyl)diphenylmethane, bis(4-hydroxyphenyl)naphthylmethane,

[0062] 1,1-Bis(4-hydroxyphenyl)ethane,

[0063] 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)-1-naphthylethane,

[0064] 1,1-Bis(4-hydroxyphenyl)butane,

[0065] 2,2-Bis(4-hydroxyphenyl)butane,

[0066] 2,2-Bis(4-hydroxyphenyl)pentane,

[0067] 1,1-Bis(4-hydroxyphenyl)hexane,

[0068] 2,2-Bis(4-hydroxyphenyl)hexane,

[0069] 1,1-Bis(4-hydroxyphenyl)octane,

[0070] 2,2-Bis(4-hydroxyphenyl)octane,

[0071] 4,4-Bis(4-hydroxyphenyl)heptane,

[0072] 2,2-Bis(4-hydroxyphenyl)nonane,

[0073] 1,1-bis(4-hydroxyphenyl)decane, and

[0074] 1,1-Bis(4-hydroxyphenyl)dodecane;

[0075] Bis(hydroxyaryl)cycloalkanes, e.g.

[0076] 1,1-Bis(4-hydroxyphenyl)cyclopentane,

[0077] 1,1-Bis(4-hydroxyphenyl)cyclohexane,

[0078] 1,1-bis(4-hydroxyphenyl)-3,3-dimethylcyclohexane,

[0079] 1,1-bis(4-hydroxyphenyl)-3,4-dimethylcyclohexane,

[0080] 1,1-bis(4-hydroxyphenyl)-3,5-dimethylcyclohexane,

[0081] 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane,

[0082] 1,1-bis(4-hydroxy-3,5-dimethylphenyl)-3,3,5-trimethylcyclohexane,

[0083] 1,1-Bis(4-hydroxyphenyl)-3-propyl-5-methylcyclohexane,

[0084] 1,1-bis(4-hydroxyphenyl)-3-tert-butylcyclohexane,

[0085] 1,1-bis(4-hydroxyphenyl)-4-tert-butylcyclohexane,

[0086] 1,1-bis(4-hydroxyphenyl)-3-phenylcyclohexane, and

[0087] 1,1-Bis(4-hydroxyphenyl)-4-phenylcyclohexane;

[0088] Cardo-containing bisphenols, such as 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene;

[0089] Dihydroxydiaryl sulfides, such as 4,4'-dihydroxydiphenyl sulfide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide;

[0090] Dihydroxydiaryl sulfoxides, such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; and

[0091] Dihydroxydiaryl sulfones, for example 4,4'-dihydroxydiphenyl sulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone.

[0092] Among the above, bis(hydroxyaryl)alkanes are preferred, bis(4-hydroxyphenyl)alkanes are preferred, and 2,2-bis(4-hydroxyphenyl)propane (ie, bisphenol A) is particularly preferred from the viewpoint of impact resistance and heat resistance.

[0093] One kind of the aromatic dihydroxy compound may be used, or any combination of two or more kinds in any ratio may be used.

[0094] The monomers included as raw materials of the aliphatic polycarbonate resin can be exemplified by the following:

[0095] Alkanediols, such as ethane-1,2-diol, propane-1,2-diol, propane-1,3-diol, 2,2-dimethylpropane-1,3-diol, 2-methyl-2-propylpropane-1,3-diol, butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol, and decane-1,10-diol;

[0096] Cycloalkane diols, such as cyclopentane-1,2-diol, cyclohexane-1,2-diol, cyclohexane-1,4-diol, 1,4-cyclohexanedimethanol, 4-(2-hydroxyethyl)cyclohexanol, and 2,2,4,4-tetramethylcyclobutane-1,3-diol;

[0097] diols, such as ethylene glycol, 2,2'-oxydiethanol (ie, diethylene glycol), triethylene glycol, propylene glycol, and spiro glycol;

[0098] Aralkyl diols, such as 1,2-benzenedimethanol, 1,3-benzenedimethanol, 1,4-benzenedimethanol, 1,4-benzenediethanol, 1,3-bis(2-hydroxyethoxy)benzene, 1,4-bis(2-hydroxyethoxy)benzene, 2,3-bis(hydroxymethyl)naphthalene, 1,6-bis(hydroxyethyl)naphthalene, 4,4'-biphenyl dimethanol, 4,4'-biphenyl diethanol, 1,4-bis(2-hydroxyethoxy)biphenyl, bisphenol A bis(2-hydroxyethyl) ether; and bisphenol S bis(2-hydroxyethyl) ether; and

[0099] Cyclic ethers such as 1,2-ethylene oxide (ie, ethylene oxide), 1,2-propylene oxide (ie, propylene oxide), 1,2-epoxycyclopentane, 1,2-epoxycyclohexane, 1,4-epoxycyclohexane, 1-methyl-1,2-epoxycyclohexane, 2,3-epoxynorbornane, and 1,3-epoxypropylene.

[0100] Among the monomers included as the raw material of the polycarbonate resin, the carbonate precursor can be exemplified by carbonyl halides and carbonate esters. One carbonate precursor may be used, or any combination of two or more in any ratio may be used.

[0101] The carbonyl halide can be specifically exemplified by phosgene; and haloformates of dihydroxy compounds and monochloroformates of dihydroxy compounds.

[0102] The carbonate esters can be specifically exemplified by diaryl carbonates such as diphenyl carbonate and ditolyl carbonate; dialkyl carbonates such as dimethyl carbonate and diethyl carbonate; and carbonates of dihydroxy compounds such as dicarbonates of dihydroxy compounds, monocarbonates of dihydroxy compounds, and cyclic carbonates.

[0103] There is no particular limitation on the method for producing the polycarbonate resin, and any method may be used. Examples thereof are interfacial polymerization, melt transesterification, pyridine method, ring-opening polymerization of cyclic carbonate compounds, and solid phase transesterification of prepolymers.

[0104] The molecular weight of the polycarbonate resin (A), expressed as a viscosity average molecular weight (Mv), is preferably in the range of 16,000 to 50,000 and is more preferably 18,000 or more and still more preferably 20,000 or more and still more preferably 45,000 or less, still more preferably 40,000 or less, and particularly preferably 38,000 or less. A viscosity average molecular weight of less than 16,000 contributes to a decrease in the impact resistance of the molded article and causes a risk of cracking, and is therefore unsuitable. A viscosity average molecular weight of more than 50,000 results in poor fluidity and contributes to problems in formability, and is therefore also unsuitable.

[0105] A mixture of two or more polycarbonate resins having different viscosity average molecular weights may be used for the polycarbonate resin (A), and in this case, a polycarbonate resin having a viscosity average molecular weight outside the above preferred range may be mixed.

[0106] In the present invention, the viscosity average molecular weight [Mv] of the polycarbonate resin refers to the viscosity average molecular weight of the polycarbonate resin using the Schnell viscosity equation, i.e., η = 1.23 × 10 -4 Mv 0.83 The value calculated is a value in which the intrinsic viscosity [η] (unit: dl / g) at 20° C. is measured using dichloromethane as a solvent and an Ubbelohde viscometer. The intrinsic viscosity [η] is a value calculated using the following formula and the specific viscosity [ηsp] measured at each solution concentration [C] (g / dl).

[0107]

[0108] In addition, the present invention may use a combination of polycarbonate resin and other thermoplastic resins. In addition, a copolymer with polycarbonate resin as the main part may be constructed, for example, a copolymer of polycarbonate resin and oligomer or polymer containing siloxane structure for the purpose of further improving flame retardancy and impact resistance; a copolymer of polycarbonate resin and monomer, oligomer, or polymer containing phosphorus atom for the purpose of further improving thermal oxidation stability and flame retardancy; a copolymer of polycarbonate resin and monomer, oligomer, or polymer containing dihydroxyanthraquinone structure for the purpose of improving thermal oxidation stability; a copolymer of polycarbonate resin and oligomer or polymer having olefinic structure such as polystyrene for the purpose of improving optical properties; or a copolymer of polycarbonate resin and polyester resin oligomer or polymer for the purpose of enhancing drug resistance.

[0109] In addition, in order to obtain an improved appearance of the molded product and improve fluidity, the polycarbonate resin may contain a polycarbonate oligomer. The viscosity average molecular weight (Mv) of the polycarbonate oligomer is generally 1500 or more, preferably 2000 or more, and generally 9500 or less, preferably 9000 or less. The incorporated polycarbonate oligomer is preferably 30% by mass or less of the polycarbonate resin (including the polycarbonate oligomer).

[0110] The polycarbonate resin may be a raw material in a virgin state, but may also be a polycarbonate resin recycled from post-consumer products (also referred to as recycled polycarbonate resin).

[0111] However, the recycled polycarbonate resin is preferably 80% by mass or less of the polycarbonate resin, and more preferably 50% by mass or less. Since the recycled polycarbonate resin has a high possibility of degradation such as thermal degradation, aging degradation, etc., the use of such polycarbonate resin in an amount larger than the specified range may result in a decrease in hue and mechanical properties.

[0112] [Ultraviolet light absorber (B1)]

[0113] The polycarbonate resin composition according to the first invention contains an ultraviolet absorber (B1) having an absorption curve determined using the following formula (1) according to JIS K7105 with a maximum absorption wavelength of 375 nm or more.

[0114] [Absorbance of polycarbonate resin containing 0.005 mass% of ultraviolet absorber] - [Absorbance of polycarbonate resin alone] (1)

[0115] In the present invention, the maximum absorption wavelength of the ultraviolet absorber (B1) is defined as the maximum absorption wavelength of the absorption curve obtained by subtracting the absorbance of a flat plate-shaped molded product of the same shape and thickness of the same polycarbonate resin not containing the ultraviolet absorber from the absorbance of a flat plate-shaped molded product of a polycarbonate resin containing 0.005% by mass of the ultraviolet absorber according to formula (1). It is considered that the maximum absorption wavelength thus defined does not change as a function of the thickness of the flat plate test piece used in principle, but in the present invention, it is preferred to compare at a thickness of 2 mm.

[0116] The same definition applies also to the maximum absorption wavelength of the ultraviolet absorbers (B2) and (B3) described below.

[0117] The specific conditions of the measurement and determination method of the maximum absorption wavelength are described in detail in the Examples.

[0118] The maximum absorption wavelength of the ultraviolet absorber (B1) is 375 nm or more, and the upper limit of the maximum absorption wavelength is preferably 420 nm or less and more preferably 400 nm or less.

[0119] Although the ultraviolet absorber (B1) can be selected from, for example, benzotriazole-based compounds, benzophenone-based compounds, triazine-based compounds, benzoate-based compounds, phenyl salicylate-based compounds, cyanoacrylate-based compounds, malonate-based compounds, and oxalic acid anilide-based compounds, etc., which have a maximum absorption wavelength of 375 nm or more in each case, a benzotriazole-based ultraviolet absorber is preferred, a benzotriazole-based ultraviolet absorber containing a sesamol group (benzo[1,3]dioxol-5-ol group) is more preferred, and an ultraviolet absorber represented by the following general formula (1) is particularly preferred.

[0120]

[0121] In the general formula (1), X is a halogen atom and is preferably a halogen atom such as chlorine, bromine, fluorine or iodine, more preferably a chlorine atom, and thus 6-(5-chloro-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol is particularly preferred.

[0122] Relative to 100 parts by mass of polycarbonate resin (A), the content of ultraviolet absorber (B1) is 0.02 to 1 part by mass. When the content is less than 0.02 parts by mass, the transmittance of the obtained resin composition in the wavelength domain of 400 to 420nm is too high. When the content exceeds 1 part by mass, the transmittance in the wavelength domain of 400 to 420nm is low, but the gas generation problem during molding becomes significant and volatiles are attached to the molded product and significantly damage the product appearance. Relative to 100 parts by mass of polycarbonate resin (A), the content of ultraviolet absorber (B1) is preferably more than 0.025 parts by mass, less than 0.8 parts by mass, more preferably less than 0.7 parts by mass, and still more preferably less than 0.6 parts by mass.

[0123] [Ultraviolet light absorber (B2)]

[0124] The polycarbonate resin composition according to the present invention preferably further contains a sesamol group-containing benzotriazole ultraviolet absorber (B2) having an absorption curve determined by formula (1) according to JIS K7105 with a maximum absorption wavelength of 360 nm or more and less than 375 nm.

[0125] Incorporation of the ultraviolet absorber (B2) makes it possible to improve the tendency that the transmittance near 320 nm tends to increase when the content of the ultraviolet absorber (B1) is relatively small.

[0126] The sesamol group-containing benzotriazole ultraviolet absorber (B2) having an absorption curve determined by formula (1) according to JIS K7105 and having a maximum absorption wavelength of 360 nm or more and less than 375 nm is preferably an ultraviolet absorber represented by the following general formula (2).

[0127]

[0128] (In the general formula (2), R represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a hydroxyl group, a carboxyl group, an alkoxycarbonyl group having 1 to 8 carbon atoms in the alkyl group, a hydroxyalkyl group having 1 to 8 carbon atoms, or an alkylcarbonyloxyalkyl group having 1 to 8 carbon atoms in each alkyl group.)

[0129] R in the general formula (2) can be specifically exemplified by the following: a hydrogen atom; an optionally substituted straight-chain or branched alkyl group having 1 to 8 carbon atoms, for example, a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-hexyl group, an n-octyl group, and a 2-ethylhexyl group; an optionally substituted straight-chain or branched alkoxy group having 1 to 8 carbon atoms, for example, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an n-hexyl group, an n-octyl group, and a 2-ethylhexyl group; a hydroxyl group; a carboxyl group; an optionally substituted straight-chain or branched alkoxycarbonyl group having 1 to 8 carbon atoms in the alkyl group, for example, a methoxycarbonyl group, an ethoxycarbonyl group, an isopropoxycarbonyl group, an n-butoxycarbonyl group, an isobutoxycarbonyl group, a sec-butoxycarbonyl group carbonyl, tert-butoxycarbonyl, n-hexyloxycarbonyl, n-octyloxycarbonyl, and 2-ethylhexyloxycarbonyl; optionally substituted straight or branched hydroxyalkyl groups having 1 to 8 carbon atoms, for example, hydroxymethyl, hydroxyethyl, hydroxypropyl, hydroxybutyl, hydroxyhexyl, and hydroxyoctyl; and optionally substituted straight or branched alkylcarbonyloxyalkyl groups having 1 to 8 carbon atoms in each alkyl group, for example, methylcarbonyloxymethyl, ethylcarbonyloxymethyl, propylcarbonyloxymethyl, butylcarbonyloxymethyl, hexylcarbonyloxymethyl, heptylcarbonyloxymethyl, octylcarbonyloxymethyl, methylcarbonyloxyethyl, ethylcarbonyloxyethyl, propylcarbonyloxyethyl, butylcarbonyloxyethyl, hexylcarbonyloxyethyl, heptylcarbonyloxyethyl, and octylcarbonyloxyethyl.

[0130] Preferred among the aforementioned R are hydrogen atom, alkyl group, alkoxy group, hydroxyl group, carboxyl group, alkoxycarbonyl group, hydroxyalkyl group, and alkylcarbonyloxyalkyl group. More preferred are hydrogen atom, methyl group, methoxy group, n-octyloxy group, hydroxyl group, carboxyl group, methoxycarbonyl group, n-octyloxycarbonyl group, hydroxyethyl group, methylcarbonyloxyethyl group, and heptylcarbonyloxyethyl group.

[0131] The following are preferred examples of the compound represented by the general formula (2) and having a maximum absorption wavelength of 360 nm or more and less than 375 nm: 6-(2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-n-heptylcarbonyloxyethyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-isoheptylcarbonyloxyethyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-methyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-methoxy-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, oxol-5-ol, 6-(5-hydroxyethyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-octyloxy-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-carboxy-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-hydroxyethyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, and 6-(5-methylcarbonyloxyethyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol.

[0132] Among the above, 6-(2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, 6-(5-n-heptylcarbonyloxyethyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol, and 6-(5-isoheptylcarbonyloxyethyl-2H-benzotriazol-2-yl)benzo[1,3]dioxol-5-ol are particularly preferred.

[0133] The preferred content of the ultraviolet absorber (B2) is 0.01 parts by mass or more and less than 0.08 parts by mass relative to 100 parts by mass of the polycarbonate resin (A). When it is less than 0.01 parts by mass, the resulting resin composition is easily permeable near a wavelength of 320 nm. When it is more than 0.08 parts by mass, gas generation during molding is promoted and the product appearance is easily damaged. The content of the ultraviolet absorber (B2) is more preferably 0.02 parts by mass or more, still more preferably 0.03 parts by mass or more, and more preferably 0.07 parts by mass or less, still more preferably 0.05 parts by mass or less, and particularly preferably 0.04 parts by mass or less relative to 100 parts by mass of the polycarbonate resin (A).

[0134] [Ultraviolet light absorber (B3)]

[0135] The polycarbonate resin composition according to the first invention preferably further contains an ultraviolet absorber (B3) having a maximum absorption wavelength of less than 360 nm in the absorption curve determined by formula (1) according to JIS K7105.

[0136] Incorporation of the ultraviolet absorber (B3) makes it possible to improve the tendency that the transmittance near 320 nm tends to increase when the content of the ultraviolet absorber (B1) is relatively small.

[0137] The ultraviolet absorber (B3) can be exemplified by benzotriazole compounds, benzophenone compounds, triazine compounds, benzoxazine compounds, benzoate compounds, phenyl salicylate compounds, cyanoacrylate compounds, malonate compounds, and oxalic acid anilide compounds. Preferred among the above are benzotriazole compounds, triazine compounds, malonate compounds, and benzoxazine compounds. One or more of these can be used.

[0138] Examples of the hydroxybenzophenone-based compound include 2-hydroxy-4-octyloxybenzophenone.

[0139] Examples of the malonate-based compound include dimethyl (p-methoxybenzylidene) malonate, 2-(1-arylalkylidene) malonate, and tetraethyl 2,2′-(1,4-phenylenedimethylene (dimethylidene)) bismalonate.

[0140] Examples of the triazine compound include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]phenol.

[0141] Examples of the benzoate-based compound include 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate.

[0142] Examples of the benzoxazine-based compound include 2,2′-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one).

[0143] The ultraviolet absorber (B3) is more preferably a benzotriazole ultraviolet absorber and particularly preferably a benzotriazole compound having no sesamol group. The following are preferred specific examples of such benzotriazole compounds: 2-(2-hydroxy-5-tert-octylphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole, 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol, 2,4-di-tert-butyl-6-(5-chlorobenzotriazol-2-yl)phenol, (2-[5-chloro(2H)-benzotriazol-2-yl]-4,6- di(tert-amyl)phenol), 3-[3-tert-butyl-5-(5-chloro-2H-benzotriazol-2-yl)-4-hydroxyphenyl]octyl propionate, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol, 2-(2H-benzotriazol-2-yl)-p-cresol, 2-[(2H)-benzotriazol-2-yl]-4,6-di(1-methyl-1-phenylethyl)phenol.

[0144] The preferred content of the ultraviolet absorber (B3) is 0.01 to 0.02 parts by mass relative to 100 parts by mass of the polycarbonate resin (A). When it is less than 0.01 parts by mass, the resulting resin composition is easily permeable near a wavelength of 320 nm. When it exceeds 0.2 parts by mass, gas generation during molding is promoted and the product appearance is easily damaged. The content of the ultraviolet absorber (B3) is more preferably 0.02 parts by mass or more, still more preferably 0.03 parts by mass or more, and more preferably 0.15 parts by mass or less relative to 100 parts by mass of the polycarbonate resin (A).

[0145] [Stabilizer (C)]

[0146] The polycarbonate resin composition according to the first invention contains a stabilizer (C). Examples of the stabilizer (C) include a phosphorus stabilizer, a phenol stabilizer, a sulfur stabilizer, etc. The polycarbonate resin composition according to the second invention also contains a stabilizer (C), and its type, content, etc. are the same as those in the first invention. The following description also applies to the stabilizer (C) in the second invention.

[0147] [Phosphorus stabilizer]

[0148] By incorporating a phosphorus-based stabilizer in the polycarbonate resin composition according to the present invention, the polycarbonate resin composition has a good hue and exhibits additional improvement in its resistance to thermal discoloration.

[0149] Any known phosphorus stabilizer can be used as the phosphorus stabilizer herein. Specific examples are phosphorus oxyacids such as phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid, and polyphosphoric acid; acidic pyrophosphate metal salts such as acidic sodium pyrophosphate, acidic potassium pyrophosphate, and acidic calcium pyrophosphate; phosphates of Group 1 or 2B metals such as potassium phosphate, sodium phosphate, cesium phosphate, and zinc phosphate; phosphate ester compounds; phosphite compounds; and phosphonite compounds, and phosphite compounds are particularly preferred. By selecting the phosphite compound, a polycarbonate resin composition exhibiting higher resistance to discoloration and better continuous productivity can be obtained.

[0150] The phosphite compound is a trivalent phosphorus compound represented by the general formula P(OR)3, wherein R represents a monovalent or divalent organic group.

[0151] The phosphite compound is exemplified by triphenyl phosphite, tris(monononylphenyl)phosphite, tris(nonyl / dinonyl-phenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, monooctyl diphenyl phosphite, dioctyl monophenyl phosphite, monodecyl diphenyl phosphite, didecyl monophenyl phosphite, tridecyl phosphite, trilauryl phosphite, tristearyl phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butyl-4-methylphenyl)phosphite, ) pentaerythritol phosphite, bis(2,6-di-tert-butylphenyl)octyl phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphite, and 6-[3-(3-tert-butyl-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphepine.

[0152] Among these phosphite compounds, aromatic phosphite compounds represented by the following general formulae (3) and (4) are more preferred because they are effective in increasing the heat discoloration resistance exhibited by the polycarbonate resin composition according to the present invention.

[0153]

[0154] (Where R 1 , R 2 , and R 3 Each independently represents an aryl group having 6 to 30 carbon atoms. )

[0155]

[0156] (Where R 4 and R 5 Each independently represents an aryl group having 6 to 30 carbon atoms. )

[0157] Among the phosphite compounds represented by formula (3), triphenyl phosphite, tris(monononylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite and the like are preferred, and tris(2,4-di-tert-butylphenyl)phosphite is more preferred.

[0158] Among the phosphite compounds represented by formula (4), those having a pentaerythritol diphosphite structure are particularly preferred, such as bis(2,4-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, and bis(2,4-dicumylphenyl)pentaerythritol diphosphite.

[0159] Among these phosphite compounds, the aromatic phosphite compound represented by formula (4) provides even better hue and is therefore more preferred.

[0160] A single phosphorus-based stabilizer may be incorporated or any combination of two or more phosphorus-based stabilizers in any ratio may be incorporated.

[0161] The content of the phosphorus stabilizer is 0.01 to 0.5 parts by mass, preferably 0.02 parts by mass or more, more preferably 0.03 parts by mass or more, and preferably 0.4 parts by mass or less, more preferably 0.3 parts by mass or less, and still more preferably 0.2 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A). When the phosphorus stabilizer content is less than 0.005 parts by mass, the hue and heat discoloration resistance are insufficient. When it exceeds 0.5 parts by mass, the heat discoloration resistance actually deteriorates and the wet heat stability is also reduced.

[0162] [Phenolic stabilizer]

[0163] The polycarbonate resin composition according to the present invention may contain a phenolic stabilizer as a stabilizer. Hindered phenolic oxidation inhibitors are examples of phenolic stabilizers. Specific examples thereof are pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N′-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 3,3′,3″,5,5′,5″-hexa-tert-butyl-α,α′,α″-(mesitylene-2,4, 6-triyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazine-2-ylamino)phenol, and 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenylacrylate.

[0164] Among the above, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Specific examples of these phenolic oxidation inhibitors include "Irganox 1010" and "Irganox 1076" from BASF and "ADK STAB AO-50" and "ADK STAB AO-60" from ADEKA.

[0165] A single phenolic stabilizer may be incorporated or any combination of two or more in any ratio may be incorporated.

[0166] The content of the phenolic stabilizer is 0.01 to 0.5 parts by mass, preferably 0.02 parts by mass or more, more preferably 0.03 parts by mass or more, and preferably 0.4 parts by mass or less, more preferably 0.3 parts by mass or less, and still more preferably 0.2 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A). When the content of the phenolic stabilizer is less than the lower limit of the specified range, the effect as a phenolic stabilizer may be insufficient. When the content of the phenolic stabilizer exceeds the upper limit of the specified range, the effect reaches a peak, so it may be uneconomical.

[0167] The phosphorus stabilizer may be used in combination with a phenol stabilizer. In this case, the total content of the phosphorus stabilizer and the phenol stabilizer is 0.01 to 0.5 parts by mass, preferably 0.02 parts by mass or more, more preferably 0.03 parts by mass or more, and preferably 0.4 parts by mass or less, more preferably 0.3 parts by mass or less, and still more preferably 0.2 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A).

[0168] [Sulfur stabilizer]

[0169] Sulfur-based stabilizers may be exemplified by dilauryl 3,3'-thiodipropionate, ditridecyl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, dodecyl stearoyl 3,3'-thiodipropionate, pentaerythritol tetrakis(3-laurylthiopropionate), bis[2-methyl-4-(3-laurylthiopropionyl oxy)-5-tert-butylphenyl]sulfide, octadecyl disulfide, mercaptobenzimidazole, 2-mercapto-6-methylbenzimidazole, and 1,1'-thiobis(2-naphthol).

[0170] Among the above, pentaerythritol tetrakis (3-laurylthiopropionate) is preferred. This sulfur-based stabilizer can be exemplified by "ADK STAB AO-412S" from ADEKA Corporation.

[0171] The content of the sulfur-based stabilizer is 0.01 to 0.5 parts by mass, preferably 0.02 parts by mass or more, more preferably 0.03 parts by mass or more, and preferably 0.4 parts by mass or less, more preferably 0.3 parts by mass or less, still more preferably 0.2 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A). When the content of the sulfur-based stabilizer is less than the lower limit of the specified range, the effect as a sulfur-based stabilizer will be insufficient. When the content of the sulfur-based stabilizer exceeds the upper limit of the specified range, the effect reaches a peak, so it will be uneconomical.

[0172] [additive]

[0173] The polycarbonate resin composition according to the first invention may contain additives other than those described above, such as release agents, fluorescent whitening agents, pigments, dyes, flame retardants, impact-resistant reinforcing agents, antistatic agents, plasticizers, compatibilizers, and the like, and may contain polymers other than polycarbonate resins. One of these additives may be incorporated or two or more of these additives may be incorporated, and one other resin or two or more other resins may be incorporated. The polycarbonate resin composition according to the second invention may also contain additives other than those described above, and their types, contents, etc. are the same as those of the first invention.

[0174] <Second Invention>

[0175] Next, the second invention will be described.

[0176] The second invention relates to a polycarbonate resin composition and a molded article described below.

[0177] [1] A polycarbonate resin comprising 0.08 to 1 parts by mass of an ultraviolet absorber (B2) having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the following formula according to JIS K7105, and 0.01 to 0.5 parts by mass of a stabilizer (C), relative to 100 parts by mass of a polycarbonate resin (A).

[0178] [Absorbance of polycarbonate resin containing 0.005 mass% of ultraviolet absorber] – [Absorbance of polycarbonate resin alone]

[0179] [2] The polycarbonate resin composition according to [1], wherein the ultraviolet absorber (B2) is a sesamol group-containing benzotriazole-based ultraviolet absorber.

[0180] [3] The polycarbonate resin composition according to [1] or [2], wherein the ultraviolet absorber (B2) is an ultraviolet absorber represented by the following general formula (2).

[0181]

[0182] (In the formula, R represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a hydroxyl group, a carboxyl group, an alkoxycarbonyl group having 1 to 8 carbon atoms in the alkyl group, a hydroxyalkyl group having 1 to 8 carbon atoms, or an alkylcarbonyloxyalkyl group having 1 to 8 carbon atoms in each alkyl group.)

[0183] [4] The polycarbonate resin composition according to any one of [1] to [3], further comprising, relative to 100 parts by mass of the polycarbonate resin (A), 0.01 to 0.2 parts by mass of an ultraviolet absorber (B3) having a maximum absorption wavelength of less than 360 nm in an absorption curve determined using the following formula in accordance with JIS K7105.

[0184] [5] The polycarbonate resin composition according to [4], wherein the ultraviolet absorber (B3) is at least one selected from a benzotriazole ultraviolet absorber without a sesamol group, a triazine ultraviolet absorber, a malonate ultraviolet absorber, and a benzoxazine ultraviolet absorber.

[0185] [6] The polycarbonate resin composition according to any one of [1] to [5], wherein the transmittance measured at a wavelength of 420 nm with respect to a 2 mm thick molded article in accordance with JIS K7105 is 25% or less.

[0186] [7] A molded article of the polycarbonate resin composition according to any one of [1] to [6].

[0187] The components themselves used in the polycarbonate resin composition according to the second invention are substantially the same as those described in the first invention of the present invention, and, unless otherwise specifically stated, the description of the first invention provided above directly applies to the components themselves used in the second invention.

[0188] [Polycarbonate resin (A)]

[0189] The polycarbonate resin (A) is as described above, and the same description also applies to the polycarbonate resin (A) according to the second invention.

[0190] [Ultraviolet light absorber (B2)]

[0191] The polycarbonate resin composition according to the second invention contains an ultraviolet absorber (B2) having an absorption curve determined using the following formula (1) according to JIS K7105 with a maximum absorption wavelength of 360 nm or more and less than 375 nm.

[0192] [Absorbance of polycarbonate resin containing 0.005 mass% of ultraviolet absorber] – [Absorbance of polycarbonate resin alone]···(1)

[0193] The ultraviolet absorber (B2) is as described above, and the same description also applies to the ultraviolet absorber (B2) according to the second invention.

[0194] The content of ultraviolet light absorber (B2) is 0.08 to 1 mass part relative to 100 mass parts of polycarbonate resin (A). When the content is less than 0.08 mass part, the transmittance of the obtained resin composition in 400 to 420nm wavelength domain is too high. When the content exceeds 1 mass part, the transmittance in 400 to 420nm wavelength domain is low, but the gas generation problem during molding becomes significant and volatiles are attached to the molded product and significantly damage the product appearance. The content of ultraviolet light absorber (B2) is preferably 0.08 to 0.9 mass part, more preferably 0.08 to 0.8 mass part, still more preferably 0.08 to 0.7 mass part, and particularly preferably 0.08 to 0.6 mass part relative to 100 mass parts of polycarbonate resin (A).

[0195] [Ultraviolet light absorber (B3)]

[0196] The polycarbonate resin composition according to the second invention preferably further contains an ultraviolet absorber (B3) having an absorption curve determined by formula (1) according to JIS K7105 and a maximum absorption wavelength of less than 360 nm.

[0197] Incorporation of the ultraviolet absorber (B3) makes it possible to improve the tendency that the transmittance near 320 nm tends to increase when the content of the ultraviolet absorber (B2) is relatively small.

[0198] Regarding the ultraviolet absorber (B3), the explanations for the ultraviolet absorber (B3) of the first invention also apply to the ultraviolet absorber (B3) of the second invention.

[0199] The content of the ultraviolet absorber (B3) is 0.01 to 0.2 parts by mass relative to 100 parts by mass of the polycarbonate resin (A). When it is less than 0.01 parts by mass, the resulting resin composition is easily permeable at a wavelength of about 320 nm. When it exceeds 0.2 parts by mass, gas generation during molding is promoted and the product appearance is easily damaged. The content of the ultraviolet absorber (B3) is more preferably 0.02 parts by mass or more, still more preferably 0.03 parts by mass or more, and more preferably 0.15 parts by mass or less relative to 100 parts by mass of the polycarbonate resin (A).

[0200] [Stabilizer (C)]

[0201] The polycarbonate resin composition according to the second invention contains a stabilizer (C). Examples of the stabilizer (C) include a phosphorus stabilizer, a phenol stabilizer, and a sulfur stabilizer.

[0202] The kind, content, etc. of the stabilizer (C) used in the second invention are the same as those in the first invention, and the foregoing description also applies to the stabilizer (C) according to the second invention.

[0203] [additive]

[0204] The polycarbonate resin composition according to the second invention may contain additives other than those described above, such as mold release agents, antioxidants, fluorescent whitening agents, pigments, dyes, flame retardants, impact-resistant reinforcing agents, antistatic agents, plasticizers, and compatibilizers, and may contain polymers other than polycarbonate resins. One of these additives may be incorporated or two or more of these additives may be incorporated, and one other resin or two or more other resins may be incorporated.

[0205] [Method for producing polycarbonate resin composition]

[0206] The method for producing the polycarbonate resin composition according to the present invention is not limited, and a known method for producing the polycarbonate resin composition can be widely adopted. The method can be exemplified by preliminarily mixing the polycarbonate resin (A), the ultraviolet absorber (B1) or (B2), the phosphorus stabilizer (C), and other components optionally blended by using any of various mixers such as a drum mixer or a Henschel mixer, followed by melt-mixing using a mixer such as a Banbury mixer, a roller, a Brabender, a single-screw mixing extruder, a twin-screw mixing extruder, and a mixer. The temperature of the melt-mixing is not particularly limited, but is generally in the range of 240°C to 320°C.

[0207] By pelletizing the aforementioned polycarbonate resin composition and forming pellets using any of various molding methods, various molded products can be manufactured from the polycarbonate resin composition of the present invention. In addition, this method does not require a pelletizing stage, and molded products can also be manufactured by directly molding the melt-kneaded resin in an extruder.

[0208] The transmittance measured at a wavelength of 420 nm according to JIS K7105 for a 2 mm thick molded body obtained by molding the polycarbonate resin composition according to the present invention is preferably 25% or less, more preferably 10% or less, even more preferably 5% or less, and particularly preferably 1% or less. When the transmittance at a wavelength of 420 nm exceeds 25%, the effect as a material intended to block the wavelength region of 400 to 420 nm, for example, as a sunglass lens or the like is insufficient.

[0209] The molded article obtained from the polycarbonate resin composition according to the present invention exhibits excellent ability to block ultraviolet light and light of 400 to 420 nm wavelength on its visible light side; and there is no problem of gas generation during molding; and it has various excellent mechanical and thermal properties exhibited by polycarbonate resin. Therefore, it can be widely and advantageously used in applications such as sheets, films, groceries, home appliance parts, automobile parts, building materials, and hollow containers, etc., where ultraviolet radiation-induced degradation is a problem. More specifically, eyeglass lenses, sunglass lenses, goggles (for skiing), protective glasses, and protective masks, etc.; roof panels of arcades, indoor swimming pools, carports, and skylights, etc.; and signal lights, soundproof walls, side windows and rear windows of cars, solar cell housings, and street lamp covers, etc. are preferred examples.

[0210] Example

[0211] Hereinafter, the present invention will be described in more detail using examples. However, the present invention should not be construed as being limited to or restricted by the following examples.

[0212] <Examples and Comparative Examples of the First Invention>

[0213] The raw materials and evaluation methods used in the following examples and comparative examples of the first invention are as follows. [Table 1]

[0214]

[0215] With respect to the maximum absorption wavelength of the ultraviolet absorber given in Table 1, the absorbance A of the composition provided by incorporating 0.005% of the specific ultraviolet absorber into the polycarbonate resin given in Table 1 was determined. λ , and determine the absorbance A of the polycarbonate resin given in Table 1 without incorporating an ultraviolet absorber λ0 The maximum absorption wavelength is obtained by λ Subtract absorbance A λ0 The absorbance provided (A λ -A λ0 ) is obtained by the absorption curve of λ and absorbance A λ0 The measurement was performed using the method described in the following [Measurement of transmittance and absorbance].

[0216] (Examples 1 to 22, Comparative Examples 1 to 9)

[0217] [Manufacturing of resin composition pellets]

[0218] The components given in Table 1 were blended in the ratios (parts by mass) indicated in Tables 2 to 4 and mixed with a tumble mixer for 20 minutes. Then, melt kneading was performed at a barrel temperature of 280° C. by a vented single screw extruder having a screw diameter of 40 mm (“VS-40” of Tanabe Plastics Machinery Co., Ltd.), and pellets of a polycarbonate resin composition were obtained by strand cutting.

[0219] [Measurement of transmittance and absorbance]

[0220] The obtained pellets were dried at 120°C for 5 hours using a hot air circulation dryer, and then molded into stepped flat test pieces with a width of 50 mm, a length of 90 mm, and three thicknesses of 1 mm, 2 mm, and 3 mm using an injection molding machine ("SE50DUZ" from Sumitomo Heavy Industries, Ltd.) under the conditions of a resin temperature of 280°C, a mold temperature of 80°C, and a molding cycle of 30 seconds.

[0221] The transmittance and absorbance were measured on a 2 mm thick portion of a stepped flat test piece using a spectrophotometer ("UV-3100PC" by Shimadzu Corporation) in accordance with JIS K7105.

[0222] Tables 2 to 4 give the transmittances (unit: %) at 420 nm, 380 nm, and 320 nm.

[0223] [Evaluation of gas generation during molding]

[0224] The obtained pellets were dried at 120° C. for 5 hours and then molten using an injection molding machine (“SE18DUZ” from Sumitomo Heavy Industries, Ltd.) and a Figure 1 The drop-shaped mold shown was injection molded for 100 shots under the conditions of a barrel temperature of 320° C., a molding cycle of 10 seconds, and a mold temperature of 80° C. The contamination state of the white deposit generated on the metal mirror surface of the cavity side after completion was visually evaluated and scored, and gas generation during molding was evaluated by using the following criteria based on comparison with Comparative Example 2.

[0225] A: The mold deposits are extremely small compared to the state after 100 rounds of molding in Comparative Example 2, so the mold contamination resistance is very good.

[0226] B: The mold deposits were less than that in the state after 100 rounds of molding in Comparative Example 2, so the mold contamination resistance was observed to some extent.

[0227] C: The mold deposits were the same as in the state after 100 rounds of forming in Comparative Example 2, and thus mold contamination was observed.

[0228] D: The mold deposits were greater than those in the state after 100 rounds of molding in Comparative Example 2, and thus mold contamination was significantly observed.

[0229] Hereinafter, Comparative Example 2 and Comparative Example 13 according to the second invention have the same degree of mold contamination.

[0230] refer to Figure 1 The drop-shaped mold in the embodiment of the present invention is used to introduce the resin composition through the gate G, and the mold is designed to promote the collection of the generated gas in the tip area P. The gate G has a width of 1 mm and a thickness of 1 mm; Figure 1 , the width h1 is 14.5 mm, the length h2 is 7 mm, the length h3 is 27 mm, and the thickness of the formed portion is 3 mm.

[0231] Tables 2 to 4 give the results of the foregoing evaluations.

[0232] [Table 2]

[0233]

[0234] [Table 3]

[0235]

[0236] [Table 4]

[0237]

[0238] <Examples and Comparative Examples of the Second Invention>

[0239] The raw materials and evaluation methods used in the following Examples and Comparative Examples of the second invention are as follows.

[0240] [Table 5]

[0241]

[0242] With respect to the maximum absorption wavelength of the ultraviolet absorber given in Table 5, the absorbance A of the composition provided by incorporating 0.005% of the specific ultraviolet absorber into the polycarbonate resin given in Table 5 was determined. λ , and determine the absorbance A of the polycarbonate resin given in Table 5 without incorporating an ultraviolet absorber λ0 The maximum absorption wavelength is obtained by λ Subtract absorbance A λ0 The absorbance (A λ -A λ0 ) is obtained by the absorption curve of λ and absorbance Aλ0 The measurement was performed using the method described in the following [Measurement of transmittance and absorbance].

[0243] (Examples 23 to 45, Comparative Examples 10 to 21)

[0244] [Manufacturing of resin composition pellets]

[0245] The components given in Table 5 were blended in the ratios (parts by mass) shown in Table 6 and mixed with a tumble mixer for 20 minutes. Then, melt kneading was performed at a barrel temperature of 280° C. by a vented single screw extruder having a screw diameter of 40 mm (“VS-40” of Tanabe Plastics Machinery Co., Ltd.), and pellets of a polycarbonate resin composition were obtained by strand cutting.

[0246] [Measurement of transmittance and absorbance]

[0247] The obtained pellets were dried at 120°C for 5 hours using a hot air circulation dryer, and then molded into stepped flat test pieces with a width of 50 mm, a length of 90 mm, and three thicknesses of 1 mm, 2 mm, and 3 mm using an injection molding machine ("SE50DUZ" from Sumitomo Heavy Industries, Ltd.) under the conditions of a resin temperature of 280°C, a mold temperature of 80°C, and a molding cycle of 30 seconds.

[0248] The transmittance and absorbance were measured on a 2 mm thick portion of a stepped flat test piece using a spectrophotometer ("UV-3100PC" by Shimadzu Corporation) in accordance with JIS K7105.

[0249] Table 6 shows the transmittance (unit: %) at 420 nm, 380 nm, and 320 nm.

[0250] [Evaluation of gas generation during molding]

[0251] The obtained pellets were dried at 120° C. for 5 hours and then molten using an injection molding machine (“SE18DUZ” from Sumitomo Heavy Industries, Ltd.) and a Figure 1 The drop-shaped mold shown was injection molded for 100 rounds under the conditions of a barrel temperature of 320° C., a molding cycle of 10 seconds, and a mold temperature of 80° C. The contamination state of the white deposit generated on the metal mirror surface on the cavity side after completion was visually evaluated and scored, and gas generation during molding was evaluated by using the following criteria based on comparison with Comparative Example 13.

[0252] A: The mold deposits were extremely small compared to the state after 100 rounds of molding in Comparative Example 13, so the mold contamination resistance was very good.

[0253] B: The mold deposits were less than those in the state after 100 rounds of molding in Comparative Example 13, so some degree of mold contamination resistance was observed.

[0254] C: The mold deposits were the same as in the state after 100 rounds of forming in Comparative Example 13, and thus mold contamination was observed.

[0255] D: The mold deposits were greater than those in the state after 100 rounds of forming in Comparative Example 13, and thus mold contamination was significantly observed.

[0256] Hereinafter, Comparative Example 13 has the same degree of mold contamination as Comparative Example 2 according to the first invention.

[0257] refer to Figure 1 The drop-shaped mold in the embodiment of the present invention is used to introduce the resin composition through the gate G, and the mold is designed to promote the collection of the generated gas in the tip area P. The gate G has a width of 1 mm and a thickness of 1 mm; Figure 1 , the width h1 is 14.5 mm, the length h2 is 7 mm, the length h3 is 27 mm, and the thickness of the formed portion is 3 mm.

[0258] Table 6 gives the results of the aforementioned evaluation.

[0259] [Table 6]

[0260]

[0261] [Table 7]

[0262]

[0263] [Table 8]

[0264]

[0265] Industrial Applicability

[0266] The molded article obtained from the polycarbonate resin according to the present invention exhibits excellent ability to block ultraviolet light and light of 400 to 420 nm on its visible light side; has no problem of gas generation during molding; and has various excellent mechanical and thermal properties exhibited by polycarbonate resins. Therefore, it can be advantageously used in applications where ultraviolet-induced degradation is a problem and thus has high industrial applicability.

Claims

1. A polycarbonate resin composition, comprising, relative to 100 parts by mass of a polycarbonate resin (A): (i) 0.02 to 1 parts by mass of a benzotriazole ultraviolet absorber (B1) containing a sesamol group having a maximum absorption wavelength of 375 nm or more in an absorption curve determined using the following formula according to JIS K7105, or (ii) 0.08 to 1 parts by mass of a sesamol group-containing benzotriazole ultraviolet absorber (B2) having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the following formula in accordance with JIS K7105; and 0.01 to 0.5 parts by mass of a stabilizer (C), wherein the stabilizer (C) is at least one selected from the group consisting of a phosphorus stabilizer and a phenol stabilizer, wherein the phosphorus stabilizer is an aromatic phosphite compound represented by one of the following general formulas (3) and (4): In the formula, R 1 , R 2 , and R 3 each independently represents an aryl group having 6 to 30 carbon atoms, and In the formula, R 4 and R 5 each independently represents an aryl group having 6 to 30 carbon atoms, [Absorbance of polycarbonate resin containing 0.005 mass% of ultraviolet absorber] - [Absorbance of polycarbonate resin alone].

2. The polycarbonate resin composition according to claim 1, comprising, relative to 100 parts by mass of the polycarbonate resin (A), 0.02 to 1 parts by mass of a benzotriazole-based ultraviolet absorber (B1) containing a sesamol group having a maximum absorption wavelength of 375 nm or more in an absorption curve determined using the formula according to JIS K7105, and 0.01 to 0.5 parts by mass of the phosphorus-based stabilizer as the stabilizer (C).

3. The polycarbonate resin composition according to claim 1, comprising, relative to 100 parts by mass of the polycarbonate resin (A), 0.08 to 1 parts by mass of a benzotriazole-based ultraviolet absorber (B2) containing a sesamol group having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the formula according to JIS K7105, and 0.01 to 0.5 parts by mass of the phosphorus-based stabilizer as the stabilizer (C).

4. The polycarbonate resin composition according to claim 1 or 2, wherein the ultraviolet absorber (B1) is an ultraviolet absorber represented by the following formula (1): in, X represents a halogen atom.

5. The polycarbonate resin composition according to claim 2, further comprising, relative to 100 parts by mass of the polycarbonate resin (A), 0.01 parts by mass or more and less than 0.08 parts by mass of a sesamol group-containing benzotriazole ultraviolet absorber (B2) having a maximum absorption wavelength of 360 nm or more and less than 375 nm in an absorption curve determined using the formula in accordance with JIS K7105.

6. The polycarbonate resin composition according to claim 1, 3 or 5, wherein the ultraviolet absorber (B2) is an ultraviolet absorber represented by the following general formula (2): in, R represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a hydroxyl group, a carboxyl group, an alkoxycarbonyl group having 1 to 8 carbon atoms in the alkyl group, a hydroxyalkyl group having 1 to 8 carbon atoms, or an alkylcarbonyloxyalkyl group having 1 to 8 carbon atoms in each alkyl group.

7. The polycarbonate resin composition according to any one of claims 1 to 6, further comprising, relative to 100 parts by mass of the polycarbonate resin (A), 0.01 to 0.2 parts by mass of an ultraviolet absorber (B3) having a maximum absorption wavelength of less than 360 nm in an absorption curve determined using the formula according to JIS K7105.

8. The polycarbonate resin composition according to claim 7, wherein the ultraviolet absorber (B3) is at least one selected from a benzotriazole ultraviolet absorber without a sesamol group, a triazine ultraviolet absorber, a malonate ultraviolet absorber, and a benzoxazine ultraviolet absorber. 9 . The polycarbonate resin composition according to claim 1 , wherein the transmittance of the molded article having a thickness of 2 mm measured at a wavelength of 420 nm in accordance with JIS K7105 is 25% or less. 10 . A molded article, which is a molded article of the polycarbonate resin composition according to claim 1 .

Citation Information