Carbon fiber sealing gasket and preparation method thereof
Through a combination of thermoplastic matrix resin, elastomer resin, modified carbon fiber and metal powder, carbon fiber sealing gaskets that are resistant to high temperature, high pressure and acid and alkali are prepared, which solves the problem that existing sealing gaskets are under high temperature, high pressure and acid and alkali environments. The corrosion problem improves the sealing performance and service life.
Patent Information
- Application Number
- CN202410971229.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
Existing sealing gaskets are prone to corrosion in high temperature, high pressure and acid-base media environments, resulting in a degradation of sealing performance, and high processing accuracy and operation complexity, making it difficult to meet the needs of high-temperature and high-pressure containers.
Using a combination of thermoplastic matrix resin, thermoplastic elastomer resin, modified carbon fiber and metal powder, carbon fiber sealing gaskets are prepared through hot pressing molding process to improve their friction resistance, high temperature resistance, acid and alkali resistance, and through modified carbon fiber and The coordinated action of metal powder enhances the mechanical properties of the sealing gasket.
The sealing gasket is achieved for a long time and stable operation in high temperature and high pressure environment, which significantly improves its friction resistance and mechanical properties, extends its service life, and reduces the risk of corrosion.
Smart Images

Figure BDA0004955279270000071 
Figure BDA0004955279270000081 
Figure BDA0004955279270000082
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, in particular to carbon fiber composite materials, and specifically to a carbon fiber sealing gasket and a preparation method thereof. Background Art
[0002] As pressure vessels develop towards high temperature, high pressure, large-scale and other directions, new materials and new structures of sealing gaskets continue to emerge, and the selection of sealing gaskets has received more and more attention. Sealing gaskets are very important sealing components on pressure vessels. They are of various types and forms. According to their material composition, they can be divided into three categories: non-metallic sealing gaskets, metal and non-metallic combined sealing gaskets, and metal sealing gaskets.
[0003] Non-metallic gaskets have the advantages of good softness, compressibility and low bolt load, and are widely used in ordinary equipment. However, they have disadvantages such as low strength, risk of penetration and leakage, and poor resilience. They are not suitable for use in high pressure and high temperature environments.
[0004] Metal and non-metallic sealing gaskets are combined gaskets made of metal and non-metallic materials. The sealing performance is between non-metallic gaskets and metal gaskets. They have the advantages of high strength and good resilience, and are suitable for working conditions with strict pressure and temperature. For example, the patent with publication number CN116554622 A discloses a modified polytetrafluoroethylene sealing ring and its preparation method. It uses silicon dioxide and calcium metal to modify polytetrafluoroethylene resin to prepare pressure vessel gaskets. It has good temperature resistance and pressure resistance. However, if the reaction medium in the pressure vessel is alkaline, it will corrode silicon dioxide and destroy the overall structure of the sealing gasket and reduce the sealing performance of the kettle body if it is modified with silicon dioxide.
[0005] Metal ring gaskets are commonly used in pressure vessels and are divided into octagonal gaskets and circular gaskets according to different cross-sectional shapes. The processing accuracy of metal ring gaskets is strict, the gasket specific pressure and gasket coefficient are relatively large, a large bolt preload is required, and the process operation requirements are high. In addition, metal gaskets are easily corroded by the reaction medium, resulting in problems such as loose sealing. Summary of the invention
[0006] An object of the present invention is to provide a carbon fiber sealing gasket, in particular a sealing gasket with good friction resistance, high temperature resistance, high pressure resistance, acid and alkali resistance, and suitable for pressure vessels.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A carbon fiber sealing gasket comprises the following components:
[0009] 100 parts by weight of thermoplastic matrix resin;
[0010] 10 to 30 parts by weight of thermoplastic elastomer resin;
[0011] 5-15 parts by weight of modified carbon fiber;
[0012] 5 to 15 parts by weight of metal powder.
[0013] In the above technical solution, the thermoplastic matrix resin is preferably selected from one or more of polyphenylene sulfide, polyimide, polyetheretherketone, and polysulfone. The thermoplastic matrix resin has the properties of softening when heated and hardening when cooled, and does not undergo chemical reactions, and can maintain this property no matter how many times the heating and cooling are repeated.
[0014] Further preferably, the thermoplastic matrix resin is polyetheretherketone, which has good processing properties.
[0015] In the above technical solution, the melting point of the thermoplastic matrix resin is preferably greater than 250°C, so that the sealing gasket can operate at high temperatures. The melting point is the melting temperature Tm. For crystalline polymers, it refers to the temperature at which the three-dimensional long-range ordered state of the macromolecular chain structure is transformed into a disordered viscous flow state. The melting point is tested by differential scanning calorimetry. In a nitrogen atmosphere, the sample is heated to 350°C using a programmed temperature increase method (10°C / min), and the peak value of the melting peak in the spectrum is read as the melting point.
[0016] In the above technical solution, the thermoplastic matrix resin preferably has a 1.8 MPa heat deformation temperature greater than 120°C, so that the sealing gasket can work in a high temperature and high pressure environment for a long time. The 1.8 MPa heat deformation temperature refers to the temperature at which the material changes shape during heating under a pressure of 1.8 MPa.
[0017] More preferably, the thermoplastic matrix resin has a heat deformation temperature of 1.8 MPa>140°C.
[0018] Preferably, in the above technical solution, the thermoplastic matrix resin is a powder with an average particle size of 5 to 100 μm, which can be fully and evenly mixed with the modified carbon fiber and the metal powder.
[0019] More preferably, the average particle size of the thermoplastic matrix resin is 5 to 50 μm.
[0020] In the above technical solution, the thermoplastic elastomer resin is preferably selected from thermoplastic styrene elastomers, thermoplastic polyolefin elastomers, thermoplastic polyurethane elastomers, thermoplastic polyester elastomers, thermoplastic polyamide elastomers, thermoplastic vulcanized rubbers, and organic fluorine elastomers. The thermoplastic elastomer resin is an environmentally friendly low-carbon polymer material that has the characteristics of rubber (high elasticity, compression set, etc.) and the processing characteristics of plastic (simple process).
[0021] Further preferably, the thermoplastic elastomer resin is one or both of thermoplastic polyurethane elastomer and thermoplastic polyamide elastomer, and has better toughness.
[0022] More preferably, the thermoplastic elastomer resin is a thermoplastic polyamide elastomer, which also has better temperature resistance.
[0023] In the above technical solution, the elongation at break of the thermoplastic matrix resin is preferably 100-300%, so that the sealing gasket has better toughness. The elongation at break is the ratio of the elongated length of the sample after breaking under a certain force to the original length, which can characterize the softness and elasticity of the sample. The larger the elongation at break, the better the softness and elasticity.
[0024] Preferably, in the above technical solution, the metal powder is selected from titanium dioxide powder, aluminum oxide powder, copper oxide powder, iron oxide powder, magnesium oxide powder, calcium oxide powder, copper powder, aluminum powder and iron powder, which meets the wear resistance and high temperature resistance of the sealing gasket.
[0025] Further preferably, the metal powder is titanium dioxide powder, so that the sealing gasket has better acid and alkali resistance and service life.
[0026] Preferably, in the above technical solution, the average particle size of the metal powder is 1 to 100 nm.
[0027] Another object of the present invention is to provide a method for preparing a carbon fiber sealing gasket.
[0028] In order to achieve the above object, the technical solution adopted by the present invention is:
[0029] A method for preparing a carbon fiber sealing gasket, comprising:
[0030] S1. Prepare modified carbon fiber: weigh a certain amount of carbon fiber, modifier 1, and modifier 2, mix and grind to obtain a mixed powder, heat the mixed powder to 600-1000° C., hold for 2-5 hours, cool to room temperature and grind to obtain modified carbon fiber, wherein: modifier 1 is a carbon fiber pore activator, and the mass ratio of carbon fiber to modifier 1 is 10-30:1; modifier 2 is a carbon fiber surface functional group agent, and the mass ratio of carbon fiber to modifier 2 is 3-20:1;
[0031] S2: preparing a sealing gasket: weighing a thermoplastic matrix resin, a thermoplastic elastomer resin, a modified carbon fiber and a metal powder according to a proportion, mixing and stirring, and then hot-pressing to obtain a sealing gasket.
[0032] In the above technical solution, the carbon fiber is preferably selected from carbon fiber powder, carbon fiber short fiber, carbon fiber long fiber, carbon fiber filament, and carbon fiber cloth. The carbon fiber is mainly composed of carbon element, and has properties such as high temperature resistance, friction resistance, acid and alkali resistance, etc. Since its graphite microcrystalline structure is preferentially oriented along the fiber axis, it has high strength and modulus along the fiber axis.
[0033] Further preferably, the carbon fiber is carbon fiber powder, which can be fully mixed with various components.
[0034] Still more preferably, the average particle size of the carbon fiber powder is 20-100 μm, so that it can be fully and evenly mixed with the first modifier and the second modifier.
[0035] In the above technical solution, the carbon fiber pore activator is preferably selected from one or more of potassium hydroxide, potassium carbonate, potassium bicarbonate, potassium nitrate, sodium hydroxide, sodium carbonate, sodium bicarbonate, zinc chloride, and zinc nitrate. The carbon fiber pore activator can decompose and produce a large amount of gas at high temperature, which can increase the specific surface area of the carbon fiber, so that the carbon fiber can fully contact with the matrix resin when preparing the sealing gasket, reduce the interface effect between the two, and improve the friction resistance of the sealing gasket.
[0036] Further preferably, the carbon fiber pore activator is one or both of zinc chloride and zinc nitrate, which meet the better specific surface area.
[0037] Further preferably, the mass ratio of carbon fiber to modifier one is 15 to 25:1, so as to improve the pore activation ability.
[0038] In the above technical solution, the carbon fiber surface functional group agent is preferably selected from one or more of ethylenediamine, urea, para-aminosalicylic acid, glycine, N-aminoethylpiperazine, diphenylaminourea, melamine, thiourea, thiol, phosphite, and boric acid. The carbon fiber surface functional group agent can be used to modify the carbon fiber in order to bond the matrix resin and the elastomer resin and reduce the interface effect between the carbon fiber and the resin. The modifier is a compound containing one or more of the elements N, S, P, and B.
[0039] Further preferably, the carbon fiber surface functional group agent is one or both of ethylenediamine and urea to bond the carbon fiber and the matrix resin to obtain better adhesion, facilitate adhesion of the carbon fiber and the resin, and improve the mechanical properties of the sealing gasket.
[0040] More preferably, the mass ratio of carbon fiber to modifier 2 is 7 to 15:1, so as to improve the functionalization rate.
[0041] Preferably, the heating temperature of the above technical solution is 700-900°C.
[0042] Preferably, in the above technical solution, the residence time is 3 to 4 hours.
[0043] Preferably, in the above technical scheme, in S2, the molding step includes: pre-pressing at a pressure of 3 to 8 MPa for 5 to 15 minutes; heating to 300 to 400°C for melting, and keeping warm for 1 to 5 hours; molding at a pressure of 3 to 8 MPa, and keeping the pressure for 10 to 30 minutes; obtaining a sample after cooling to room temperature, annealing at a constant temperature of 200 to 300°C for 60 to 180 minutes, and then processing it into the required sealing gasket.
[0044] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0045] The present invention enhances the mechanical properties of thermoplastic matrix resin by adding modified carbon fiber, improves the surface friction of thermoplastic matrix resin, protects thermoplastic matrix resin during the operation of sealing gasket, prolongs the working time of sealing gasket, and has better acid resistance and alkali resistance; the sealing gasket has better bonding between elastomer resin and matrix resin and carbon fiber and metal powder, and the mechanical properties of the gasket are significantly improved; under the coordinated effect of modified carbon fiber and metal powder, it has better friction resistance. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] The raw materials used in each embodiment and comparative example are as follows:
[0048]
Thermoplastic matrix resin
[0049] A1: Polyetheretherketone, 770PF produced by Changchun Jida Special Plastic Engineering Research Co., Ltd., with an average particle size of 17μm, a melting point of 325℃, and a heat deformation temperature of 145℃ at 1.8MPa.
[0050] A2: Polyetheretherketone, 330PF produced by Changchun Jida Special Plastic Engineering Research Co., Ltd., with an average particle size of 65μm, a melting point of 303℃, and a heat deformation temperature of 128℃ at 1.8MPa.
[0051]
Thermoplastic elastomer resin
[0052] B: Thermoplastic polyolefin elastomer, Pebax4033 SA01MED polyamide elastic produced by Shanghai Hongsu Plastic Chemical Co., Ltd., with an elongation at break of 230%.
[0053]
Modified carbon fiber
[0054] C1: Weigh the materials according to the mass ratio, carbon fiber with an average particle size of 35μm: zinc chloride: urea = 20:1:2, pour into the crusher, crush for 5 minutes, then pour into the mortar and grind thoroughly. Put the obtained powder into the reactor, seal the reactor body with nitrogen replacement, heat to 800℃, stay for 3h, cool to room temperature and grind again to obtain modified carbon fiber.
[0055] C2: Weigh the materials according to the mass ratio, carbon fiber with an average particle size of 145μm: zinc chloride: urea = 20:1:2, pour into the crusher, crush for 5 minutes, then pour into the mortar and grind thoroughly. Put the obtained powder into the reactor, seal the reactor body with nitrogen replacement, heat to 800℃, stay for 3h, cool to room temperature and grind again to obtain modified carbon fiber.
[0056] C3: Weigh the materials according to the mass ratio, carbon fiber with an average particle size of 35μm: zinc nitrate: urea = 20:1:2, pour into the crusher, crush for 5 minutes, then pour into the mortar and grind thoroughly. Put the obtained powder into the reactor, seal the reactor body with nitrogen replacement, heat to 800℃, stay for 3h, cool to room temperature and grind again to obtain modified carbon fiber.
[0057] C4: Weigh the materials according to the mass ratio, carbon fiber with an average particle size of 35μm: zinc chloride: ethylenediamine = 20:1:2, pour into the crusher, crush for 5 minutes, then pour into the mortar and grind thoroughly. Put the obtained powder into the reactor, seal the reactor body with nitrogen replacement, heat to 800℃, stay for 3h, cool to room temperature and grind again to obtain modified carbon fiber.
[0058] C5: Weigh the materials according to the mass ratio, carbon fiber with an average particle size of 35μm: zinc chloride: urea = 10:1:2, pour into the crusher, crush for 5 minutes, then pour into the mortar and grind thoroughly. Put the obtained powder into the reactor, seal the reactor body with nitrogen replacement, heat to 800℃, stay for 3h, cool to room temperature and grind again to obtain modified carbon fiber.
[0059] C6: Weigh the materials according to the mass ratio, carbon fiber with an average particle size of 35μm: zinc chloride: urea = 30:1:2, pour into the crusher, crush for 5 minutes, then pour into the mortar and grind thoroughly. Put the obtained powder into the reactor, seal the reactor body with nitrogen replacement, heat to 800℃, stay for 3h, cool to room temperature and grind again to obtain modified carbon fiber.
[0060]
Metal powder
[0061] D1: Titanium dioxide powder, JWN-A10 titanium dioxide powder produced by Ningbo Jiwei Nano New Material Technology Co., Ltd., with an average particle size of 3-5nm.
[0062] D2: Titanium dioxide powder, JWN-A30 titanium dioxide powder produced by Ningbo Jiwei Nano New Material Technology Co., Ltd., with an average particle size of 20-40nm.
[0063] Prepare the sealing gasket by the following method:
[0064] After weighing the raw materials according to the proportion in the formula table 1, put them into a high-speed mixer and stir them for 20 minutes. After stirring, the ingredients are hot-pressed and molded:
[0065] A mold with an outer diameter of 10 cm, an inner diameter of 9 cm, and a thickness of 0.5 cm was selected, the mold was first cleaned, and then a release agent was evenly sprayed on the mold surface, the ingredients were loaded into the mold, the mold was closed, and pre-pressed for 10 minutes, with a pressure of 5 MPa; then the ingredients and the mold were placed in a furnace for heating and melting at a temperature of 350°C for 3 hours; then the mold was put back into the flat vulcanizer for molding at a molding pressure of 5 MPa and a holding time of 30 minutes; then it was air-cooled to room temperature, and the mold was opened for sampling; finally, the prepared samples were annealed at a constant temperature of 250°C for 90 minutes; the annealed samples were machined into the required experimental bars.
[0066] The sealing gaskets were subjected to the following tests. Unless otherwise specified, all tests were conducted at 25°C. The reference standard was HG / T2579-2008. The main indicators are as follows:
[0067] 1. Hardness (Shore hardness);
[0068] 2. Tensile strength (MPa);
[0069] 3. Compression permanent deformation (300℃×22h%). The smaller the compression permanent deformation, the smaller the deformation of the sealing gasket under high temperature and high pressure, and the better the sealing performance;
[0070] 4. Hot air aging (300℃×70h), including changes in hardness, tensile strength, and fracture growth rate;
[0071] 5. Liquid resistance (300℃×70h in standard oil), including hardness change and volume change. The better the change, the better the sealing gasket's medium resistance and the longer its service life.
[0072] Table 1:
[0073]
[0074]
[0075] Table 2:
[0076]
[0077]
[0078] As shown in Table 1 and Table 2, compared with the comparative example, the sealing gasket prepared in the embodiment has better mechanical properties, better oil resistance, temperature resistance and pressure resistance, the sealing gasket prepared in the embodiment has better aging resistance and a longer service life.
[0079] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A carbon fiber sealing gasket, characterized in that: It contains the following components: 100 parts by weight of thermoplastic matrix resin; 10 to 30 parts by weight of thermoplastic elastomer resin; 5-15 parts by weight of modified carbon fiber; 5 to 15 parts by weight of metal powder.
2. The carbon fiber sealing gasket according to claim 1, characterized in that: The thermoplastic matrix resin is selected from one or more of polyphenylene sulfide, polyimide, polyetheretherketone and polysulfone.
3. The carbon fiber sealing gasket according to claim 1, characterized in that: The melting point of the thermoplastic matrix resin is greater than 250°C; and / or The thermoplastic matrix resin has a heat deformation temperature of 1.8 MPa> 120°C; and / or The thermoplastic matrix resin is powder with an average particle size of 5 to 100 μm.
4. The carbon fiber sealing gasket according to claim 1, characterized in that: The thermoplastic elastomer resin is selected from thermoplastic styrene elastomers, thermoplastic polyolefin elastomers, thermoplastic polyurethane elastomers, thermoplastic polyester elastomers, thermoplastic polyamide elastomers, thermoplastic vulcanized rubbers, and organic fluorine elastomers.
5. The carbon fiber sealing gasket according to claim 1, characterized in that: The breaking elongation of the thermoplastic matrix resin is 100-300%.
6. The carbon fiber sealing gasket according to claim 1, characterized in that: The metal powder is selected from titanium dioxide powder, aluminum oxide powder, copper oxide powder, iron oxide powder, magnesium oxide powder, calcium oxide powder, copper powder, aluminum powder and iron powder.
7. The carbon fiber sealing gasket according to claim 1, characterized in that: The average particle size of the metal powder is 1-100 nm.
8. A method for preparing the carbon fiber sealing gasket according to any one of claims 1 to 7, characterized in that: include: S1. Preparation of modified carbon fiber: weigh a certain amount of carbon fiber, modifier 1, and modifier 2, mix and grind to obtain a mixed powder, heat the mixed powder to 600-1000° C., hold for 2-5 hours, cool to room temperature and grind to obtain modified carbon fiber, wherein: modifier 1 is a carbon fiber pore activator, and the mass ratio of carbon fiber to modifier 1 is 10-30:1; modifier 2 is a carbon fiber surface functional group agent, and the mass ratio of carbon fiber to modifier 2 is 3-20:1; S2: preparing a sealing gasket: weighing a thermoplastic matrix resin, a thermoplastic elastomer resin, a modified carbon fiber and a metal powder according to a proportion, mixing and stirring, and then hot-pressing to obtain a sealing gasket.
9. The preparation method according to claim 8, characterized in that: In S1, the carbon fiber is selected from carbon fiber powder, carbon fiber short fibers, carbon fiber long fibers, carbon fiber filaments, and carbon fiber cloth. When carbon fiber powder is selected, the average particle size of the carbon fiber powder is 20 to 100 μm; and / or The carbon fiber pore activator is selected from one or more of potassium hydroxide, potassium carbonate, potassium bicarbonate, potassium nitrate, sodium hydroxide, sodium carbonate, sodium bicarbonate, zinc chloride, and zinc nitrate; and / or The carbon fiber surface functional group agent is selected from one or more of ethylenediamine, urea, p-aminosalicylic acid, glycine, N-aminoethylpiperazine, diphenylaminourea, melamine, thiourea, mercaptan, phosphite, and boric acid.
10. The preparation method according to claim 8, characterized in that: In S2, the molding steps include: pre-pressing at a pressure of 3 to 8 MPa for 5 to 15 minutes; heating to 300 to 400°C for melting, and keeping the temperature for 1 to 5 hours; molding at a pressure of 3 to 8 MPa, and keeping the pressure for 10 to 30 minutes; obtaining a sample after cooling to room temperature, annealing at a constant temperature of 200 to 300°C for 60 to 180 minutes, and then processing it into the required sealing gasket.