Foaming material and preparation method thereof, antenna and base station equipment
By introducing triazine ring groups into the foamed material and controlling process parameters, the thermal expansion coefficient of the foamed material is reduced, the problem of mismatch with the metal conductor layer CTE is solved, and the temperature adaptability and stability of the material are improved.
Patent Information
- Application Number
- CN202310532487.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
The thermal expansion coefficient of the existing foaming materials is high, which leads to mismatch with the CTE of the metal conductor layer, which easily causes the falloff and failure of the dielectric and metal conductor layers.
Using cyanate foaming materials, the thermal expansion coefficient is reduced by introducing triazine ring groups into the main chain of the molecular, and the pore size distribution and glass transition temperature are controlled through low-temperature prepolymerization and high-temperature foaming processes to improve the rigidity of the material and Temperature adaptability.
The low thermal expansion coefficient of the foamed material is achieved, the temperature adaptability with the metal conductor layer is improved, the separation problem caused by CTE differences is avoided, and the stability and insulation of the dielectric layer are improved.
Smart Images

Figure CN118931157A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of foaming materials, and in particular to a foaming material and a preparation method thereof, an antenna and a base station device. Background Art
[0002] There are many types of polymer foam materials, such as polyurethane foam, phenolic foam, polyamide foam, high temperature resistant polyether foam, etc. Due to the low density, low dielectric constant and low dielectric loss of the foam material itself, it is expected to be used as a dielectric material in communication radio frequency equipment. However, the coefficient of thermal expansion (CTE) of the existing foam materials used as dielectrics is usually greater than 50ppm. When used as a dielectric in combination with a metal conductor layer or other structural materials, there is a CTE mismatch problem, which can easily cause the metal conductive layer to fall off and fail. Summary of the invention
[0003] The present application provides a foaming material and a preparation method thereof, an antenna and a base station device, so as to reduce the thermal expansion coefficient of the foaming material and improve its compatibility with a metal conductor layer when used as a dielectric.
[0004] In a first aspect, the present application provides a foaming material. The foaming material is a cyanate foaming material, and the infrared spectrum of the foaming material has a cyanate group characteristic peak and a triazine ring characteristic peak, and the cyanate group characteristic peak is located at 2248-2252cm -1 The characteristic peak of the triazine ring is located at 1368-1372 cm -1 Place.
[0005] The foaming material of the present application is a cyanate foaming material, which contains a cyanate group and a triazine ring in its molecular main chain. The infrared spectrum of the foaming material has infrared characteristic peaks of cyanate-OCN and infrared characteristic peaks of triazine ring. Since the triazine ring has higher rigidity and higher spatial structural stability, it can prevent the cyanate main chain structure from twisting or rotating. Therefore, the cyanate foaming material with a triazine ring group has a lower thermal expansion coefficient, and its thermal expansion coefficient can be reduced to 30ppm and below. Compared with existing foaming materials, it can have higher temperature adaptability with the metal conductor layer, avoiding separation of the dielectric and the metal conductor layer due to large differences in thermal expansion coefficients.
[0006] In one implementation, in the pore size distribution diagram of the foaming material, the difference between the pore size D90 and the pore size D10 is less than 10 μm. Wherein, D10 is the pore size corresponding to when the cumulative pore size distribution number of the foaming material reaches 10%; D90 is the pore size corresponding to when the cumulative pore size distribution number of the foaming material reaches 90%. The difference between the pore size D90 and the pore size D10 of the foaming material of the present application is less than 10 μm, indicating that the internal pore size of the foaming material is more uniform, thereby making the isotropic properties of the foaming material more uniform.
[0007] In one implementation, the glass transition temperature of the foaming material is greater than 200° C. The glass transition temperature of the foaming material is strongly correlated with the rigidity of the foaming material. The foaming material of the implementation of the present application has a higher glass transition temperature, which can indicate that the foaming material has a higher rigidity, thereby helping to improve the thermal stability of the foaming material and reduce the thermal expansion coefficient.
[0008] In one implementation, the softening point of the foaming material at 0.45 MPa is greater than or equal to 180°C.
[0009] In one implementation, the expansion coefficient of the foaming material at -45 to 150° C. is ≤30 ppm. Compared with existing cyanate foaming materials, the foaming material of the implementation of the present application has a lower thermal expansion coefficient. Therefore, when used for dielectrics, it can have better adaptability with the metal conductor layer, reduce the thermal expansion difference between the two, and improve the stability of the connection between the dielectric and the metal conductor layer.
[0010] In one implementation, the density of the foaming material is 50 to 300 kg / m 3 The foam material has a lower density, which can effectively reduce the amount of foam material used and help reduce the quality of devices containing the foam material and the metal conductor.
[0011] In one implementation, the water absorption rate of the foaming material is less than 0.8%. The lower water absorption rate of the foaming material can reduce the entry of water vapor into the foaming material. When the foaming material is used as a dielectric layer, the insulation of the dielectric layer can be improved.
[0012] In a second aspect, the present application provides a method for preparing a foaming material, the preparation method comprising:
[0013] A raw material mixture of cyanate ester or cyanate ester oligomer with a molecular weight less than 2000, a blowing agent, a catalyst and a curing agent is placed at 40°C to 120°C for 5 to 20 days for low-temperature prepolymerization to obtain a prepolymer; the prepolymer is placed at a temperature of 150 to 200°C for foaming for 1 to 8 hours to obtain the foaming material.
[0014] In the preparation method of the present application, cyanate or cyanate oligomer is first prepolymerized under low temperature environment, and part of cyanate groups are polymerized to form triazine ring groups during the low temperature prepolymerization process. After testing, the foaming material obtained by the preparation method of the present application has characteristic peaks of cyanate groups and characteristic peaks of triazine ring groups in its infrared spectrum. Since the triazine ring has higher rigidity and higher spatial structural stability, it can prevent the cyanate main chain structure from twisting or rotating. Therefore, the cyanate foaming material with triazine ring groups has a lower thermal expansion coefficient, and its thermal expansion coefficient can be reduced to 30ppm and below. Compared with existing foaming materials, it can have higher temperature adaptability with the metal conductor layer, avoiding separation of the dielectric and the metal conductor layer due to large differences in thermal expansion coefficients.
[0015] In one implementation, the raw material mixture includes, by weight: 30 to 80 parts of cyanate ester or cyanate ester oligomer with a molecular weight less than 2000, 3 to 30 parts of foaming agent, 0.1 to 5 parts of catalyst and 1 to 30 parts of curing agent. In a preferred implementation, the raw material mixture includes, by weight: 50 to 70 parts of cyanate ester or cyanate ester oligomer with a molecular weight less than 2000, 7 to 15 parts of foaming agent, 0.2 to 2 parts of catalyst and 7 to 15 parts of curing agent. The foaming material composed of the raw materials can be conducive to the formation of triazine rings with uniform and moderate content in the main chain structure of the cyanate resin, so as to obtain a foaming material with high heat resistance, low thermal expansion coefficient, low density, low water absorption and low dielectric loss.
[0016] In one implementation, the raw material mixture also includes a toughening agent, and the amount of the toughening agent added is 5 to 30 parts by weight; the toughening agent is a resin with a flexible chain. By adding a resin with a flexible chain as a toughening agent, the toughness of the foaming material can be increased, its brittleness can be reduced, and the impact resistance of the foaming material can be improved.
[0017] In one implementation, the foaming agent is a liquid foaming agent, and before the low-temperature prepolymerization, the preparation method further includes: dissolving the curing agent and the foaming agent in the toughening agent under pressure, and then mixing with the cyanate ester or the cyanate ester oligomer. The toughening agent can be a solid toughening agent or a liquid toughening agent. When the toughening agent is a liquid toughening agent, during the process of mixing the raw materials, the curing agent and the foaming agent can be first dissolved in the toughening agent under pressure to improve the mixing uniformity of the raw materials. When the toughening agent is a liquid toughening agent, during the low-temperature prepolymerization, the temperature can be about 20°C lower than the boiling point of the toughening agent.
[0018] In one implementation, the viscosity of the prepolymer at 150°C is 3000-30000 cp. By controlling the viscosity of the prepolymer at 150°C, it is helpful to control the number of triazine rings formed in the prepolymer to form a rigid skeleton structure and facilitate rapid foaming in a high temperature environment. In the prepolymerization stage, the cyanate ester oligomer is slowly self-polymerized in a low temperature environment to form a cyanate ester resin oligomer with a larger molecular weight. Then, the cyanate ester resin oligomer undergoes a curing reaction and a foaming reaction in a high temperature environment, thereby obtaining a foam material containing triazine ring groups and uniform pore size.
[0019] In a third aspect, the present application provides an antenna, comprising a dielectric and a metal conductor layer arranged on the dielectric, wherein the material of the dielectric is the foaming material of the present application or the foaming material is obtained by using the preparation method of the present application.
[0020] The antenna of the present application has higher stability because the dielectric layer adopts the foam material of the present application. On the basis of the high heat resistance and low linear expansion coefficient of the foam material of the present application, the antenna of the present application can have higher stability. Under the change of high temperature difference, the dielectric and metal conductor layers in the antenna can also maintain high adaptability, avoiding the problem of line shedding or delamination due to the large difference in thermal expansion coefficient between the two.
[0021] In a fourth aspect, the present application provides a base station device, which includes the antenna of the present application.
[0022] The technical effects that can be achieved in the fourth aspect mentioned above can be described with reference to the corresponding effects in the third aspect mentioned above, and will not be repeated here.
[0023] Among them, the data in the above-mentioned possible implementation methods of the present application, such as the band corresponding to the first characteristic peak in the infrared spectrum, the band corresponding to the second characteristic peak in the infrared spectrum, the glass transition temperature, density, water absorption rate of the foaming material, and the temperature and time in the preparation process of the foaming material, etc., when measuring, the values within the scope of engineering measurement error should be understood to be within the scope specified in the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the infrared spectrum of the foaming material of Example 1 of the present application;
[0025] Figure 2 This is the infrared spectrum of the foaming material of Comparative Example 1. DETAILED DESCRIPTION
[0026] In order to make the objectives, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings.
[0027] The terms used in the following embodiments are only for the purpose of describing specific embodiments and are not intended to be limiting of the present application. As used in the specification and appended claims of the present application, the singular expressions "a", "an", "above", "the" and "this" are intended to also include expressions such as "one or more", unless there is a clear contrary indication in the context.
[0028] The foam material can be used as a dielectric material for electromagnetic radio frequency devices. In order to obtain a foam material with a low CTE that is more consistent with the CTE of a metal material, an embodiment of the present application provides a foam material. The foam material is a cyanate foam material, and the infrared spectrum of the foam material has a cyanate group characteristic peak and a triazine ring characteristic peak. The cyanate group characteristic peak is located at 2248-2252cm -1 The characteristic peak of triazine ring is located at 1368-1372cm -1 Place.
[0029] The foaming material of the embodiment of the present application is a cyanate resin foaming material. Its main chain macromolecular structure is formed by polymerization of cyanate, and its main chain contains triazine ring groups. Among them, through infrared spectroscopy testing, the foaming material has characteristic peaks of cyanate-OCN groups and characteristic peaks of triazine ring groups. The formation of triazine ring groups can make the main chain of the foaming material have a certain rigidity, so as to improve the temperature stability of the foaming material and reduce its thermal expansion coefficient.
[0030] In the pore size distribution diagram of the foaming material of the embodiment of the present application, the difference between the pore size D90 and the pore size D10 is less than 10μm. Among them, the pore size D10 is the pore size corresponding to the cumulative pore size distribution number of the foaming material reaching 10%, and its physical meaning is that the proportion of holes with a pore size smaller than it is 10%. The pore size D90 is the pore size corresponding to the cumulative pore size distribution number of the foaming material reaching 90%. Its physical meaning is that the proportion of holes with a pore size smaller than it is 90%. In the foaming material of the embodiment of the present application, the difference between the pore size D90 and the pore size D10 is less than 10μm. When the difference between the pore size D90 and the pore size D10 is less than 10μm, the pore size distribution range of the foaming material is narrow, which indicates that the pore size of the foaming material is more uniform. The foaming material with uniform pore size has a higher degree of isotropy, which can make the foaming material have the same heat resistance everywhere inside.
[0031] Among them, the glass transition temperature of the foaming material of the embodiment of the present application is ≥200°C. Exemplarily, its glass transition temperature may be, for example, 200°C, 205°C, 210°C, 220°C, 230°C, 240°C, 250°C or higher. The glass ring transition temperature of the foaming material may be lower than 300°C. Compared with the traditional simple cyanate ester resin foaming material, when the cyanate ester groups are polymerized to form a triazine ring, the rigidity of the main chain structure of the cyanate ester resin can be improved. The glass transition temperature of the foaming material is strongly related to the main chain rigidity of the cyanate ester main resin. Therefore, the foaming material of the present application may have a higher glass transition temperature.
[0032] In one implementation, the softening point of the foaming material at 0.45 MPa is greater than or equal to 180° C. Compared with the conventional cyanate resin without triazine ring group, the softening point of the present application is higher, so as to improve the heat resistance of the foaming material.
[0033] The expansion coefficient of the foaming material at -45 to 150° C. is ≤30 ppm. The thermal expansion coefficient of the foaming material is typically but not limited to 30 ppm, 28 ppm, 26 ppm, 24 ppm, 22 ppm, 20 ppm, 18 ppm, 18 ppm, 16 ppm, 15 ppm or lower, and the lower the expansion coefficient of the foaming material, the higher the heat resistance.
[0034] The density of the foam material is 50~300kg / m 3 For example, the density of the foamed material may be 50 kg / m 3 、60kg / m 3 、80kg / m 3 , 100kg / m 3 , 120kg / m 3 , 150kg / m 3 、170kg / m 3 , 200kg / m 3 , 220kg / m 3 , 250kg / m 3 、270kg / m 3 or 300kg / m 3 The water absorption rate of the foaming material is less than 0.8%. For example, the water absorption rate of the foaming material may be 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2% or 0.1%. The foaming material of the embodiment of the present application may have a lower density and a lower water absorption rate to further reduce the weight of the foaming material itself and facilitate its use as a dielectric material.
[0035] The preparation method of the foaming material of the embodiment of the present application may include the following steps:
[0036] S11, placing a raw material mixture of a cyanate ester or a cyanate ester oligomer having a molecular weight less than 2000, a blowing agent, a catalyst and a curing agent at 40° C. to 120° C. for 5 to 20 days for low-temperature prepolymerization to obtain a prepolymer;
[0037] S12, placing the prepolymer at a temperature of 150 to 200° C. for foaming for 1 to 8 hours to obtain the foamed material.
[0038] The preparation method of the present application firstly mixes the raw material of cyanate ester with the catalyst, curing agent and foaming agent, then makes the cyanate ester undergo self-polymerization reaction at a relatively low temperature to form a prepolymer of cyanate ester resin with a relatively large molecular weight, then makes the prepolymer undergo curing reaction and foaming reaction under a high temperature environment, thereby obtaining a foaming material with uniform properties. In the preparation method, the cyanate ester is made to produce a rigid triazine ring group by a self-polymerization catalysis method, so as to increase the heat resistance of the foaming material.
[0039] In the process of preparing the foaming material, the viscosity of the prepolymer prepared in step S11 is 3000-30000 cp at 150° C. The reaction node of the prepolymer reaction is determined by detecting the viscosity of the prepolymer at 150° C.
[0040] The raw material mixture includes, by weight: 30-80 parts of cyanate ester or cyanate ester oligomer with a molecular weight less than 2000, 3-30 parts of foaming agent, 0.1-5 parts of catalyst, 1-30 parts of curing agent, and 5-30 parts of toughening agent, which are optional. Preferably, 50-70 parts of cyanate ester or cyanate ester oligomer with a molecular weight less than 2000, 5-15 parts of foaming agent, 0.2-2 parts of catalyst, 5-15 parts of curing agent, and 5-25 parts of toughening agent, which are optional.
[0041] Wherein, cyanate or cyanate oligomer includes but is not limited to at least one of bisphenol A cyanate, phenolic cyanate formed by common phenol formaldehyde, biphenyl phenolic cyanate, dicyclopentadiene cyanate, bisphenol E cyanate, and bisphenol M cyanate. In the raw material mixture, by weight, the addition amount of cyanate or cyanate oligomer is typically but not limited to 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts, 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, 62 parts, 64 parts, 66 parts, 68 parts or 70 parts or the numerical value between any of the above numerical values. It is understandable that the upper limit or lower limit of the addition amount of cyanate or cyanate oligomer can be selected from one of the above-mentioned numerical values.
[0042] The selection of the foaming agent is mainly based on the decomposition temperature matching the foaming temperature and the inert gas generated after decomposition without affecting the foaming. For example, the foaming agent can be nitrogen or carbon dioxide or alkane gas after decomposition. The foaming agent includes but is not limited to azo foaming agents or alkane foaming agents. Among them, the azo foaming agent can be, for example, azobisisobutyronitrile, and the alkane foaming agent can be, for example, cyclohexane.
[0043] Catalyst includes but is not limited to at least one of organic cobalt catalyst, organic tin catalyst, organic zinc catalyst and organic manganese catalyst. Exemplarily, the catalyst can be dibutyltin dilaurate, dibutyltin diacetate or 2-methylpyridine organic cobalt catalyst. In the raw material mixture, by weight, the addition amount of the catalyst is typically but not limited to 0.1 part, 0.2 part, 0.5 part, 0.8 part, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts or the numerical value between any of the above values. It is understood that the upper limit or lower limit of the addition amount of the catalyst can be selected from one of the above-listed numerical values.
[0044] Curing agent includes but is not limited to low molecular weight phenolic resin, organic amine curing agent, illustratively, such as triethylamine, ethylenediamine. In the raw material mixture, by weight, the addition amount of curing agent is typically but not limited to 1 part, 2 parts, 4 parts, 5 parts, 7 parts, 10 parts, 12 parts, 14 parts, 15 parts, 16 parts, 18 parts, 20 parts, 25 parts, 30 parts or the numerical value between any of the above numerical values. It is understood that the upper limit or lower limit of the addition amount of curing agent can be selected from one of the above listed numerical values.
[0045] Toughener is a resin with a flexible chain, including but not limited to oligomers, epoxy glycidyl esters or epoxy glycidyl ethers of bisphenol A epoxy resin. In the raw material mixture, the addition amount of curing agent is typically but not limited to 1 part, 2 parts, 4 parts, 5 parts, 7 parts, 10 parts, 12 parts, 14 parts, 15 parts, 16 parts, 18 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts or the value between any of the above values by weight. It is understandable that the upper limit or lower limit of the addition amount of toughener can be selected from one of the above listed values.
[0046] In the method for preparing the foaming material, when the foaming agent is solid, the raw materials can be directly mixed to obtain a raw material mixture. When the foaming agent is a liquid physical foaming agent, in addition to directly mixing the raw materials for prepolymerization and foaming, before the low-temperature prepolymerization, a step of dissolving the curing agent and the foaming agent in the toughening agent under pressure can also be included. Among them, by pressurized dissolution, the toughening agent can be softened by the foaming agent, so that the foaming agent and the toughening agent are mixed more evenly, so as to improve the mixing uniformity of the raw material mixture.
[0047] The foaming material will be described in detail below in conjunction with specific embodiments.
[0048] Example 1
[0049] This embodiment is a foaming material, and its preparation method includes the following steps:
[0050] Step S11, providing 70 parts of cyanate oligomer, 10 parts of foaming agent, 0.5 parts of catalyst, 10 parts of curing agent, and 10 parts of toughening agent by weight; fully stirring and mixing the above raw materials to uniformly dissolve, to obtain a raw material mixture.
[0051] The molecular weight of the cyanate oligomer is less than 2000 and it is in liquid state at 50°C. The foaming agent is an azo foaming agent (such as azobisisobutyronitrile) that can be decomposed at 150°C. The catalyst is organic tin. The curing agent is triethylamine. The toughening agent is an epoxy resin with a flexible chain (such as isocyanate-modified epoxy resin).
[0052] Step S12, controlling the reaction temperature of the raw material mixture at 70°C, reacting slowly for 7 days to obtain a prepolymer, and stopping the reaction when the viscosity of the prepolymer at 150°C reaches 10000cp.
[0053] Step S13, placing the prepolymer in a heat transfer mold, and heating the prepolymer in an oil bath, so that the temperature of the prepolymer is quickly heated to 180° C., reacting for 2 hours to form a foamed material after foaming and cross-linking.
[0054] Figure 1 It is the infrared spectrum of Example 1. Figure 1 As shown, the foamed material of this embodiment is at 2250cm -1 There is a characteristic peak of cyanate group at 1370cm -1 There is a characteristic peak of triazine ring.
[0055] Example 2
[0056] This embodiment is a foaming material, which is different from the embodiment 1 in that the amount of raw materials added is different. In this embodiment, the raw materials constituting the foaming material include, by weight: 50 parts of cyanate oligomer, 10 parts of foaming agent, 3 parts of catalyst, 5 parts of curing agent, and 10 parts of toughening agent.
[0057] Example 3
[0058] This embodiment is a foaming material, which is different from the embodiment 1 in that the amount of raw materials added is different. In this embodiment, the raw materials constituting the foaming material include, by weight: 60 parts of cyanate oligomer, 15 parts of foaming agent, 2 parts of catalyst, 8 parts of curing agent, and 15 parts of toughening agent.
[0059] Example 4
[0060] This embodiment is a foaming material, and its preparation method includes the following steps:
[0061] Step S11, providing 70 parts of cyanate oligomer, 10 parts of foaming agent, 0.5 parts of catalyst, 10 parts of curing agent, and 10 parts of toughening agent by weight; fully stirring and mixing the above raw materials to uniformly dissolve, to obtain a raw material mixture.
[0062] The molecular weight of the cyanate oligomer is less than 2000 and it is in liquid state at 50°C. The foaming agent is an azo foaming agent (azobisisobutyronitrile) that can be decomposed at 150°C. The catalyst is organic tin. The curing agent is triethylamine. The toughening agent is an epoxy resin with a flexible chain (isocyanate modified epoxy resin).
[0063] Step S12, control the reaction temperature of the raw material mixture at 70°C, react slowly for 10 days to obtain a prepolymer, and stop the reaction when the viscosity of the prepolymer at 150°C reaches 20,000cp. (It affects the uniformity of the blastholes and the proportion of triazine rings is relatively high) Step S13, place the prepolymer in a heat transfer mold, and heat the prepolymer through an oil bath to quickly heat the temperature of the prepolymer to 180°C, react for 3 hours to form a foamed material after foaming and cross-linking.
[0064] Example 5
[0065] This embodiment is a foaming material, and its preparation method includes the following steps:
[0066] Step S11, by weight, provide 70 parts of cyanate oligomer, 10 parts of foaming agent, 0.5 parts of catalyst, 10 parts of curing agent, and 10 parts of toughening agent. Among them, the molecular weight of cyanate oligomer is 2000-20000, and it is in liquid state at 50°C. The foaming agent is an alkane foaming agent (cyclohexane) with a boiling point of 120-150°C. Reduce the viscosity of the resin and promote the dissolution of each material. The catalyst is organic tin. The curing agent is ethylenediamine. The toughening agent is an epoxy resin with a flexible chain (isocyanate-modified epoxy resin).
[0067] Step S12: first dissolve the foaming agent and the curing agent in the toughening agent under a pressurized environment, and then fully stir and mix with other raw materials to obtain a raw material mixture.
[0068] Step S13, at a temperature 20° C. lower than the boiling point of the blowing agent, the raw material mixture is slowly reacted for 10 days to obtain a prepolymer, and the viscosity of the prepolymer at 150° C. reaches 20,000 cp.
[0069] Step S14, placing the prepolymer in a heat transfer mold, and heating the prepolymer in an oil bath, so that the temperature of the prepolymer is quickly heated to 180° C., reacting for 3 hours to form a foamed material after foaming and cross-linking.
[0070] Example 6
[0071] This embodiment is a foaming material, and its preparation method includes the following steps:
[0072] Step S11, by weight, provide 70 parts of cyanate oligomer, 10 parts of foaming agent, 0.5 parts of catalyst, 10 parts of curing agent, and 10 parts of toughening agent. Among them, the molecular weight of cyanate oligomer is 2000-20000, and it is in liquid state at 50°C. The foaming agent is an alkane foaming agent (cyclohexane) with a boiling point of 120-150°C. The catalyst is organic tin. The curing agent is ethylenediamine. The toughening agent is an epoxy resin with a flexible chain (isocyanate modified epoxy resin).
[0073] Step S12: Firstly, the foaming agent and the curing agent are dissolved in the toughening agent by pressurizing, and then the foaming agent and the curing agent are fully stirred and mixed with other raw materials to obtain a raw material mixture.
[0074] Step S13, at a temperature 20° C. lower than the boiling point of the blowing agent, the raw material mixture is slowly reacted for 10 days to obtain a prepolymer, and the viscosity of the prepolymer at 150° C. reaches 20,000 cp.
[0075] Step S14, placing the prepolymer in a heat transfer mold, and heating the prepolymer in an oil bath, so that the temperature of the prepolymer is quickly heated to 180° C., reacting for 2 hours to form a foamed material after foaming and cross-linking.
[0076] Comparative Example 1
[0077] This comparative example is a foaming material, and its preparation method comprises the following steps:
[0078] Step S11, providing 70 parts of cyanate oligomer, 10 parts of foaming agent, 0.5 parts of catalyst, 10 parts of curing agent, and 10 parts of toughening agent by weight; fully stirring and mixing the above raw materials to uniformly dissolve, to obtain a raw material mixture.
[0079] The molecular weight of the cyanate oligomer is less than 2000 and it is in liquid state at 50°C. The foaming agent is an azo foaming agent (such as azobisisobutyronitrile) that can be decomposed at 150°C. The catalyst is organic tin. The curing agent is triethylamine. The toughening agent is an epoxy resin with a flexible chain (such as isocyanate-modified epoxy resin).
[0080] Step S12, placing the raw material mixture in a heat transfer mold, and heating the raw material mixture in an oil bath, so that the temperature of the raw material mixture is quickly heated to 180° C., reacting for 2 hours to form a foaming material after foaming and cross-linking.
[0081] Figure 2 It is the infrared spectrum of comparative example 1. Figure 2 As shown, the foaming material of this comparative example does not have the characteristic peak of triazine ring, indicating that the foaming material having triazine ring cannot be obtained according to the method of comparative example 1.
[0082] The pore size, glass transition temperature, softening point, density, heat deformation temperature, CTE and water absorption of the foaming materials of each embodiment and comparative example were tested respectively. The test results are listed in Table 1.
[0083] Among them, the performance testing methods of various foaming materials are as follows.
[0084] The pore size test method of the foam material is determined according to GB / T 12811-1991 Test method for average pore size of rigid foam plastics.
[0085] Test method for glass transition temperature: Determined according to the method of GB / T 1634-2004 for glass transition temperature of plastics.
[0086] Test method for softening point: Determined according to GB-T 1633-2000 Vicat softening temperature of thermoplastics.
[0087] Density test method: Determine according to the method of apparent density of foam plastics GB-T-6343-2009.
[0088] Test method for heat deformation temperature: Test according to GB / T 1634.2-2004 Plastic heat deformation temperature method.
[0089] CTE test method: Determined according to the method of linear thermal expansion coefficient of GB / T 36800.2-2018.
[0090] Test method for water absorption: Determine according to the method for water absorption of rigid foam plastics in GB T 8810-2005.
[0091] Table 1
[0092]
[0093] It can be seen from the relevant test data in Table 1 that the CTE of Examples 1-6 of the present application is 30ppm or less. The CTE of Comparative Example 1 reaches 50ppm. The softening point and thermal deformation temperature of Examples 1-6 are higher. This shows that the foaming materials of the embodiments of the present application can have better heat resistance. In addition, compared with Comparative Example 1, the density of the foaming materials of the embodiments of the present application is also lower, and the pore size distribution is also more uniform, and the uniformity of the various properties of the corresponding foaming materials is also better.
[0094] From the comparative data of Examples 1 to 3, it can be seen that when the raw material composition of the foaming material is changed, the various properties of the obtained foaming material are changed. However, due to the presence of triazine rings in their molecular structures, the CTE of the foaming materials of Examples 1-3 is lower than the cyanate resin foaming material obtained by the traditional foaming form in Comparative Example 1.
[0095] From the comparison data of Example 1 and Example 4, it can be seen that the properties of the foamed material obtained by low-temperature prepolymerization are slightly different when the viscosity is different. When the viscosity of the obtained prepolymer is higher, it means that the number of triazine ring groups in the prepolymer is more, so that the CTE of the obtained foamed material is lower.
[0096] From the relevant test data of Example 4, Example 5 and Example 6, it can be seen that when the type of foaming agent is changed, the CTE of the obtained foaming material is basically the same. However, the uniformity of the pore size of the foaming material is improved. It shows that when the foaming agent is a liquid foaming agent and the foaming agent, curing agent and toughening agent are mixed by pressurization, the mixing uniformity of the raw materials can be improved, which is conducive to improving the uniformity of the foaming material.
[0097] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A foaming material, characterized in that: The foaming material is a cyanate foaming material. The infrared spectrum of the foaming material has a cyanate group characteristic peak and a triazine ring characteristic peak. The cyanate group characteristic peak is located at 2248-2252 cm -1 The characteristic peak of the triazine ring is located at 1368-1372 cm -1 Place.
2. The foam material according to claim 1, characterized in that: In the pore size distribution diagram of the foaming material, the difference between the pore size D90 and the pore size D10 is less than 10 μm.
3. The foam material according to claim 1 or 2, characterized in that: The glass transition temperature of the foaming material is ≥200°C, and the softening point of the foaming material at 0.45 MPa is greater than or equal to 180°C.
4. The foaming material according to any one of claims 1 to 3, characterized in that: The expansion coefficient of the foaming material at -45 to 150° C. is ≤30 ppm.
5. The foaming material according to any one of claims 1 to 4, characterized in that: The density of the foaming material is 50-300 kg / m 3 .
6. The foaming material according to any one of claims 1 to 5, characterized in that: The water absorption rate of the foaming material is less than 0.8%.
7. A method for preparing a foaming material, characterized in that: include: The raw material mixture of cyanate ester or cyanate ester oligomer with a molecular weight less than 2000, a blowing agent, a catalyst and a curing agent is placed at 40° C. to 120° C. for 5 to 20 days for low temperature prepolymerization to obtain a prepolymer; The prepolymer is placed at a temperature of 150 to 200° C. for foaming for 1 to 8 hours to obtain the foamed material.
8. The preparation method according to claim 7, characterized in that: The raw material mixture comprises, by weight: 30-80 parts of cyanate ester or cyanate ester oligomer with a molecular weight less than 2000, 3-30 parts of foaming agent, 0.1-5 parts of catalyst and 1-30 parts of curing agent.
9. The preparation method according to claim 7 or 8, characterized in that: The raw material mixture also includes a toughening agent, and the addition amount of the toughening agent is 5 to 30 parts by weight; the toughening agent is a resin with a flexible chain.
10. The preparation method according to claim 9, characterized in that: The foaming agent is a liquid foaming agent. Before the low-temperature prepolymerization, the preparation method further comprises the steps of dissolving the curing agent and the foaming agent in the toughening agent under pressure, and then mixing them with the catalyst, the cyanate ester or the cyanate ester oligomer.
11. The preparation method according to any one of claims 7 to 10, characterized in that: The viscosity of the prepolymer at 150° C. is 3000 to 30000 cp.
12. An antenna, characterized in that: It comprises a dielectric and a metal conductor layer arranged on the dielectric, wherein the material of the dielectric is the foaming material as described in any one of claims 1 to 6 or the foaming material obtained by the preparation method as described in any one of claims 7 to 11.
13. A base station device, characterized in that: Comprising the antenna as claimed in claim 12.