Cellulose micropowder exterior wall coating as well as preparation method and application thereof

By using cellulose micropowder exterior wall coatings with specific particle size and aspect ratios, combined with other additives, the problems of easy damage and insufficient hydrophobic performance of exterior wall coatings in the natural environment are solved, and the high stability, durability and Improved aesthetics.

CN118931279APending Publication Date: 2024-11-12WUHAN TEXTILE UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411108772.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing exterior wall coatings are prone to cracking, pulverizing, peeling and fading in the natural environment, and have insufficient hydrophobic properties, making them difficult to resist moisture penetration, affecting the service life of the building and the comfort of the living environment.

Method used

Using cellulose micropowder exterior wall coating, the first and second cellulose micropowders with specific particle size and aspect ratio are obtained by micronizing the cellulose fibers, combined with silane coupling agent, acrylate copolymer, film forming additive, flow Flat agent, defoaming agent and anti-mold agent form coatings with excellent hydrophobic properties and anti-fouling properties.

Benefits of technology

It improves the stability, sun resistance, water resistance and adhesion of the coating, enhances the anti-crack, sun protection and waterproof performance of the coating, and improves the stain removal ability and aesthetics of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931279A_ABST
    Figure CN118931279A_ABST
Patent Text Reader

Abstract

The invention provides a cellulose micro-powder exterior wall coating and a preparation method and application thereof, and the exterior wall coating is prepared by taking a cellulose micro-powder mixture with specific particle size and length-diameter ratio as a pigment filler. The synergistic effect between the first cellulose micro powder and the second cellulose micro powder which are different in size performance in the cellulose micro powder mixture can be utilized, all components in the coating can be evenly mixed, meanwhile, the hydrophobicity and roughness of the coating are improved, the interface bonding firmness between a base material and the coating is enhanced, the stability of the coating in the using process is improved, and the service life of the coating is prolonged. And a texture structure can be formed on the coating by means of the size difference of the cellulose micro powder in the coating forming process. By adopting the mode, the cellulose micro-powder exterior wall coating with strong dirt-removing power, stability, solarization resistance, water resistance and cleanability is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating preparation, and in particular to a cellulose micropowder exterior wall coating and a preparation method and application thereof. Background Art

[0002] In recent years, the use of exterior wall coatings in the construction industry has become increasingly popular, but the current products in the exterior wall coating industry have exposed several shortcomings. During long-term outdoor use, exterior wall coatings are extremely susceptible to the severe test of the natural environment, including wind, sun, rain, salt spray erosion, and large temperature fluctuations, which in turn lead to cracking, powdering, peeling, fading and other degradation phenomena of the coating. This condition not only weakens the decorative aesthetic value of the coating, but also may reduce its function of protecting the wall and accelerate the natural aging process of the wall. In addition, some exterior wall coatings have defects in hydrophobicity and are difficult to effectively resist the penetration of water, causing the wall to be easily damp and moldy, which has an adverse effect on the long-term service life of the building and the comfort of the living environment. Over time, exterior wall coatings are also susceptible to a variety of pollutants in outdoor environments, such as dust accumulation and impurities carried in rainwater. If the scrub resistance of the coating is insufficient, it is difficult to restore its original cleanliness and aesthetics even with regular cleaning, which brings additional challenges to building maintenance.

[0003] In view of this, it is necessary to design an improved cellulose micropowder exterior wall coating and its preparation method and application to solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to provide a cellulose micropowder exterior wall paint and a preparation method and application thereof.

[0005] To achieve the above-mentioned object of the invention, on the one hand, the present invention provides a cellulose micropowder exterior wall coating, comprising the following raw materials: a cellulose micropowder mixture, a silane coupling agent, an acrylate copolymer, a film-forming aid, a leveling agent, a defoaming agent, and a mildew preventer, wherein the cellulose micropowder mixture is obtained by mixing a first cellulose micropowder obtained by micronizing cellulose fibers and a second cellulose micropowder;

[0006] The mass ratio of the first cellulose micropowder to the second cellulose micropowder is 1:1-1:5, the particle size of the first cellulose micropowder is 3-100 μm, and the aspect ratio is 5:1-30:1, and the particle size of the second cellulose micropowder is 100-500 nm, and the aspect ratio is 1:1-1.5:1.

[0007] Preferably, the cellulose powder exterior wall paint comprises the following raw materials in parts by weight: 1-5 parts of cellulose powder mixture, 5-10 parts of silane coupling agent, 30-40 parts of acrylate copolymer, 15-30 parts of film-forming aid, 2-5 parts of leveling agent, 2-5 parts of defoaming agent, and 2-5 parts of mildewproofing agent.

[0008] Preferably, the silane coupling agent is one of vinyl silane, amino silane, urea silane, amide silane, aminopropyl silane, aryl silane and cationic silane.

[0009] Preferably, the film-forming aid is one of propylene glycol butyl ether, benzyl alcohol, hexadecyl alcohol ester, and dicyclopentenyloxyethyl acrylate; the leveling agent is one of water-based polyurethane leveling agent, polyether leveling agent, acrylate leveling agent, fluorocarbon leveling agent, and silicone leveling agent; the defoaming agent is one of polysiloxane defoaming agent, polyether defoaming agent, mineral oil defoaming agent, magnesium silicate defoaming agent, and aluminum hydroxide defoaming agent; the mildew inhibitor is one of biphenyl, o-phenylphenol, ammonium persulfate, calcium phosphate, zinc ion, silver ion, copper ion compound, and mustard extract.

[0010] Furthermore, the present invention also provides a method for preparing the cellulose micropowder exterior wall paint, comprising the following steps:

[0011] S1. Crush a cellulose fabric with a cutting machine to obtain colored staple fibers, and micronize the colored staple fibers to obtain a first cellulose micropowder slurry and a second cellulose micropowder slurry; dry the first cellulose micropowder slurry and the second cellulose micropowder slurry to obtain a first cellulose micropowder and a second cellulose micropowder, and mix the first cellulose micropowder and the second cellulose micropowder in a mass ratio of 1:1-1:5 to obtain a cellulose micropowder mixture;

[0012] S2. Evenly mix the cellulose powder mixture obtained in step S1 with a silane coupling agent, an acrylate copolymer, a film-forming aid, a leveling agent, a defoaming agent, and a mildew preventer to obtain a cellulose powder exterior wall coating.

[0013] Preferably, in step S1, the micronization treatment is carried out as follows: after mixing the colored staple fibers and deionized water, the colored staple fibers are treated with zirconium oxide spheres as ball milling media, and after the ball milling, the mixture is cooled to 16-30°C to obtain a first cellulose micropowder slurry or a second cellulose micropowder slurry.

[0014] Preferably, in the preparation process of the first cellulose micropowder, the mass ratio of colored staple fibers to deionized water is 1:10-1:30, the size of the zirconium oxide spheres is 6-8 mm, the amount added is 20-25 kg, the ball milling time is 1-6 h, and the rotation speed of the ball milling process is 180-330 rpm.

[0015] Preferably, in the preparation process of the second cellulose micropowder, the mass ratio of colored staple fibers to deionized water is 1:10-1:30, the size of the zirconium oxide spheres is 2-4 mm, the amount added is 20-25 kg, the ball milling time is 6-12 h, and the rotation speed of the ball milling process is 180-330 rpm.

[0016] Preferably, in step S1, during the drying process, the inlet temperature is 180°C, the outlet temperature is 100-130°C, and the flow rate of the first cellulose micropowder slurry and the second cellulose micropowder slurry is 20-40 mL / min.

[0017] In particular, the cellulose micropowder exterior wall paint prepared by the preparation method proposed in the present invention can be applied to the field of construction.

[0018] The beneficial effects of the present invention are:

[0019] 1. The preparation method of the cellulose micropowder exterior wall paint provided by the present invention is to further prepare the paint by using a cellulose micropowder mixture with a specific particle size and aspect ratio as a pigment filler. The process can utilize the synergistic effect between the first cellulose micropowder and the second cellulose micropowder with different size properties in the cellulose micropowder mixture, which is conducive to the uniform mixing of the various components in the paint, and at the same time improves the hydrophobicity of the paint, prompting the paint to have a larger roughness after forming the coating, improves the firmness of the interface bonding between the substrate and the paint, and improves the stability of the paint during use. By adopting the above method, the present invention prepares a cellulose micropowder exterior wall paint with strong decontamination ability, stability, sunlight resistance, water resistance, and cleanability.

[0020] 2. The preparation method of the cellulose powder exterior wall coating provided by the present invention, by adding cellulose powders of different sizes, the size characteristics between the two can be used to synergistically enhance the hydrophobicity and roughness of the coating, giving the coating excellent anti-fouling performance, improving the bonding force between the coating and the substrate during use, improving the stability of the coating as a whole, and obtaining a coating with excellent performance; by regulating the conditions of the micronization treatment, the size of the cellulose powder can be accurately regulated to achieve controllable preparation of the coating; by adjusting the addition amount of the first cellulose powder and the second cellulose powder, the fine regulation of the coating performance is achieved. In this process, the first cellulose powder of large size can be used to change the viscosity of the coating, and in the subsequent coating process, the texture structure is formed on the coating with the help of the first cellulose powder, giving the coating better aesthetics, on the other hand, the first cellulose powder can be used together with the second cellulose powder of small size to improve the roughness and hydrophobicity of the coating, and improve the adhesion of the coating. Under the joint action of the above-mentioned aspects, the adhesion between the coating and the substrate is improved, and a cellulose powder exterior wall coating with excellent anti-cracking, sunscreen and waterproof performance is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM image of the cellulose powder mixture prepared in Example 1 of the present invention;

[0022] Figure 2 The WCA test results of the coating prepared in Example 1 of the present invention;

[0023] Figure 3 It is a cross-sectional view of the coating prepared in Example 1 of the present invention and the coating prepared without adding cellulose powder after forming a coating;

[0024] Figure 4 This is a graph showing the adhesion test of the coating prepared in Example 1 of the present invention;

[0025] Figure 5 This is a color uniformity distribution diagram of the coating prepared in Example 1 of the present invention in a sunlight resistance test;

[0026] Figure 6 This is a diagram showing uniform color distribution of the coating prepared in Example 1 of the present invention in a water resistance experiment. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0028] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0029] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0030] On the one hand, the present invention provides a cellulose micropowder exterior wall paint, which includes the following raw materials: 1-5 parts of a cellulose micropowder mixture, 5-10 parts of a silane coupling agent, 30-40 parts of an acrylate copolymer, 15-30 parts of a film-forming aid, 2-5 parts of a leveling agent, 2-5 parts of a defoaming agent, and 2-5 parts of a mildew preventer. The cellulose micropowder mixture is obtained by mixing a first cellulose micropowder obtained by micronizing cellulose fibers and a second cellulose micropowder, the mass ratio of the first cellulose micropowder to the second cellulose micropowder is 1:1-1:5, the particle size of the first cellulose micropowder is 3-100 μm, and the aspect ratio is 5:1-30:1, and the particle size of the second cellulose micropowder is 100-500 nm, and the aspect ratio is 1:1-1.5:1.

[0031] Furthermore, the present invention also provides a method for preparing the above-mentioned cellulose micropowder exterior wall coating, comprising the following steps:

[0032] S1. Preparation of a cellulose micropowder mixture: pure color waste cellulose fabric is crushed by a cutting machine to obtain colored staple fibers, and the colored staple fibers are micronized to obtain a first cellulose micropowder slurry and a second cellulose micropowder slurry with different particle sizes and aspect ratios; the first cellulose micropowder slurry and the second cellulose micropowder slurry are dried to obtain a first cellulose micropowder and a second cellulose micropowder, and the first cellulose micropowder and the second cellulose micropowder are uniformly mixed in a mass ratio of 1:1-1:5 to obtain a cellulose micropowder mixture;

[0033] S2. Preparation of cellulose micropowder exterior wall paint: The cellulose micropowder mixture prepared in step S1 is evenly mixed with a silane coupling agent, an acrylate copolymer, a film-forming aid, a leveling agent, a defoaming agent, and a mildew preventer to prepare a cellulose micropowder exterior wall paint.

[0034] As an embodiment of the present invention, in step S1, the pure color waste cellulose fabric is one of cotton fabric, linen fabric, wool fabric, and silk fabric, and the particle size of the colored staple fiber is 10-1000 μm. In the above process, by selecting pure color waste cellulose fabric as the cellulose source, on the one hand, the recycling of resources is achieved, and on the other hand, by introducing colored cellulose, the amount of pigment used in the coating preparation process is reduced, thereby reducing the production cost of the coating.

[0035] As an embodiment of the present invention, in step S1, the micronization treatment is carried out as follows: a mixture of colored staple fibers and deionized water is put into a ball mill, and the colored staple fibers are treated with zirconium oxide spheres as ball milling media. After the ball milling, the mixture is cooled to 16-30°C to obtain a first cellulose micropowder slurry / a second cellulose micropowder slurry.

[0036] Furthermore, in the process of obtaining the first cellulose micropowder slurry, the mass ratio of colored staple fibers to deionized water is 1:10-1:30, the size of the zirconium oxide spheres is 6-8 mm, the amount thereof added is 20-25 kg, the ball milling time is 1-6 h, and the speed of the ball milling process is 180-330 rpm; in the process of obtaining the second cellulose micropowder slurry, the mass ratio of colored staple fibers to deionized water is 1:10-1:30, the size of the zirconium oxide spheres is 2-4 mm, the amount thereof added is 20-25 kg, the ball milling time is 6-12 h, and the speed of the ball milling process is 180-330 rpm. In the above process, by adjusting the process conditions of the ball milling process, cellulose micropowders with the required aspect ratio and particle size can be accurately obtained.

[0037] As an embodiment of the present invention, in step S1, during the drying process, the inlet temperature is 180°C, the outlet temperature is 100-130°C, and the flow rate of the first cellulose micropowder slurry and the second cellulose micropowder slurry is 20-40 mL / min.

[0038] As an embodiment of the present invention, in step S2, the silane coupling agent is one of vinyl silane, amino silane, urea silane, amide silane, aminopropyl silane, aryl silane, and cationic silane.

[0039] As an embodiment of the present invention, in step S2, the film-forming aid is one of propylene glycol butyl ether, benzyl alcohol, hexadecene, dicyclopentenyloxyethyl acrylate, etc., the leveling agent is one of water-based polyurethane leveling agent, polyether leveling agent, acrylate leveling agent, fluorocarbon leveling agent, silicone leveling agent, etc., the defoaming agent is one of polysiloxane defoaming agent, polyether defoaming agent, mineral oil defoaming agent, magnesium silicate defoaming agent, aluminum hydroxide defoaming agent, etc., and the mildew inhibitor is one of biphenyl, o-phenylphenol, ammonium persulfate, calcium phosphate, zinc ion, silver ion, copper ion compound, mustard extract, etc.

[0040] Furthermore, the cellulose micropowder exterior wall paint prepared by the above method can be applied to the construction field, and during the application process, it only needs to be directly coated on the surface of the substrate, and the substrate includes ceramic tiles, cement boards, wooden boards, metal plates, and glass plates.

[0041] The cellulose powder exterior wall coating and its preparation method and application proposed by the present invention are further described below in conjunction with specific embodiments:

[0042] Example 1

[0043] This example prepares a cellulose micropowder exterior wall paint, and the preparation method is as follows:

[0044] S1. Pure color waste cotton fabric is crushed with a cutting machine to obtain colored staple fibers with a particle size of 10-1000 μm; 100 g of colored staple fibers and deionized water are mixed evenly at a mass ratio of 1:10, and zirconium oxide spheres with a diameter of about 8 mm are used as ball milling media, the amount of which is 20 kg, the rotation speed of the ball milling process is 180 rpm, the time is 1 h, and the temperature range of the grinding tank after water cooling during the micronization process is 20° C., and a first cellulose micropowder slurry with a particle size of 50 μm and an aspect ratio of 20:1-30:1 is obtained; the first cellulose micropowder slurry is dried to obtain a first cellulose micropowder, the inlet temperature during the drying process is 180° C., the outlet temperature is 115° C., and the flow rate of the first cellulose micropowder slurry is 30 mL / min;

[0045] 100g of colored staple fibers and deionized water were mixed evenly in a mass ratio of 1:10, and zirconium oxide spheres with a diameter of about 4mm were used as ball milling media. The amount of zirconia spheres added was 20kg, the rotation speed of the ball milling process was 180rpm, the time was 6h, and the temperature range of the grinding tank after water cooling during the micronization process was 20°C, and a second cellulose micropowder slurry with a particle size of 400nm and an aspect ratio of 1.5:1-1.3:1 was obtained; the second cellulose micropowder slurry was dried to obtain a second cellulose micropowder, the inlet temperature during the drying process was 180°C, the outlet temperature was 115°C, and the flow rate of the second cellulose micropowder slurry was 30mL / min;

[0046] The first cellulose micropowder and the second cellulose micropowder were uniformly mixed in a mass ratio of 1:1 to obtain a cellulose micropowder mixture, the SEM image of which is shown in FIG. Figure 1 As shown in the figure, it can be seen that the small-sized second cellulose micropowder is adsorbed on the surface of the first cellulose micropowder;

[0047] S2, 5 parts of the cellulose powder mixture prepared in step S1 according to the mass ratio are mixed evenly with 10 parts of γ-aminopropyl triethoxysilane, 40 parts of acrylate copolymer, 30 parts of alcohol ester hexadecane, 5 parts of acrylate leveling agent BYK-258N, 5 parts of polysiloxane defoamer, and 5 parts of calcium phosphate to prepare cellulose powder exterior wall coating. The surface WCA test results of the cellulose powder exterior wall coating are shown in the figure below: Figure 2 As shown in Figure 2, the initial contact angle of the coating surface increased from 95.7° without powder to 145.8° after adding powder, and remained above 140° after 80s. The results show that the addition of cellulose powder improves the hydrophobicity of the coating; SEM images are shown in Figure 2 Figure 3 As shown in b, the SEM images of the coating prepared by adding the cellulose powder and the coating without adding the cellulose powder are shown in Figure 3 By comparison with a, it can be seen that after adding cellulose powder, cellulose powder with aspect ratio appears inside the coating. Large-sized cellulose powder exists as white flocs, and small-sized cellulose powder is attached to the surface of the white flocs or dispersed in the rest of the raw materials. The adhesion test of the coating and the substrate is shown in the figure Figure 4 As shown in b, the adhesion test diagram of the coating made with and without cellulose powder Figure 4 By comparison with a, it can be seen that the coating obtained by adding cellulose micropowder will not peel off from the substrate when subjected to external force. This is because the tough structure of cellulose itself will play a buffering role in the event of external force damage, indicating that the adhesion level of the coating is improved after the addition of cellulose micropowder.

[0048] In this embodiment, the cellulose powder exterior wall paint is applied to a 15 cm × 15 cm asbestos-free fiber cement board that meets the GB / T9271 (paint and varnish-standard test board) standard after being polished with 200 sandpaper and cured to form a coating. The sun resistance and water resistance of the asbestos-free fiber cement board after coating with dye are investigated. A 300W xenon lamp is used to irradiate the asbestos-free fiber cement board for 10 hours. The color uniformity distribution of the coating after irradiation is as shown in the figure below. Figure 5 As shown in the figure, the color difference of the cement board before and after irradiation is ΔE<2, and the color of the sample is almost unchanged, indicating that the coating has excellent sunlight resistance. After the above-mentioned asbestos-free fiber cement board is immersed in deionized water for 72 hours, the color uniformity of the coating is shown in the figure Figure 6 As shown, the results show that the color of the coating remains almost unchanged before and after irradiation.

[0049] Example 2

[0050] This example prepares a cellulose micropowder exterior wall paint, and the preparation method is as follows:

[0051] S1. Pure color waste cotton fabric is crushed with a cutting machine to obtain colored staple fibers with a particle size of 10-1000 μm; 100 g of colored staple fibers and deionized water are mixed evenly at a mass ratio of 1:20, and zirconium oxide spheres with a diameter of about 7 mm are used as ball milling media, the amount of which is 23 kg, the rotation speed of the ball milling process is 280 rpm, the time is 2 h, and the temperature range of the grinding tank after water cooling during the micronization process is 16 ° C, and a first cellulose micropowder slurry with a particle size of 20 μm and an aspect ratio of 10: 1-15: 1 is obtained; the first cellulose micropowder slurry is dried to obtain a first cellulose micropowder, the inlet temperature during the drying process is 180 ° C, the outlet temperature is 130 ° C, and the flow rate of the first cellulose micropowder slurry is 20 mL / min;

[0052] 100g of colored staple fibers and deionized water were mixed evenly at a mass ratio of 1:20, and zirconium oxide spheres with a diameter of about 3mm were used as ball milling media. The amount of zirconia spheres added was 23kg, the rotation speed of the ball milling process was 280rpm, the time was 9h, and the temperature range of the grinding tank after water cooling during the micronization process was 16°C, and a second cellulose micropowder slurry with a particle size of 300nm and an aspect ratio of 1.3:1-1.1:1 was obtained; the second cellulose micropowder slurry was dried to obtain a second cellulose micropowder, the inlet temperature during the drying process was 180°C, the outlet temperature was 130°C, and the flow rate of the second cellulose micropowder slurry was 20mL / min;

[0053] The first cellulose micropowder and the second cellulose micropowder are uniformly mixed in a mass ratio of 1:3 to prepare a cellulose micropowder mixture;

[0054] S2. Evenly mix 3 parts of the cellulose powder mixture prepared in step S1 according to the mass ratio with 8 parts of γ-aminopropyltriethoxysilane, 30 parts of acrylate copolymer, 25 parts of alcohol ester hexadecene, 3 parts of acrylate leveling agent BYK-258N, 3 parts of polysiloxane defoaming agent, and 3 parts of calcium phosphate to prepare a cellulose powder exterior wall coating.

[0055] In this embodiment, the cellulose micropowder exterior wall paint is applied to a tinplate of 12 cm×2.5 cm×0.3 mm and then cured to form a coating.

[0056] Example 3

[0057] This example prepares a cellulose micropowder exterior wall paint, and the preparation method is as follows:

[0058] S1. Pure color waste cotton fabric is crushed with a cutting machine to obtain colored staple fibers with a particle size of 10-1000 μm; 100 g of colored staple fibers and deionized water are mixed evenly at a mass ratio of 1:30, and zirconium oxide spheres with a diameter of about 6 mm are used as ball milling media, the amount of which is 25 kg, the rotation speed of the ball milling process is 330 rpm, the time is 3 h, and the temperature range of the grinding tank after water cooling during the micronization process is 25 ° C, and a first cellulose micropowder slurry with a particle size of 16 μm and an aspect ratio of 5: 1-8: 1 is obtained; the first cellulose micropowder slurry is dried to obtain a first cellulose micropowder, the inlet temperature during the drying process is 180 ° C, the outlet temperature is 105 ° C, and the flow rate of the first cellulose micropowder slurry is 40 mL / min;

[0059] 100g of colored staple fibers and deionized water were mixed evenly at a mass ratio of 1:30, and zirconium oxide spheres with a diameter of about 2mm were used as ball milling media. The amount of zirconia spheres added was 25kg, the rotation speed of the ball milling process was 330rpm, the time was 12h, and the temperature range of the grinding tank after water cooling during the micronization process was 25°C, and a second cellulose micropowder slurry with a particle size of 150nm and an aspect ratio of 1.1:1-1:1 was obtained; the second cellulose micropowder slurry was dried to obtain a second cellulose micropowder, the inlet temperature during the drying process was 180°C, the outlet temperature was 105°C, and the flow rate of the second cellulose micropowder slurry was 40mL / min;

[0060] The first cellulose micropowder and the second cellulose micropowder are uniformly mixed in a mass ratio of 1:5 to prepare a cellulose micropowder mixture;

[0061] S2. Evenly mix 2 parts of the cellulose powder mixture prepared in step S1 according to the mass ratio with 6 parts of γ-aminopropyltriethoxysilane, 25 parts of acrylate copolymer, 20 parts of alcohol ester hexadecene, 2 parts of acrylate leveling agent BYK-258N, 2 parts of polysiloxane defoaming agent, and 2 parts of calcium phosphate to prepare a cellulose powder exterior wall coating.

[0062] In this embodiment, the cellulose powder exterior wall paint is also applied to a 20cm×30cm×0.8cm asbestos-free fiber cement board to form a coating after curing. The color properties of the coatings formed in Examples 1 to 3 are shown in Table 1. The results show that the color brightness of the coatings prepared in the embodiments remains constant, the color uniformity is good (ΔE<2), and there is no color difference when observed with the naked eye. In this process, if the amount of cellulose powder with a specific aspect ratio added is too much, the micron-sized fiber powders will be bent and entangled with each other during the adhesion test tape adhesion stage, resulting in powder shedding, thereby reducing the adhesion level; if the amount of cellulose powder added is insufficient, the buffering effect between the coating and the substrate will be reduced during the adhesion test tape adhesion stage, thereby reducing the adhesion level.

[0063] The ΔE calculation formula is as follows:

[0064]

[0065] Among them, Δa, Δb and ΔL are equal to the difference between a, b and L between the samples before and after sun exposure. a represents the range of components from green to red in the hue, b represents the range of components from blue to yellow in the hue, and L is the brightness of the color. ΔE is the color difference factor in the chromaticity space. Studies have shown that ΔE values ​​below 2 can only be perceived by trained eyes, values ​​between 3.5 and 5 indicate obvious differences, and values ​​above 5 indicate recognizable color contrast.

[0066] The coating performance comparisons obtained in Examples 1 to 3 are shown in Table 2. During the experiment, the above results were also compared with the blank sample (cellulose powder was not added to prepare the coating). Among them, the sun resistance was determined by the artificial aging resistance test of GB / T 23987-2009. The specific test method is as follows: a 7.5 cm × 7.5 cm (width × length) substrate coated with the coating was placed under a 300 W xenon lamp, the xenon lamp was about 35 cm away from the sample, and the irradiation was started. The experimental time was 10 hours. The xenon lamp was turned off every 1 hour, and the CIE L*a*b* colorimeter was used for measurement and analysis. During the experiment, the fan was always turned on to prevent the irradiation time from being too long and causing the temperature to be too high, thereby affecting the experiment; the water resistance was determined by referring to the coating water resistance determination method of GB / T 1733. The specific test method is as follows: a 7.5 cm × 7.5 cm (width × length) substrate coated with the coating was placed in a water tank and soaked for 72 hours, then taken out and wiped dry, and the substrate was dried according to the product standard (GB / T 1766-2008) inspection sample; cleanability and stain removal ability are tested with reference to GB / T41954-2022 paint and varnish-exterior wall coating on-site quality assessment method. The specific test method is as follows: take a 7.5cm×7.5cm (width×length) substrate coated with paint, apply balsamic vinegar stains / black tea stains according to the standard for 15-20 minutes, then immerse the sponge in the cleaning medium and perform a scrubbing cycle. After the coating surface is dry, measure it, and calculate the cleanability through the three stimulus values ​​in accordance with the CIE 1964 color space to evaluate the stain removal ability. The experimental results show that after the test, the exterior wall paint with the addition of cellulose powder has a stain resistance level that is improved from level 3 to level 1.5 (taking Zhenjiang balsamic vinegar stains as an example) regardless of whether it is coated with balsamic vinegar stains or black tea stains; the adhesion refers to ISO The paint film adhesion test method of 2409:2020 is used for testing. The specific test method is as follows: take a 7.5cm×7.5cm (width×length) substrate coated with paint, put it on the table, cut the designated area with a multi-blade cutting tool, use tape to adhere the cut area, leave it for 5-10s, tear it off immediately, and lightly brush the surface with a brush. Then judge the grade according to the standard. The experimental results show that the introduction of cellulose micropowder with a certain aspect ratio will increase the adhesion between the coating and the substrate.

[0067] Table 1 Color properties of the coatings formed in Examples 1 to 3

[0068] project Lightness (L*) Color uniformity (ΔE) Example 1 88.21 0.88 Example 2 89.92 0.60 Example 3 90.08 0.93

[0069] Table 2 Comparison of coating properties formed in Examples 1 to 3

[0070]

[0071] Comparative Example 1

[0072] The difference between Comparative Example 1 and Example 1 is that only the first cellulose powder is added, and the amount of the first cellulose powder added is the same as the amount of the first cellulose powder and the second cellulose powder added in Example 1. Other experimental parameters are the same as those in Example 1 and will not be repeated here.

[0073] Comparative Example 2

[0074] The difference between Comparative Example 2 and Example 1 is that only the second cellulose powder is added, and the amount of the second cellulose powder added is the same as the amount of the first cellulose powder and the second cellulose powder added in Example 1. Other experimental parameters are the same as those in Example 1 and will not be repeated here.

[0075] Comparative Examples 3 to 6

[0076] The difference between Comparative Examples 3 to 6 and Example 1 is that the particle size and aspect ratio of the first cellulose micropowder and the second cellulose micropowder are different from those in Example 1, and other experimental parameters are the same as those in Example 1, which will not be repeated here. The size characteristics of the first cellulose micropowder and the second cellulose micropowder in Example 1 and Comparative Examples 3 to 6 are shown in Table 3.

[0077] Comparative Examples 7 to 8

[0078] The only difference between Comparative Examples 7 to 8 and Example 1 is that the ratio of the added amount of the first cellulose powder and the second cellulose powder is different from that in Example 1, but the total added amount of the first cellulose powder and the second cellulose powder is the same as that in Example 1, and other experimental parameters are the same as those in Example 1, which will not be repeated here.

[0079] The ratio of the addition amount of the first cellulose micropowder and the second cellulose micropowder in Example 1 and Comparative Examples 7-8 is shown in Table 4. The properties of the coatings prepared in Example 1 and Comparative Examples 1-8 are shown in Table 5. It can be seen from the data in the table that the coating prepared by the method proposed in the present invention has the best performance. This is because: when the first cellulose micropowder and the second cellulose micropowder with specific sizes (particle size, aspect ratio) are mixed in a specific ratio and used as pigments and fillers to prepare the coating, the micropowders meeting the above properties have a larger specific surface area, which is conducive to increasing the contact area between the dye coating and the substrate, and enhancing the bonding between the coating and the substrate. The combined effect improves the stability of the coating during application and avoids the phenomenon of coating shedding or cracking. At the same time, the micropowder retains the polar groups on the cellulose fibers very well. The polar groups can react chemically with the resin to form hydrogen bonds or ester bonds. The above two effects enhance the firmness of the bonding interface between cellulose and the coating substrate. Furthermore, the cellulose fibers obtained by fabric treatment have a certain flexibility and elasticity, which gives the coating formed on the surface of the substrate a certain flexibility and elasticity, and can play a certain buffering role when the coating is subjected to external forces, thereby protecting the coating and the substrate inside it.

[0080] Table 3 Size characteristics of the first cellulose powder and the second cellulose powder in Example 1 and Comparative Examples 3 to 6

[0081]

[0082]

[0083] Table 4 Ratio of the amount of the first cellulose powder to the amount of the second cellulose powder added in Example 1 and Comparative Examples 7-8

[0084]

[0085] Table 5 Comparison of coating properties obtained in Example 1 and Comparative Examples 1-8

[0086]

[0087] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A cellulose micropowder exterior wall paint, characterized in that: The raw materials include: a cellulose micropowder mixture, a silane coupling agent, an acrylate copolymer, a film-forming aid, a leveling agent, a defoaming agent, and a mildew preventer, wherein the cellulose micropowder mixture is obtained by mixing a first cellulose micropowder obtained by micronizing cellulose fibers and a second cellulose micropowder; The mass ratio of the first cellulose micropowder to the second cellulose micropowder is 1:1-1:5, the particle size of the first cellulose micropowder is 3-100 μm, and the aspect ratio is 5:1-30:1, and the particle size of the second cellulose micropowder is 100-500 nm, and the aspect ratio is 1:1-1.5:

1.

2. The cellulose micropowder exterior wall paint according to claim 1, characterized in that: The cellulose micropowder exterior wall paint comprises the following raw materials in parts by weight: 1-5 parts of cellulose micropowder mixture, 5-10 parts of silane coupling agent, 30-40 parts of acrylate copolymer, 15-30 parts of film-forming aid, 2-5 parts of leveling agent, 2-5 parts of defoaming agent and 2-5 parts of mildewproofing agent.

3. The cellulose micropowder exterior wall paint according to claim 2, characterized in that: The silane coupling agent is one of vinyl silane, amino silane, urea silane, amide silane, aminopropyl silane, aryl silane and cationic silane.

4. The cellulose micropowder exterior wall paint according to claim 2, characterized in that: The film-forming aid is one of propylene glycol butyl ether, benzyl alcohol, hexadecene alcohol ester, and dicyclopentenyloxyethyl acrylate; the leveling agent is one of a water-based polyurethane leveling agent, a polyether leveling agent, an acrylate leveling agent, a fluorocarbon leveling agent, and a silicone leveling agent; the defoaming agent is one of a polysiloxane defoaming agent, a polyether defoaming agent, a mineral oil defoaming agent, a magnesium silicate defoaming agent, and an aluminum hydroxide defoaming agent; and the mildew inhibitor is one of biphenyl, o-phenylphenol, ammonium persulfate, calcium phosphate, zinc ions, silver ions, copper ion compounds, and mustard extracts.

5. A method for preparing the cellulose micropowder exterior wall paint according to any one of claims 1 to 4, characterized in that: The steps include: S1. Crush a cellulose fabric with a cutting machine to obtain colored staple fibers, and micronize the colored staple fibers to obtain a first cellulose micropowder slurry and a second cellulose micropowder slurry; dry the first cellulose micropowder slurry and the second cellulose micropowder slurry to obtain a first cellulose micropowder and a second cellulose micropowder, and mix the first cellulose micropowder and the second cellulose micropowder in a mass ratio of 1:1-1:5 to obtain a cellulose micropowder mixture; S2. Evenly mix the cellulose powder mixture obtained in step S1 with a silane coupling agent, an acrylate copolymer, a film-forming aid, a leveling agent, a defoaming agent, and a mildew preventer to obtain a cellulose powder exterior wall coating.

6. The preparation method according to claim 5, characterized in that: In step S1, the micronization treatment is performed as follows: after mixing the colored staple fibers and deionized water, the colored staple fibers are treated with zirconium oxide spheres as ball milling media. After the ball milling is completed, the mixture is cooled to 16-30°C to obtain a first cellulose micropowder slurry or a second cellulose micropowder slurry.

7. The preparation method according to claim 6, characterized in that: In the preparation process of the first cellulose micropowder, the mass ratio of colored staple fibers to deionized water is 1:10-1:30, the size of the zirconium oxide spheres is 6-8 mm, the amount added is 20-25 kg, the ball milling time is 1-6 h, and the rotation speed of the ball milling process is 180-330 rpm.

8. The preparation method according to claim 6, characterized in that: During the preparation of the second cellulose micropowder, the mass ratio of colored staple fibers to deionized water is 1:10-1:30, the size of the zirconium oxide spheres is 2-4 mm, the amount added is 20-25 kg, the ball milling time is 6-12 h, and the rotation speed of the ball milling process is 180-330 rpm.

9. The preparation method according to claim 5, characterized in that: In step S1, during the drying process, the inlet temperature is 180°C, the outlet temperature is 100-130°C, and the flow rate of the first cellulose micropowder slurry and the second cellulose micropowder slurry is 20-40 mL / min.

10. Use of the cellulose micropowder exterior wall paint according to any one of claims 1 to 4 or the cellulose micropowder exterior wall paint prepared by the preparation method according to any one of claims 5 to 9 in the field of construction.

Citation Information

Patent Citations

  • Weather-resistant paint for external walls and preparation method

    CN105273512A

  • Highly-elastic waterproof coating used for walls, and preparation method thereof

    CN107163735A

  • Water-based coating composition and preparation method thereof

    CN115975457A

  • Anticorrosive hydrophobic coating as well as preparation method and application method thereof

    CN117801674A