Swelling adhesive tape for lithium battery and preparation method of swelling adhesive tape
By using a composite structure of modified mica powder and specific adhesive layer in the swelling tape for lithium batteries, the problem of shrinkage and deformation at high temperature in the prior art is solved, effective filling and high temperature stability of the gap of lithium batteries are achieved, and lithium is improved Battery performance and safety.
Patent Information
- Application Number
- CN202411039890.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
AI Technical Summary
Existing swelling tape for lithium batteries is prone to shrink and deform at high temperatures, and cannot effectively fill the gap between the bare battery cell and the cylindrical shell of the lithium battery, affecting the performance and posing safety hazards.
A specific base layer and adhesive layer composite structure is adopted. The base layer contains modified mica powder. The adhesive layer consists of -2-ethylhexyl acrylic acid, methacrylic acid, benzoyl peroxide and polyisocyanate curing agent, through a microconcave Coating technology is prepared to ensure that there is no shrinkage at high temperatures and maintain a high expansion ratio.
The swelling tape for lithium batteries does not shrink at high temperatures, and does not deform after long-term immersion in the electrolyte, which improves high temperature resistance and use stability.
Smart Images

Figure BDA0004972114630000131 
Figure BDA0004972114630000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of swelling tapes, and in particular relates to a swelling tape for lithium batteries and a preparation method thereof. Background Art
[0002] Cylindrical lithium batteries have the advantages of high stability, overcharge resistance, high temperature resistance, and long service life. They are widely used in the preparation of power supplies for mobile phones, digital cameras, MP3s, laptops, car starters, power tools, and other portable electronic products. There is a certain gap between the bare cell and the cylindrical outer shell of the cylindrical lithium battery, which affects the performance of the lithium battery and also creates a great safety hazard. Therefore, it is necessary to bond the bare cell and the cylindrical shell and fill the gap between them. At present, the base material used in the swelling tape for lithium batteries mostly swells in the thickness direction, but it is easy to shrink and deform at high temperatures, and cannot effectively fill the gap between the bare cell and the cylindrical shell of the lithium battery. Summary of the invention
[0003] The object of the present invention is to provide a swelling tape for lithium batteries and a preparation method thereof. The swelling tape can expand at a high rate in an electrolyte and does not shrink at high temperatures, and can be widely used in lithium battery production processes.
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] A swelling tape for a lithium battery comprises a base layer and an adhesive layer, wherein the base layer comprises the following components in parts by weight: 95-98 parts of thermoplastic polyurethane particles, 10-15 parts of polyethersulfone particles, 0.2-0.4 parts of modified mica powder, 0.1-0.3 parts of an antioxidant and 0.2-0.5 parts of a leveling agent; and the adhesive layer comprises the following components in parts by weight: 20-35 parts of 2-ethylhexyl acrylate, 15-25 parts of n-butyl acrylate, 9-15 parts of methacrylic acid, 0.5-1.5 parts of benzoyl peroxide and 0.1-0.6 parts of a polyisocyanate curing agent.
[0006] Furthermore, the antioxidant is BASF antioxidant 5057.
[0007] Furthermore, the leveling agent is BYK9565.
[0008] Furthermore, the polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0009] Furthermore, the preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.5-0.9 parts of silane coupling agent KH550 are added, stirred at 55° C. for 2-4 hours, filtered, and dried to obtain the modified mica powder.
[0010] Furthermore, the particle size of the mica powder is 20-50 μm.
[0011] Furthermore, the volume ratio of the ethanol to water is 2:1.
[0012] The present invention also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0013] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 3-5 hours to obtain a mixed solution;
[0014] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0015] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0016] Furthermore, the thickness of the adhesive layer is 5 μm.
[0017] Furthermore, the thickness of the base layer is 15 μm.
[0018] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: the present invention provides a swelling tape for a lithium battery and a preparation method thereof, which is compounded through a specific base layer and an adhesive layer. The modified mica powder is added to the base layer of the present invention, which has a good effect on improving the high temperature resistance. The adhesive layer is coated on the base layer after mixing 2-ethylhexyl acrylate, hydroxypropyl methacrylate, methacrylic acid, benzoyl peroxide and a polyisocyanate curing agent, and the compatibility of the two is better. The prepared swelling tape for a lithium battery can still maintain a high expansion ratio without shrinking at high temperature, and will not deform after being immersed in an electrolyte for a long time. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] The present embodiment provides a swelling tape for a lithium battery, comprising a base layer and an adhesive layer, wherein the base layer comprises the following components in parts by weight: 96 parts of thermoplastic polyurethane particles, 13 parts of polyethersulfone particles, 0.3 parts of modified mica powder, 0.2 parts of antioxidant and 0.4 parts of leveling agent; the adhesive layer comprises the following components in parts by weight: 30 parts of 2-ethylhexyl acrylate, 17 parts of n-butyl acrylate, 12 parts of methacrylic acid, 1 part of benzoyl peroxide and 0.4 parts of polyisocyanate curing agent.
[0022] The antioxidant is BASF antioxidant 5057.
[0023] The leveling agent is BYK9565.
[0024] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0025] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.7 parts of silane coupling agent KH550 are added, stirred at 55° C. for 3 hours, filtered, and dried to obtain the modified mica powder.
[0026] The particle size of the mica powder is 20-50 μm.
[0027] The volume ratio of the ethanol to water is 2:1.
[0028] This embodiment also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0029] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 4 hours to obtain a mixed solution;
[0030] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0031] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0032] The thickness of the adhesive layer is 5 μm.
[0033] The thickness of the base layer is 15 μm.
[0034] Example 2
[0035] The present embodiment provides a swelling tape for a lithium battery, comprising a base layer and an adhesive layer, wherein the base layer comprises the following components in parts by weight: 95 parts of thermoplastic polyurethane particles, 10 parts of polyethersulfone particles, 0.2 parts of modified mica powder, 0.1 parts of antioxidant and 0.2 parts of leveling agent; the adhesive layer comprises the following components in parts by weight: 20 parts of 2-ethylhexyl acrylate, 15 parts of n-butyl acrylate, 9 parts of methacrylic acid, 0.5 parts of benzoyl peroxide and 0.1 parts of polyisocyanate curing agent.
[0036] The antioxidant is BASF antioxidant 5057.
[0037] The leveling agent is BYK9565.
[0038] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0039] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.5 parts of silane coupling agent KH550 are added, stirred at 55° C. for 2 hours, filtered, and dried to obtain the modified mica powder.
[0040] The particle size of the mica powder is 20-50 μm.
[0041] The volume ratio of the ethanol to water is 2:1.
[0042] This embodiment also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0043] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 3-5 hours to obtain a mixed solution;
[0044] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0045] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0046] The thickness of the adhesive layer is 5 μm.
[0047] The thickness of the base layer is 15 μm.
[0048] Example 3
[0049] The present embodiment provides a swelling tape for a lithium battery, comprising a base layer and an adhesive layer, wherein the base layer comprises the following components in parts by weight: 98 parts of thermoplastic polyurethane particles, 15 parts of polyethersulfone particles, 0.4 parts of modified mica powder, 0.3 parts of an antioxidant, and 0.5 parts of a leveling agent; the adhesive layer comprises the following components in parts by weight: 35 parts of 2-ethylhexyl acrylate, 25 parts of n-butyl acrylate, 15 parts of methacrylic acid, 1.5 parts of benzoyl peroxide, and 0.6 parts of a polyisocyanate curing agent.
[0050] The antioxidant is BASF antioxidant 5057.
[0051] The leveling agent is BYK9565.
[0052] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0053] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.9 parts of silane coupling agent KH550 are added, stirred at 55° C. for 4 hours, filtered, and dried to obtain the modified mica powder.
[0054] The particle size of the mica powder is 20-50 μm.
[0055] The volume ratio of the ethanol to water is 2:1.
[0056] A method for preparing a swelling tape for a lithium battery comprises the following steps:
[0057] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 10 h until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 5 h to obtain a mixed solution;
[0058] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0059] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0060] The thickness of the adhesive layer is 5 μm.
[0061] The thickness of the base layer is 15 μm.
[0062] Comparative Example 1
[0063] The difference between this comparative example and Example 1 is that the raw material composition of the substrate layer is different.
[0064] Specifically: a swelling tape for lithium batteries, comprising a base layer and an adhesive layer, the base layer comprising the following components in parts by weight: 89 parts of thermoplastic polyurethane particles, 23 parts of polyethersulfone particles, 0.2 parts of modified mica powder, 0.3 parts of antioxidant and 0.4 parts of leveling agent; the adhesive layer comprising the following components in parts by weight: 30 parts of 2-ethylhexyl acrylate, 17 parts of n-butyl acrylate, 12 parts of methacrylic acid, 1 part of benzoyl peroxide and 0.4 parts of polyisocyanate curing agent.
[0065] The antioxidant is BASF antioxidant 5057.
[0066] The leveling agent is BYK9565.
[0067] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0068] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.7 parts of silane coupling agent KH550 are added, stirred at 55° C. for 3 hours, filtered, and dried to obtain the modified mica powder.
[0069] The particle size of the mica powder is 20-50 μm.
[0070] The volume ratio of the ethanol to water is 2:1.
[0071] This comparative example also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0072] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 4 hours to obtain a mixed solution;
[0073] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0074] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0075] The thickness of the adhesive layer is 5 μm.
[0076] The thickness of the base layer is 15 μm.
[0077] Comparative Example 2
[0078] The difference between this comparative example and Example 1 is that the base layer does not include polyethersulfone particles.
[0079] Specifically: a swelling tape for lithium batteries, comprising a base layer and an adhesive layer, the base layer comprising the following components in parts by weight: 96 parts of thermoplastic polyurethane particles, 0.3 parts of modified mica powder, 0.2 parts of antioxidant and 0.4 parts of leveling agent; the adhesive layer comprising the following components in parts by weight: 30 parts of 2-ethylhexyl acrylate, 17 parts of n-butyl acrylate, 12 parts of methacrylic acid, 1 part of benzoyl peroxide and 0.4 parts of polyisocyanate curing agent.
[0080] The antioxidant is BASF antioxidant 5057.
[0081] The leveling agent is BYK9565.
[0082] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0083] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.7 parts of silane coupling agent KH550 are added, stirred at 55° C. for 3 hours, filtered, and dried to obtain the modified mica powder.
[0084] The particle size of the mica powder is 20-50 μm.
[0085] The volume ratio of the ethanol to water is 2:1.
[0086] This comparative example also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0087] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 4 hours to obtain a mixed solution;
[0088] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0089] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0090] The thickness of the adhesive layer is 5 μm.
[0091] The thickness of the base layer is 15 μm.
[0092] Comparative Example 3
[0093] The difference between this comparative example and Example 1 is that the mica powder is not modified.
[0094] Specifically: a swelling tape for lithium batteries, comprising a base layer and an adhesive layer, the base layer comprising the following components in parts by weight: 96 parts of thermoplastic polyurethane particles, 13 parts of polyethersulfone particles, 0.3 parts of mica powder, 0.2 parts of antioxidant and 0.4 parts of leveling agent; the adhesive layer comprising the following components in parts by weight: 30 parts of 2-ethylhexyl acrylate, 17 parts of n-butyl acrylate, 12 parts of methacrylic acid, 1 part of benzoyl peroxide and 0.4 parts of polyisocyanate curing agent.
[0095] The antioxidant is BASF antioxidant 5057.
[0096] The leveling agent is BYK9565.
[0097] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0098] The particle size of the mica powder is 20-50 μm.
[0099] The volume ratio of the ethanol to water is 2:1.
[0100] This comparative example also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0101] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 4 hours to obtain a mixed solution;
[0102] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0103] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0104] The thickness of the adhesive layer is 5 μm.
[0105] The thickness of the base layer is 15 μm.
[0106] Comparative Example 4
[0107] The difference between this comparative example and Example 1 is that the particle size of the mica powder is 100-200 μm.
[0108] Specifically: a swelling tape for lithium batteries, comprising a base layer and an adhesive layer, the base layer comprising the following components in parts by weight: 96 parts of thermoplastic polyurethane particles, 13 parts of polyethersulfone particles, 0.3 parts of modified mica powder, 0.2 parts of antioxidant and 0.4 parts of leveling agent; the adhesive layer comprising the following components in parts by weight: 30 parts of 2-ethylhexyl acrylate, 17 parts of n-butyl acrylate, 12 parts of methacrylic acid, 1 part of benzoyl peroxide and 0.4 parts of polyisocyanate curing agent.
[0109] The antioxidant is BASF antioxidant 5057.
[0110] The leveling agent is BYK9565.
[0111] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0112] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.7 parts of silane coupling agent KH550 are added, stirred at 55° C. for 3 hours, filtered, and dried to obtain the modified mica powder.
[0113] The particle size of the mica powder is 100-200 μm.
[0114] The volume ratio of the ethanol to water is 2:1.
[0115] This comparative example also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0116] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 4 hours to obtain a mixed solution;
[0117] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0118] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0119] The thickness of the adhesive layer is 5 μm.
[0120] The thickness of the base layer is 15 μm.
[0121] Comparative Example 5
[0122] The difference between this comparative example and Example 1 is that the raw material composition of the adhesive layer is different.
[0123] Specifically: a swelling tape for lithium batteries, comprising a base layer and an adhesive layer, the base layer comprising the following components in parts by weight: 96 parts of thermoplastic polyurethane particles, 13 parts of polyethersulfone particles, 0.3 parts of modified mica powder, 0.2 parts of antioxidant and 0.4 parts of leveling agent; the adhesive layer comprising the following components in parts by weight: 20 parts of 2-ethylhexyl acrylate, 30 parts of hydroxypropyl acrylate, 6 parts of acrylic acid, 1 part of benzoyl peroxide and 0.4 parts of polyisocyanate curing agent.
[0124] The antioxidant is BASF antioxidant 5057.
[0125] The leveling agent is BYK9565.
[0126] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0127] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.7 parts of silane coupling agent KH550 are added, stirred at 55° C. for 3 hours, filtered, and dried to obtain the modified mica powder.
[0128] The particle size of the mica powder is 20-50 μm.
[0129] The volume ratio of the ethanol to water is 2:1.
[0130] This comparative example also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0131] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 4 hours to obtain a mixed solution;
[0132] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0133] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0134] The thickness of the adhesive layer is 5 μm.
[0135] The thickness of the base layer is 15 μm.
[0136] Comparative Example 6
[0137] The difference between this comparative example and Example 1 is that the raw materials and composition of the adhesive layer are different.
[0138] Specifically: a swelling tape for lithium batteries, comprising a base layer and an adhesive layer, the base layer comprising the following components in parts by weight: 96 parts of thermoplastic polyurethane particles, 13 parts of polyethersulfone particles, 0.3 parts of modified mica powder, 0.2 parts of antioxidant and 0.4 parts of leveling agent; the adhesive layer comprising the following components in parts by weight: 15 parts of 2-ethylhexyl acrylate, 35 parts of n-butyl acrylate, 6 parts of methacrylic acid, 0.5 parts of benzoyl peroxide and 0.6 parts of polyisocyanate curing agent.
[0139] The antioxidant is BASF antioxidant 5057.
[0140] The leveling agent is BYK9565.
[0141] The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
[0142] The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.7 parts of silane coupling agent KH550 are added, stirred at 55° C. for 3 hours, filtered, and dried to obtain the modified mica powder.
[0143] The particle size of the mica powder is 20-50 μm.
[0144] The volume ratio of the ethanol to water is 2:1.
[0145] This comparative example also provides a method for preparing a swelling tape for a lithium battery, comprising the following steps:
[0146] (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 4 hours to obtain a mixed solution;
[0147] (2) coating the mixed solution on a PET release film at a temperature of 130° C. and a coating speed of 8 m / min; drying and removing the PET release film to obtain a base layer.
[0148] (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
[0149] The thickness of the adhesive layer is 5 μm.
[0150] The thickness of the base layer is 15 μm.
[0151] Performance Testing
[0152] The swellable adhesive tapes for lithium batteries prepared in Examples 1-3 and Comparative Examples 1-6 were cut into samples with a length of 55 mm and a width of 58 mm, and immersed in an electrolyte at 100°C for 5 hours to observe their swelling and shape retention capabilities. According to the "Test Method for Tensile Strength and Elongation at Break, GB / T30776-2014 Edition", the swellable adhesive tapes for lithium batteries prepared in Examples 1-3 and Comparative Examples 1-6 were cut into samples with a width of 10 mm and a length of 200 mm, and the spacing between the samples in the tensile machine was 100 mm to measure the tensile force and swelling rate.
[0153] Table 1 Performance test results
[0154]
[0155]
[0156] It can be seen from Examples 1-3 that the swelling tape for lithium batteries prepared by the present invention has good comprehensive performance in terms of swelling state and swelling rate. It can be seen from Comparative Examples 1-6 that the comprehensive performance decreases to varying degrees when the raw materials and composition of the preparation are changed.
[0157] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A swelling tape for lithium batteries, comprising a base layer and an adhesive layer, characterized in that: The base layer comprises the following components in parts by weight: 95-98 parts of thermoplastic polyurethane particles, 10-15 parts of polyethersulfone particles, 0.2-0.4 parts of modified mica powder, 0.1-0.3 parts of antioxidant and 0.2-0.5 parts of leveling agent; the adhesive layer comprises the following components in parts by weight: 20-35 parts of 2-ethylhexyl acrylate, 15-25 parts of n-butyl acrylate, 9-15 parts of methacrylic acid, 0.5-1.5 parts of benzoyl peroxide and 0.1-0.6 parts of polyisocyanate curing agent.
2. A swelling tape for lithium batteries according to claim 1, characterized in that: The antioxidant is BASF antioxidant 5057.
3. A swelling tape for lithium batteries according to claim 1, characterized in that: The leveling agent is BYK9565.
4. A swelling tape for lithium batteries according to claim 1, characterized in that: The polyisocyanate curing agent is 1,6-hexamethylene diisocyanate trimer.
5. The swelling tape for lithium battery according to claim 1, characterized in that: The preparation method of the modified mica powder is as follows: by weight, 10 parts of mica powder are added to a mixture of 30 parts of ethanol and water, 0.5-0.9 parts of silane coupling agent KH550 are added, the mixture is stirred at 55° C. for 2-4 hours, filtered, and dried to obtain the modified mica powder.
6. A swelling tape for lithium batteries according to claim 5, characterized in that: The particle size of the mica powder is 20-50 μm.
7. A swelling tape for lithium batteries according to claim 5, characterized in that ,, the volume ratio of ethanol to water is 2:
1.
8. The method for preparing the swelling tape for lithium battery according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) adding thermoplastic polyurethane particles and polyethersulfone particles to N,N-dimethylformamide and heating to 95° C., stirring for 6-10 hours until the particles are completely dissolved, and then adding modified mica powder, antioxidant and leveling agent, stirring at 35° C., stirring at a speed of 500 rpm / min, and stirring for 3-5 hours to obtain a mixed solution; (2) coating the mixed solution on the PET release film at a temperature of 130°C and a coating speed of 8 m / min; Drying, removing the PET release film, and obtaining the base layer. (3) Mix the raw materials of the adhesive layer, apply them on the base layer by micro-concave coating, dry them, and obtain a swelling tape for lithium battery, which is then laminated to the surface of the base film to prepare a swelling tape.
9. The method for preparing the swelling tape for lithium battery according to claim 8, characterized in that: The thickness of the adhesive layer is 5 μm.
10. The method for preparing the swelling tape for lithium battery according to claim 8, characterized in that: The thickness of the base layer is 15 μm.