CuNiAl alloy electroslag remelting preparation method

The impurities and shrinkage defects in CuNiAl alloy are removed through the electroslag remelting process, and the problem of unstable alloy performance in the vacuum induction smelting process is solved, and the preparation of CuNiAl alloys with high purity and high performance is achieved, suitable for precision manufacturing and high-temperature environments .

CN118932197APending Publication Date: 2024-11-12DALIAN JIAOTONG UNIVERSITY

Patent Information

Application Number
CN202410944801.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The vacuum induction smelting process cannot effectively remove impurities and shrinkage defects in CuNiAl alloy, resulting in unstable high-temperature performance of the alloy.

Method used

The electroslag remelting process is adopted to generate heat in the slag material through current and gradually melt the consumable electrode. It is refined using a slag pool to remove impurities and form a high-purity CuNiAl alloy ingot.

Benefits of technology

It significantly reduces the hole size in the alloy, improves hardness and tensile strength, enhances the durability and high-temperature performance stability of the alloy, and meets the needs of precision manufacturing and high-performance materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004945310440000011
    Figure HDA0004945310440000011
  • Figure HDA0004945310440000012
    Figure HDA0004945310440000012
  • Figure HDA0004945310440000021
    Figure HDA0004945310440000021
Patent Text Reader

Abstract

The invention discloses an electroslag remelting and refining preparation method of a CuNiAl alloy. An electroslag remelting (ESR) method is adopted. According to the method, a consumable electrode is melted through resistance heat generated when current penetrates through slag, refining is conducted through a slag pool, and finally the consumable electrode is condensed into a cast ingot in a water-cooling crystallizer. The technology aims at solving the problems of shrinkage cavities and looseness of a CuNiAl alloy cast ingot after vacuum induction melting, and the alloy purity is effectively improved. Experimental results show that the electroslag remelting process can significantly reduce the hole size in the alloy, improve the as-cast average hardness and high-temperature hardness, and maintain good tensile deformation capacity at high temperature. The preparation method is efficient and reliable, is suitable for preparing the CuNiAl alloy with stable performance and high purity, and has wide application prospects in the fields of precision manufacturing, aerospace, nuclear energy and the like with high requirements for material performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electroslag remelting preparation process of a CuNiAl alloy, which is suitable for application scenarios such as engine high-temperature combustion chambers and brake pads for flying cars. The alloy has excellent high-temperature resistance and self-lubricating properties. The alloy is prepared by an electroslag remelting process to improve metal purity and related properties. Background Art

[0002] CuNiAl alloy (also known as nickel aluminum bronze, NAB), in which the main strengthening phases are martensitic β phase (based on Cu3Al) and κ phase with shape memory effect, among which κi, κii, κiv phases (based on Fe3Al) are rich in iron, and κiii phase (based on NiAl) is rich in nickel. The alloy is often prepared by vacuum induction melting (VIM). In order to precipitate more multi-γ′ or γ" strengthening phases, more Al is added as a strengthening element during the smelting process. However, Al is a volatile element and will cause great burn loss when smelted under atmospheric conditions. Therefore, it is more suitable for vacuum induction melting. However, vacuum induction melting cannot effectively solve the reaction between the melt and the melting crucible at high temperature, and it is difficult to remove impurity elements such as S, P, and C, as well as defects such as shrinkage cavities and looseness inside the ingot. Therefore, it is necessary to carry out electroslag remelting on the basis of vacuum induction melting.

[0003] As a remelting process, electroslag remelting (ESR) can regulate the solidification structure of the alloy and further reduce the impurity content of the alloy. Electroslag remelting is a smelting method developed from electroslag welding technology in the 1950s, and was widely used in smelting metallurgy and other fields in the 1970s and 1980s by countries around the world (Duan Shengchao. Basic research on oxidation control of alloy elements in large IN718 nickel-based alloy ingots by electroslag remelting [D]. Beijing University of Science and Technology, 2021.). The basic principle of electroslag remelting is that when the current passes through the slag, a large amount of heat will be generated due to the large resistance of the slag. The slag is used to resist heat and gradually melt the electrodes that need to be remelted. The molten metal is purified through the slag in the form of droplets, and finally solidified from bottom to top in a water-cooled crystallizer.

[0004] The parameters of slag system selection, proportion and dosage of electroslag remelting (ESR) have a decisive influence on the electroslag smelting process and the quality of electroslag ingots. There are a series of slag-metal reactions in the process of contact between the metal droplet and the liquid slag, and the slag-metal contact area can reach 3200mm 2 / g or above, which allows non-metallic inclusions and harmful elements such as S, P, and Sb in the metal droplets to be absorbed and removed by the slag, while easily oxidizable elements such as Al and Ti fully react with the oxides in the slag, thereby achieving good control of the cleanliness of the alloy (Liu Y, Wang Y, Li G, et al. Investigation on the structure, fluo-ride vaporization and crystallization behavior of CaF2–CaO–Al2O3–(SiO2) slag for electroslag remelting[J]. Journal of Thermal Analysis and Calorimetry, 2020, 139(2): 923-931.).

[0005] In view of this, the present invention introduces the electroslag remelting (ESR) process to eliminate the problem of contamination of the alloy melt caused by the reaction between the molten metal and the crucible material during the smelting process of the CuNiAl alloy, and the problem of large shrinkage holes in the vacuum ingot produced by the inability to perform shrinkage compensation during the casting process. The preparation process can ensure the improvement of the alloy purity, effectively control the defects caused by smelting, and effectively improve the performance. Summary of the invention

[0006] The object of the present invention is to provide a new preparation process of CuNiAl alloy, which adopts the electroslag remelting (ESR) method, utilizes the resistance heat generated by the current passing through the slag to melt the consumable electrode, and makes the molten metal drip and then pass through the slag pool to achieve the purpose of refining. After passing through the slag pool, the metal droplets enter the water-cooled crystallizer and condense into an ingot, which can better improve the organizational properties of the ingot and remove the inclusions in the alloy; the method focuses on solving the defects of the CuNiAl alloy ingot after vacuum induction melting, such as more shrinkage cavities and looseness, and effectively improves the purity of the alloy. It can solve the shortcomings of the high-temperature performance instability caused by the presence of more shrinkage cavities in the CuNiAl alloy. Through the preparation method of this patent, a CuNiAl alloy with stable performance and high purity can be obtained, with high preparation efficiency, which can meet different processing requirements. These optimization effects make the electroslag remelting CuNiAl alloy have broad application prospects in fields with high requirements for material performance, such as precision manufacturing, aerospace, and nuclear energy.

[0007] Specifically, the CuNiAl alloy electroslag remelting and refining method of the present invention comprises the following steps:

[0008] a. preparing and smelting a CuNiAl alloy raw material to form an original ingot, wherein the composition of the CuNiAl alloy ranges from 50 to 60wt% Cu, 35 to 45wt% Ni, and 3 to 8wt% Al;

[0009] b. processing the original ingot into a consumable electrode having an electrode size suitable for electroslag remelting equipment and surface treatment to improve remelting efficiency;

[0010] c. Select slag with a melting point 100-300°C lower than that of CuNiAl alloy and conduct pre-drying treatment at a temperature of 600-800°C for no less than 4 hours;

[0011] d. Preparation of furnace environment: evacuate the furnace to an absolute pressure of less than 20Pa, fill it with argon gas to an absolute pressure between 100 and 500Pa, and create an inert atmosphere;

[0012] e. Electroslag remelting: Under the above step d environment, the applied current intensity is 3500±200A, and the holding time is 15 to 35 minutes to complete the electroslag remelting process of the alloy, and a high-purity CuNiAl alloy ingot is formed through slag pool refining, impurity removal and recasting.

[0013] For the technical solution described above, it is further preferred that the current is maintained at 3500±50A during the electroslag remelting process.

[0014] For the technical solution described above, it is further preferred that the holding time during the electroslag remelting process is at least 20 minutes.

[0015] For the technical solution described above, it is further preferred that the consumable electrode has a diameter of 150-250 mm, a length of 1000-2000 mm, and a surface roughness Ra≤1.6 μm. It is further preferred that the diameter is 150-200 mm and the length is 1500 mm.

[0016] For the technical solution described above, it is further preferred that the step a is to place the copper and nickel raw materials at 10 -3 ~10 -2 Pa vacuum, preheat treatment for 5 to 15 minutes, introduce argon atmosphere, heat until Cu and Ni are completely melted, maintain the molten state for 5 to 15 minutes to fully homogenize the matrix; add aluminum element and mix thoroughly, and perform insulation treatment for 2 to 5 minutes for mold casting. This process design focuses on strengthening the preheating and key insulation steps, and improves the comprehensive performance and structural consistency of alloy products by accurately controlling time and vacuum degree.

[0017] For the technical solution described above, it is further preferred that the surface roughness of the consumable electrode Ra≤0.8 μm.

[0018] For the technical solution described above, it is further preferred that the drying condition is 700±100° C. and the drying time is at least 5 hours.

[0019] For the technical solution described above, it is further preferred that the vacuum degree in the furnace is 3×10 -3 Pa, then preheat for at least 5 minutes and fill with argon to an absolute pressure of 200 Pa.

[0020] For the technical solution described above, it is further preferred that the slag material is selected from CaF2-Al2O3 slag system. The beneficial effects of the present invention compared with the prior art are as follows:

[0021] 1. Pore reduction and optimization:

[0022] The average pore area of ​​CuNiAl ingots cast by vacuum induction melting is 5.74 μm 2 , most of the pores are between 0 and 10 μm in size 2 After electroslag remelting, the average pore area of ​​the alloy was reduced to 0.93μm 2 , and 95.92% of the pores have a diameter of 2μm 2 This data shows that electroslag remelting technology can significantly reduce the size of pores in the alloy and improve the density and performance of the alloy.

[0023] 2. Hardness improvement:

[0024] The average as-cast hardness of the vacuum induction melted CuNiAl alloy is 331.6HV. After electroslag remelting, the average as-cast hardness increases to 342.2HV, showing a significant increase in hardness. This increase indicates that the alloy after electroslag remelting has higher strength and wear resistance.

[0025] 3. Improved strength and plasticity:

[0026] The cast tensile strength of the vacuum induction melted CuNiAl alloy is 384.2MPa and the strain is 0.66%. After electroslag remelting, the tensile strength is increased to 803.8MPa and the strain is increased to 2.46%, showing a significant improvement in strength and plasticity. This improvement indicates that the alloy composition after electroslag remelting is more uniform, the pore size inside the alloy is reduced, and the durability of the alloy is enhanced.

[0027] 4. High temperature hardness maintenance:

[0028] In the high temperature test, the hardness of the vacuum induction melted samples dropped rapidly after 700°C. In contrast, the electroslag remelted samples can still maintain a higher hardness value under the same conditions. This data proves that the electroslag remelting technology has a stronger ability to maintain the hardness of the material under high temperature environment and is suitable for applications in high temperature working environments.

[0029] 5. High temperature tensile deformation capacity:

[0030] The electroslag remelted samples showed good deformation ability in the high temperature tensile test. Although the tensile strength and plasticity decreased with the increase of temperature, they still maintained a certain performance stability at 500-600°C. This result shows that the method of the present invention can improve the deformation ability of the alloy at high temperature and broaden its application range. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Porosity statistics of CuNiAl alloy after vacuum induction melting, where the X-axis is the pore size and the Y-axis is the frequency of occurrence.

[0032] Figure 2 The porosity statistics of CuNiAl alloy after electroslag remelting, where the X-axis is the pore size and the Y-axis is the frequency of occurrence.

[0033] Figure 3 Comparative test results of room temperature hardness of vacuum induction melting and electroslag remelting samples.

[0034] Figure 4 Comparative test results of as-cast room temperature tensile properties of CuNiAl samples after vacuum induction melting and electroslag remelting.

[0035] Figure 5 Comparative test results of high temperature hardness of vacuum induction melting and electroslag remelting samples.

[0036] Figure 6 This is a test diagram of the high-temperature tensile properties of the electroslag remelted sample. DETAILED DESCRIPTION

[0037] The following examples will further illustrate the present invention.

[0038] The composition of CuNiAl alloy is:

[0039] element Cu Ni Al wt / % 50~60 35~45 3~8

[0040] Embodiment 1:

[0041] The preparation method of the CuNiAl alloy involved in this experiment is:

[0042] High-purity metal materials are used and the ingredients are prepared according to mass percentage, and the raw materials are electrically pure copper (99.9wt%), electrically pure nickel (99.9wt%), and electrically pure aluminum (99.9wt%). A high-purity graphite crucible is selected to prepare the alloy in a vacuum induction melting furnace.

[0043] During the operation of this embodiment, the CuNiAl alloy ingot contains 55.59wt% of electro-pure copper, 38.51wt% of electro-pure nickel and 5.9wt% of electro-pure aluminum.

[0044] During the smelting process, the Cu block and the Ni block are placed in a crucible and the vacuum is drawn to 3×10 -3 Pa, preheat the crucible and raw materials at a lower power, fill with argon after preheating for 10 minutes. Then increase the power until the Cu block and Ni block melt, keep them warm for 10 minutes at the current power, then add the Al block, keep warm for 3 minutes to ensure uniformity, and finally keep the current power to cast into a high-purity graphite mold.

[0045] The furnace cooling method is adopted to obtain more γ′(Ni3Al) phase. The CuNiAl ingot obtained after vacuum induction melting is then used as electrode material, and is turned into a consumable electrode with a diameter of 150mm and a length of 1500mm. The electrode surface is finely polished before electroslag remelting.

[0046] When selecting slag, the melting point of the slag system should be 100 to 200°C lower than that of the CuNiAl alloy. The slag system should be selected as the CaF2-Al2O3 slag system, which is a common electroslag remelting slag system for nickel-based high-temperature alloys. A pre-melted slag of 50% CaF2-25% Al2O3-25% CaO is used, and the slag is placed in a muffle furnace for drying for 6 hours before use. The drying temperature is 700°C. Before starting, the air in the furnace body is extracted by a vacuum pump, and the absolute pressure in the furnace body is less than 10Pa. Then argon gas is filled in so that the vacuum degree in the furnace body reaches an absolute pressure of 200Pa, forming an inert atmosphere remelting environment. Under this condition, arcing, slag melting, and smelting are completed. During the melting process, a current of 3500A is maintained, and the insulation time is 25min.

[0047] Comparative Example 1

[0048] The vacuum melting method of CuNiAl alloy is the same as that of Example 1, and the electroslag remelting method is not adopted. The cast state is stretched at room temperature and the strength is compared with that of the sample after electroslag remelting. Figure 4 It can be seen that after electroslag remelting, the mechanical properties of the material have been greatly improved.

[0049] Comparative Example 2

[0050] The vacuum melting method of CuNiAl alloy is the same as that of Example 1, but during the electroslag remelting process, the current of 3500 A maintained during the melting process of the alloy is reduced to 3300 A. It is found by comparison that after reducing the current by 200 A, the surface quality of the electroslag ingot is not much different, and the performance is similar.

[0051] Comparative Example 3

[0052] The vacuum melting method of the CuNiAl alloy is the same as that of Example 1, but during the electroslag remelting process, the current of 3500A maintained during the melting process of the alloy is increased to 3700A. By comparison, it is found that although the surface morphology does not change much after the current is increased, the performance is similar.

[0053] After exploring two different current intensities during electroslag remelting, the mechanical properties are shown in Table 1. The current intensity range applied during electroslag remelting of CuNiAl alloy is: 3500±200 (A).

[0054] Table 1. Comparison of electroslag ingot performance under different currents

[0055] Comparative Example 2 Example 1 Comparative Example 3 Current (A) 3300 3500 3700 Hardness (HV) 337.5 342.2 335.6 Tensile strength(MPa) 789.7 803.8 775.4

[0056] From the data in Table 1, it can be seen that when the current intensity is 3500A, the hardness and tensile strength of the alloy reach 342.2HV and 803.8MPa respectively, which is the highest value among the three current intensities tested (3300A, 3500A, 3700A). Compared with the hardness of 337.5HV and tensile strength of 789.7MPa at 3300A, and the hardness of 335.6HV and tensile strength of 775.4MPa at 3700A, the performance improvement at 3500A is not only a conventional improvement, but a significant improvement, because it exceeds the performance of adjacent current intensity levels and is determined as the central value of a narrower optimal current intensity range (3500±50A), which has important guiding significance in actual production.

[0057] Effect example

[0058] The organizational structure and performance analysis method of the CuNiAl alloy involved in this application are:

[0059] The as-cast samples were metallographically prepared, and the microscopic morphology of the samples was preliminarily observed using a light microscope. The organizational structure of the samples was observed in detail using a transmission electron microscope, and a dispersed granular precipitate phase was observed. The phase composition of the alloy was analyzed using an X-ray diffractometer, and combined with TEM-EDS analysis, the second phase in the alloy was mainly γ′ (Ni3Al) phase. The tensile strength of the samples was tested using a universal testing machine; and the high-temperature hardness test of the samples was performed using an in-situ hardness tester.

[0060] The measured performance is as follows:

[0061] 1. Porosity analysis

[0062] Depend on Figure 1 It can be seen that the average area of ​​the pores in the CuNiAl ingot cast by conventional vacuum induction melting is 5.74 μm. 2 , of which 55.25% are 0~5μm2 Holes of size: 28.76% are 5 to 10 μm 2 Size holes.

[0063] And by Figure 2 It can be seen that after electroslag remelting, the pores of CuNiAl alloy appear most frequently in the particle size range of about 0.6 microns to 1.2 microns. As the pore size increases (from 1.2 microns to 11 microns), the frequency of pores gradually decreases. The average area of ​​the pores is 0.93μm 2 , of which 65.69% are 0~1μm 2 Holes of size: 30.23% are 1 to 2 μm 2 Compared with the CuNiAl alloy produced by vacuum induction melting, 95.92% of the holes in this alloy are 2μm in diameter. 2 Below, there is a clear optimization performance of void reduction, proving that the larger pores are gradually eliminated or reduced by electroslag remelting.

[0064] 2. Casting average hardness test

[0065] Depend on Figure 3 It can be seen that the average as-cast hardness of the CuNiAl alloy melted by vacuum induction melting is 331.6 HV, while the average as-cast hardness after electroslag remelting is 342.2 HV.

[0066] 3. Normal temperature casting stretching

[0067] Depend on Figure 4 It can be seen that the tensile strength of the CuNiAl alloy melted by vacuum induction is 384.2MPa and the strain is only 0.66%. After the electroslag remelting process, the composition of the material is more uniform and the size of the pores in the alloy is effectively reduced, which greatly improves the performance. The tensile strength is increased to 803.8MPa and the strain is also increased to 2.46%.

[0068] 4. High temperature hardness test

[0069] The two groups of samples were subjected to high temperature hardness tests, with the temperature ranging from 100℃ to 1000℃, and the test was carried out at 100℃ intervals. Figure 5 It can be seen that at low temperatures (such as below 200°C), the hardness values ​​of the two processes are relatively high and close, which may be because the internal structure of the material is relatively stable at this time, and the temperature change has little effect on the hardness. However, as the temperature gradually increases, the hardness values ​​of the two processes begin to decrease to varying degrees. In particular, the softening temperature of the vacuum induction melting and electroslag remelting cast samples is maintained at 700°C, but after 700°C, the hardness of the vacuum induction melting sample decreases rapidly with the increase of temperature, while the electroslag remelting sample can still maintain the hardness of the sample.

[0070] In addition, it can be seen from the figure that under the same temperature conditions, the hardness values ​​of the electroslag remelted samples are generally higher than those of the vacuum induction melted samples. This proves that the electroslag remelted materials are less affected by heat and can form a more uniform and dense grain structure, thereby improving the hardness and strength of the material.

[0071] In summary, Figure 5 The content proves that under high temperature conditions, the electroslag remelting process has certain advantages over the vacuum induction melting process in maintaining material hardness. This has important practical significance and application value for metal materials that require a high temperature working environment.

[0072] 5. High temperature cast tensile test

[0073] The electroslag remelted samples were subjected to high temperature tensile tests at temperatures ranging from 100°C to 800°C, with the samples being kept warm at 100°C intervals and tested. Figure 6 The tensile properties test results of the electroslag remelted samples at high temperatures are shown. According to the curve graph given, we can clearly see that as the temperature increases, the percentage of engineering strain that the material can withstand is also gradually increasing. This phenomenon reflects the deformation ability of the material in a high temperature environment. As the temperature of the electroslag remelted sample increases, the tensile strength and plasticity are constantly decreasing, but it can still maintain a certain performance stability at 500℃ to 600℃, which has been a significant improvement.

[0074] From the specific numerical value, when the temperature increases from 0℃ to 200℃, the engineering strain increases from almost no change to an engineering strain value corresponding to about 600MPa. Subsequently, as the temperature continues to rise, the engineering strain still increases, but the rate of increase gradually slows down. At 300℃, the engineering strain decreases to a value corresponding to 400MPa; at 400℃, it further decreases to 300MPa; at 600℃, it is about 200MPa; at 700℃, it is close to 180MPa, and finally stabilizes at about 100MPa at 800℃.

[0075] This trend indicates that as the temperature increases, the elastic modulus of the material in the tensile test decreases, allowing greater deformation without fracture. At the same time, the changes in the internal microstructure of the material at high temperature may also affect its mechanical properties.

[0076] In short, by Figure 6 It can be seen that the electroslag remelted samples have good tensile deformation capacity at high temperatures, and their engineering strain increases with increasing temperature. This property is of great significance for the use of materials in high temperature environments, especially in application scenarios that need to withstand large deformation without breaking.

[0077] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing CuNiAl alloy by electroslag remelting and refining, It is characterized in that The following steps are involved: a. preparing and smelting a CuNiAl alloy raw material to form an original ingot, wherein the CuNiAl alloy has a Cu content of 50 to 60wt%, a Ni content of 35 to 45wt%, and an Al content of 3 to 8wt%; b. processing the original ingot into a consumable electrode and performing surface treatment; c. Select slag with a melting point 100-300°C lower than that of CuNiAl alloy and conduct pre-drying treatment at a temperature of 600-800°C for no less than 4 hours; d. Preparation of furnace environment: evacuate the furnace to an absolute pressure of less than 20Pa, fill it with argon gas to an absolute pressure between 100 and 500Pa, and create an inert atmosphere; e. Electroslag remelting: Under the above step d environment, the applied current intensity is 3500±200A, and the holding time is 15 to 35 minutes to complete the electroslag remelting process of the alloy, through slag pool refining, impurity removal and recasting.

2. The method according to claim 1, It is characterized in that The current is maintained at 3500±50A during the electroslag remelting process.

3. The method according to claim 1, It is characterized in that The consumable electrode has a diameter of 150-250 mm, a length of 1000-2000 mm, and a surface roughness Ra≤1.6 μm.

4. The method according to claim 1, It is characterized in that Step a is to place the copper and nickel raw materials at 10 -3 ~10 -2 Pa vacuum, preheat treatment for 5 to 15 minutes, introduce argon atmosphere, heat until Cu and Ni are completely melted, maintain the molten state for 5 to 15 minutes to fully uniform the matrix; add aluminum element and mix thoroughly, and perform insulation treatment for 2 to 5 minutes for mold casting.

5. The method according to claim 1, It is characterized in that The surface roughness of the consumable electrode is Ra≤0.8 μm.

6. The method according to claim 1, It is characterized in that The drying condition is 700±50° C. and the drying time is at least 5 hours.

7. The method according to claim 1, It is characterized in that The vacuum degree in the furnace is 3×10 -3 Pa, then preheat for at least 5 minutes and fill with argon to an absolute pressure of 200 Pa.

8. The method according to claim 1, It is characterized in that The holding time during the electroslag remelting process is at least 20 minutes.

9. The method according to any one of claims 1 to 8, It is characterized in that The slag material is selected from CaF 2 -Al 2 O 3 Trash system.

Citation Information

Patent Citations

  • Electroslag remelting slag for nickel aluminum bronze

    CN101285125A

  • Cu-Ni-Al alloy powder and preparation method thereof

    CN102489700A

  • Method for preparing high-performance CuMnNi alloy through duplex process

    CN116623022A

Cited By

  • Rare earth CuNiAl alloy and preparation method and application thereof

    CN121065531A