Laser shock peening method for connecting hole of thin-wall structural part

By setting a rigid mandrel and a pad in the connection hole of thin-walled structural parts, the interface waves are generated by laser shock for strengthening, the fatigue failure problem of thin-walled structural parts connection holes under fatigue loads in the prior art is solved, and the hole is realized Efficient reinforcement of walls and surfaces ensures improved pore accuracy and fatigue life.

CN118932265AActive Publication Date: 2024-11-12SUZHOU LAIKU AVIATION EQUIP TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410955206.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-12
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

In the prior art, thin-walled structural parts connection holes are prone to fatigue failure under fatigue loads. The extrusion strengthening method causes overall deformation when the thickness of some wall panels is small. Laser impact strengthening can only strengthen the hole surface, and When the aperture is less than 3mm, the mandrel is prone to breaking, and the hole wall cannot be effectively strengthened, affecting the hole accuracy.

Method used

By using the laser impact enhancement method, by setting a rigid mandrel and a pad in the connection hole, the focusing laser beam is aligned with the irradiation point, the interface wave is generated to make the hole wall squeeze strengthen, and the reverse is suppressed by the pad with low wave impedance. Deform the direction to ensure the accuracy of the hole position.

Benefits of technology

It effectively improves the fatigue performance of the connecting holes, avoids overall deformation caused by extrusion strengthening and laser impact strengthening of peri-hole collapse, ensures hole accuracy, and can be strengthened when the hole diameter is less than 3mm, significantly improving the fatigue life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932265A_ABST
    Figure CN118932265A_ABST
Patent Text Reader

Abstract

The invention provides a laser shock peening method for a connecting hole of a thin-wall structural part, which comprises the following steps: placing the thin-wall structural part with the connecting hole on a cushion block, arranging a rigid mandrel in the connecting hole, sequentially arranging a restraint layer and an absorption layer at the top of the cushion block from top to bottom, and at least covering the connecting hole by the restraint layer and the absorption layer along the longitudinal direction; a plurality of irradiation points are symmetrically and uniformly arranged at the edge of the connecting hole by taking the center of the connecting hole as a symmetric center, and the focused laser beams penetrate through the restraint layer at the top of the restraint layer and are sequentially aligned with the two symmetric irradiation points in the longitudinal direction so as to sequentially irradiate the absorption layer. By means of the method, the fatigue performance of the hole structure is improved, and deformation of the thin-wall structural part can be prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser processing, and in particular to a laser shock strengthening method for connecting holes of thin-walled structural parts. Background Art

[0002] Thin-walled structural parts are usually made of thin plates and thin shells. Typical thin-walled structural parts include blades and aircraft panels. Taking aircraft panels as an example, a large number of connection holes need to be opened during the manufacturing and use of aircraft panels. Based on this, factors that are not conducive to their fatigue performance will occur during use. Specifically, during the high-speed flight of the aircraft, the connection holes will be subjected to alternating loads. Since stress concentration is easily generated around the hole structure, the aircraft panel is very likely to fail due to fatigue when used under fatigue load conditions.

[0003] In the prior art, in order to improve the fatigue performance of the hole structure, two methods are usually used: extrusion strengthening and laser shock strengthening. Extrusion strengthening refers to the use of the direct contact between the extrusion strengthening tool (for example, the mandrel) and the hole wall, and the relative extrusion amount is all applied to the hole wall. The extrusion strengthening tool extrudes the hole wall, and the hole wall material is subjected to the extrusion force to produce metal flow and elastic-plastic deformation to achieve hole extrusion strengthening. However, due to the small thickness of some wall panels, after the extrusion strengthening is completed, the release of residual stress will cause the surface layer around the hole to deform as a whole; laser shock strengthening is to irradiate the material with shock waves emitted by a high-power short-pulse laser in a very short time, and quickly heat the material surface to the vaporization temperature, so that the material surface undergoes plastic deformation. Therefore, this method can only strengthen the hole surface, but not the surface layer around the hole. At the same time, when the aperture of the connecting hole is less than 3mm, the mandrel is easy to break, so the extrusion strengthening method cannot be used. Conventional laser shock strengthening will cause the surface layer around the hole to collapse inward, which will affect the hole accuracy and there is a problem that the hole wall cannot be strengthened.

[0004] In view of this, it is necessary to improve the strengthening method of the connection hole of the thin-walled structural parts in the prior art to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that in the existing extrusion strengthening method, when the thickness of some wall panels is small, the release of residual stress will cause overall deformation of the surface layer around the hole, the laser shock strengthening method can only strengthen the hole surface but not the surface layer around the hole, and when the hole diameter of the connecting hole is less than 3mm, the core shaft is easy to break and the extrusion strengthening method cannot be used. The laser shock strengthening method will cause the surface layer around the hole to collapse inward, which will affect the hole accuracy and there is a problem that the hole wall cannot be strengthened.

[0006] To achieve the above object, the present invention provides a laser shock strengthening method for connecting holes of thin-walled structural parts, comprising:

[0007] Placing a thin-walled structural part with a connection hole on a cushion block, setting a rigid core shaft in the connection hole, and sequentially setting a constraint layer and an absorption layer from top to bottom on the top of the cushion block, wherein the constraint layer and the absorption layer at least cover the connection hole in the longitudinal direction;

[0008] A plurality of irradiation points are symmetrically and evenly arranged at the edge of the connection hole with the center of the connection hole as the symmetry center. The focused laser beam passes through the constraint layer at the top of the constraint layer and is aligned with the two symmetrical irradiation points in sequence along the longitudinal direction to irradiate the absorption layer in sequence.

[0009] As a further improvement of the present invention, the diameter of the rigid mandrel is 0.02 to 0.04 mm smaller than the diameter of the connecting hole, the height of the rigid mandrel is 0.1 to 0.15 mm greater than the thickness of the thin-walled structural part, and the lower surface of the rigid mandrel and the lower surface of the thin-walled structural part are located on the same horizontal plane.

[0010] As a further improvement of the present invention, the wave impedance corresponding to the material of the cushion block is 0.2 to 1*10 lower than the wave impedance corresponding to the material of the thin-walled structural part. 7 kg·m -2 ·s -1 .

[0011] As a further improvement of the present invention, the material of the thin-walled structural part is titanium alloy or aluminum alloy, and the thickness of the thin-walled structural part is 2 to 3 mm.

[0012] As a further improvement of the present invention, the material of the pad is alumina ceramic or high-strength aluminum alloy.

[0013] As a further improvement of the present invention, the material of the rigid core shaft is tungsten steel or high-strength titanium alloy.

[0014] As a further improvement of the present invention, the constrained layer is a flowing water film, and the thickness of the water film is 1 to 1.5 mm, and the flow rate of the water film is 5 to 10 cm / min.

[0015] As a further improvement of the present invention, the absorption layer is an aluminum foil or polyester tape with adhesive, and the thickness of the aluminum foil or polyester tape is 100-150 microns, and the thickness of the adhesive is 10 microns.

[0016] As a further improvement of the present invention, the wavelength of the laser beam is 532nm or 1064nm, the pulse width is 15-25ns, and the power density is 2-4GW / cm 2 The spot diameter of the focused laser beam is 3 to 5 mm.

[0017] As a further improvement of the present invention, the overlap rate between two adjacent light spots is 50-75%.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The laser beam spot is longitudinally aligned with the irradiation point, and the irradiation point is set at the edge of the connection hole, so that the spot acts on the surface of the connection hole and the rigid mandrel at the same time. Due to the high strength of the rigid mandrel, 2-4GW / cm 2 The laser beam with a power density of 1000W does not cause plastic deformation of the rigid mandrel. Under the action of the laser shock wave induced by the laser beam, an interface wave will be generated between the interface of the rigid mandrel and the wall of the connecting hole, causing the wall of the connecting hole to be squeezed. Since the rigid mandrel will not produce plastic deformation, the surface of the connecting hole and the wall of the connecting hole are squeezed and strengthened. By using a pad with low wave impedance, when the laser shock wave is transmitted to the interface between the thin-walled structural parts and the pad, most of the shock wave energy can be transmitted to the pad, thereby effectively suppressing the reverse deformation caused by the action of the laser shock wave. Under the action of the laser shock wave, the surface layer around the hole will produce plastic deformation. If the laser shock is performed on the hole in a circular order, the plastic deformation of the surface layer around the hole will accumulate, thereby reducing the accuracy of the hole position. However, the symmetrical and sequential shock method will not cause the accumulation of plastic deformation, and the accuracy of the hole position is guaranteed to the greatest extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A schematic diagram of the steps of a laser shock strengthening method for a connecting hole of a thin-walled structural part shown in the present invention;

[0021] Figure 2 It is a schematic diagram of the structure of the laser beam, the constraining layer, the absorbing layer, the rigid mandrel, the thin-walled structural parts and the spacer;

[0022] Figure 3 A schematic diagram of 8 irradiation points being symmetrically and evenly arranged at the edge of the connection hole;

[0023] Figure 4 TEM image of the surface layer around the pore;

[0024] Figure 5 This is the TEM diffraction pattern of the surface layer around the hole. DETAILED DESCRIPTION

[0025] The present invention is described in detail below in conjunction with the various embodiments shown in the accompanying drawings, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.

[0026] Ginseng Figures 1 to 4 As shown, the present invention shows a specific implementation method of a laser shock strengthening method for connecting holes of thin-walled structural parts (hereinafter referred to as "the method"), which is used to strengthen the connecting holes 51 opened on the thin-walled structural parts 5 to improve the fatigue performance of the hole structure and prevent the deformation of the thin-walled structural parts 5.

[0027] Ginseng Figure 1 As shown, the method includes the following steps S1 to S2.

[0028] Step S1, placing a thin-walled structural part with a connecting hole on a cushion block, setting a rigid core shaft in the connecting hole, and setting a constraint layer and an absorption layer in sequence from top to bottom on the top of the cushion block.

[0029] Specifically, refer to Figure 2 and Figure 3 As shown, the constraint layer 2, the absorption layer 3, the thin-walled structural part 5 and the cushion block 6 are arranged in sequence from top to bottom, a connection hole 51 is opened on the cushion block 6, and a rigid core shaft 4 is arranged in the connection hole 51. Among them, the constraint layer 2 and the absorption layer 3 at least cover the connection hole 51 in the longitudinal direction. The diameter of the rigid core shaft 4 is 0.02~0.04mm smaller than the hole diameter of the connection hole 51, the height of the rigid core shaft 4 is 0.1~0.15mm larger than the thickness of the thin-walled structural part 5, and the lower surface of the rigid core shaft 4 and the lower surface of the thin-walled structural part 5 are located in the same horizontal plane, that is, the rigid core shaft 4 is arranged in the connection hole 51 opened in the thin-walled structural part 5, and the end of the rigid core shaft 4 slightly protrudes from the connection hole 51. The wave impedance corresponding to the material of the cushion block 6 is 0.2~1*10 lower than the wave impedance corresponding to the material of the thin-walled structural part 5. 7 kg·m -2 ·s -1 The material of the pad 6 is alumina ceramic or high-strength aluminum alloy, and the material of the rigid core shaft 4 is tungsten steel or high-strength titanium alloy. The constraint layer 2 is a flowing water film, and the thickness of the water film is 1 to 1.5 mm, and the flow rate of the water film is 5 to 10 cm / min to obtain a stable water film. The absorption layer 3 is an aluminum foil or polyester tape with adhesive, and the thickness of the aluminum foil or polyester tape is 100 to 150 microns, and the thickness of the adhesive is 10 microns.

[0030] Step S2, with the center of the connection hole as the symmetry center, multiple irradiation points are symmetrically and evenly set at the edge of the connection hole, and the focused laser beam passes through the constraining layer at the top of the constraining layer and is aligned with the two symmetrically set irradiation points in sequence along the longitudinal direction to irradiate the absorption layer in sequence.

[0031] Specifically, the laser beam 1 is focused, and the focused laser beam 1 passes through the constrained layer 2 from the top of the constrained layer 2 and irradiates the absorption layer 3. Multiple irradiation points are symmetrically and evenly arranged from the center of the connection hole 51 as the symmetric center and are arranged at the edge of the connection hole 51, that is, the number of irradiation points is even, and because the laser beam 1 is aligned with the irradiation points in the longitudinal direction, it can also be understood that the number of irradiations of the laser beam 1 is even. At the same time, during the irradiation process, two irradiation points symmetrically arranged from the center of the connection hole 51 are grouped together, and multiple groups are formed by multiple irradiation points. The focused laser beam 1 is aligned with the two irradiation points of each group in sequence in a group to pass through the constrained layer 2 and irradiate the absorption layer 3. Among them, the wavelength of the laser beam 1 is 532nm or 1064nm, the pulse width is 15-25ns, and the power density is 2-4GW / cm 2 The diameter of the spot 11 of the focused laser beam 1 is 3 to 5 mm, and the overlap rate between two adjacent spots 11 is 50 to 75%.

[0032] It should be noted that when strengthening the connection hole 51, the center point corresponding to the spot 11 of the focused laser beam 1 is aligned with the irradiation point in the longitudinal direction, that is, the center point corresponding to the spot 11 of the focused laser beam 1 is aligned with the edge of the connection hole 51 in the longitudinal direction, and the number of irradiation points is even and symmetrically and evenly arranged from the center point of the connection hole 51. A group of irradiation points (that is, two symmetrically arranged irradiation points) is selected from a plurality of irradiation points, and one of the irradiation points in the group is selected as the first irradiation point, and the spot of the focused laser beam 1 is aligned with the first irradiation point in the longitudinal direction to complete the irradiation of the first irradiation point, and then another irradiation point in the group is selected as the second irradiation point, and the spot of the focused laser beam 1 is aligned with the second irradiation point in the longitudinal direction to complete the irradiation of the second irradiation point, thereby completing the irradiation of one group, and then the second group of irradiation points are selected to irradiate in sequence, and so on, until the irradiation of all irradiation points is completed.

[0033] by Figure 3Taking the 8 irradiation points shown as an example, irradiation point a and irradiation point a1 are a group of irradiation points symmetrically set, irradiation point b and irradiation point b1 are a group of irradiation points symmetrically set, irradiation point c and irradiation point c1 are a group of irradiation points symmetrically set, and irradiation point d and irradiation point d1 are a group of irradiation points symmetrically set. Select irradiation point a as the first irradiation point, align the spot 11 of the focused laser beam 1 with the irradiation point a in the longitudinal direction, and the laser beam 1 passes through the constrained layer 2 from the top of the constrained layer 2 to irradiate the absorption layer 3, so as to irradiate the first irradiation point (i.e., irradiation point a); select irradiation point a1 as the second irradiation point, align the spot 11 of the focused laser beam 1 with the irradiation point a1, and the laser beam 1 passes through the constrained layer 2 from the top of the constrained layer 2 to irradiate the absorption layer 3, so as to irradiate the second irradiation point (i.e., irradiation point a1); select irradiation point b as the third irradiation point, align the spot 11 of the focused laser beam 1 with the irradiation point b in the longitudinal direction, and the laser beam 1 passes through the constrained layer 2 from the top of the constrained layer 2 to irradiate the absorption layer 3, so as to irradiate the third irradiation point (i.e., irradiation point b); and so on, the order of aligning the irradiation points is a, a1, b, b1, c, c1, d, d1.

[0034] It should be noted that the spot 11 of the laser beam 1 is longitudinally aligned with the irradiation point, and the irradiation point is set at the edge of the connection hole 51, so that the spot 11 acts on the surface of the connection hole 51 and the rigid core shaft 4 at the same time. Due to the high strength of the rigid core shaft 4, 2 to 4 GW / cm 2 The laser beam 1 with a power density of 1000W does not cause plastic deformation of the rigid core shaft 4. Under the action of the laser shock wave 12 induced by the laser beam 1, an interface wave 13 is generated between the interface of the rigid core shaft 4 and the hole wall of the connecting hole 51 (in shock dynamics, when a shock wave passes through materials with different wave impedances, an interface wave is generated at the interface), causing the hole wall of the connecting hole 51 to be squeezed. Since the rigid core shaft 4 does not produce plastic deformation, the surface of the connecting hole 51 and the hole wall of the connecting hole 51 are squeezed and strengthened. By using a pad 6 with a lower wave impedance, when the laser shock wave 12 is transmitted to the interface between the thin-walled structural part 5 and the pad 6, most of the shock wave energy can be transmitted to the pad 6, thereby effectively suppressing the reverse deformation caused by the action of the laser shock wave 12. Under the action of the laser shock wave 12, the surface around the hole will produce plastic deformation. If the laser shock is performed on the surface around the hole in a circular order, the plastic deformation of the surface around the hole will accumulate, thereby reducing the accuracy of the hole position. However, using a symmetrical and sequential shock method will not cause the accumulation of plastic deformation, thereby ensuring the accuracy of the hole position to the greatest extent.

[0035] Ginseng Figure 4 and Figure 5As shown, in a laser shock strengthening method for connecting holes of thin-walled structural parts shown in the present application, under the action of the forward laser shock wave 12 and the lateral interface wave 13, the hole wall material of the connecting hole 51 is squeezed, thereby playing an extrusion strengthening role, and at the same time, the hole surface is affected by the laser shock wave 12 and is also strengthened, and a high-amplitude residual compressive stress layer can be obtained on the hole surface and the hole periphery; by changing the material of the pad 6, the deformation of the thin-walled structural part 5 caused by the release of residual compressive stress during the action of the laser shock wave 12 can be effectively suppressed; because the hole wall material is subjected to the dual action of the forward laser shock wave 12 and the lateral interface wave 13, the grains of the surface layer around the hole are refined, and nanocrystals are formed on the surface layer around the hole formed by the connecting hole 51, thereby improving the fatigue performance of the connecting hole 51; because the rigid core shaft 4 does not run inside the connecting hole 51, the laser shock strengthening method for connecting holes of thin-walled structural parts shown in the present application can strengthen the connecting hole 51 with a hole diameter less than 1 mm, and the accuracy loss of the connecting hole 51 is reduced. Since the hole wall material will be deformed under the action of the laser shock wave 12, the hole structure will lose its positional dimensional accuracy. Therefore, in the present application, the strain generated by the laser shock wave 12 is balanced and offset by a method of symmetrical shocks in sequence, thereby achieving the purpose of ensuring the positional dimensional accuracy of the hole structure. This solves the problem that when the thickness of some wall panels is small, the release of residual stress in the existing extrusion strengthening method will cause the surface layer around the connecting hole formed by thin-walled structural parts (for example, aircraft wall panels) to deform as a whole. The laser shock strengthening method can only strengthen the hole surface but not the surface layer around the hole. When the hole diameter of the connecting hole is less than 3mm, the core shaft is easy to break and the extrusion strengthening method cannot be used. The laser shock strengthening method will cause the surface layer around the hole to collapse inward, which will affect the hole accuracy and there is a problem that the hole wall cannot be strengthened. More specifically, Figure 5 The diffraction patterns shown in the figure indicate that by implementing the present invention, nanocrystals are obtained in the hole surface and hole wall strengthening area, and the grains are greatly refined, which is beneficial to improving the fatigue life of the hole-containing structural part.

[0036] Embodiment 1:

[0037] A laser shock strengthening method for connecting holes of thin-walled structural parts comprises the following steps:

[0038] In this embodiment, the rigid mandrel 4 and the connecting hole 51 are selected with a diameter and a hole diameter of 1 mm. In fact, the diameter of the rigid mandrel 4 is 0.02-0.025 mm smaller than the hole diameter of the connecting hole 51. The material of the thin-walled structural part 5 is 7050 aluminum alloy, and the wave impedance is 1.85×10 7 kg·m -2 ·s -1, thickness is 2mm; the height of the rigid mandrel 4 is 2.1mm, and the material is TC17 titanium alloy; the material of the pad 6 is alumina ceramic, and the wave impedance is 0.96×10 7 kg·m -2 ·s -1 ; The pulse width of laser beam 1 is 15ns and the power density is 2GW / cm 2 , the diameter of the spot 11 is 3mm; the absorption layer 3 is an aluminum foil with adhesive, the thickness of the aluminum foil is 100 microns, and the thickness of the adhesive is 10 microns; the constraint layer 2 is a flowing water film with a thickness of about 1mm and a flow rate of 5cm / min. In this embodiment, four irradiation points are symmetrically and evenly arranged with the center of the connecting hole 51 as the symmetry center, that is, two groups of irradiation points, one of the irradiation points is selected, and any irradiation point in the group of irradiation points is selected as the first irradiation point, and the focused laser beam 1 is irradiated from the top of the constraint layer 2 through the constraint layer 2 on the absorption layer 3, and the spot 11 of the laser beam 1 is aligned with the first irradiation point in the longitudinal direction to complete the irradiation of the first irradiation point, and then another irradiation point in the group of irradiation points is selected as the second irradiation point, and the focused laser beam 1 is irradiated from the top of the constraint layer 2 through the constraint layer 2 on the absorption layer 3, and the spot 11 of the laser beam 1 is aligned with the second irradiation point in the longitudinal direction to complete the second Irradiation of the irradiation points; then select the second group of irradiation points from the two groups of irradiation points, and select any irradiation point in the second group of irradiation points as the third irradiation point, and irradiate the focused laser beam 1 from the top of the constrained layer 2 through the constrained layer 2 on the absorption layer 3, and align the spot 11 of the laser beam 1 with the third irradiation point along the longitudinal direction to complete the irradiation of the third irradiation point, and finally select another irradiation point in the second group of irradiation points as the fourth irradiation point, and irradiate the focused laser beam 1 from the top of the constrained layer 2 through the constrained layer 2 on the absorption layer 3, and align the spot 11 of the laser beam 1 with the fourth irradiation point along the longitudinal direction to complete the irradiation of the fourth irradiation point, thereby realizing impact strengthening of the connecting hole 51. After strengthening, the accuracy of the position of the connection hole 51 was tested. After testing, the accuracy of the position of the connection hole 51 did not change, and the average residual compressive stress value of the hole surface was 134MPa through XRD testing. The hole was cut open and the residual compressive stress of the hole wall was measured. The results showed that the average residual compressive stress value of the hole wall was 149MPa. The surface layer around the hole was observed by TEM, and it was found that the material of the outermost layer was nanocrystalline. At the same time, under the same test conditions, 5 groups of sample tests were conducted, and it was found that the average fatigue life of the hole structure parts strengthened by the laser shock strengthening method for connecting holes of thin-walled structural parts disclosed in this application was 3.47 times the average fatigue life of the unstrengthened hole structure parts.

[0039] Embodiment 2:

[0040] A laser shock strengthening method for connecting holes of thin-walled structural parts comprises the following steps:

[0041] In this embodiment, the rigid mandrel 4 and the connecting hole 51 are selected with a diameter and a hole diameter of 25 mm. In fact, the diameter of the rigid mandrel 4 is 0.035-0.04 mm smaller than the hole diameter of the connecting hole 51. The material of the thin-walled structural part 5 is TC4 titanium alloy, and the wave impedance is 2.21×10 7 kg·m -2 ·s -1 , thickness is 3mm; the height of the rigid mandrel 4 is 3.15mm, and the material is tungsten steel; the material of the pad 6 is 7050 aluminum alloy, and the wave impedance is 1.85×10 7 kg·m -2 ·s -1 ; The pulse width of laser beam 1 is 25ns and the power density is 4GW / cm 2 , the diameter of the spot 11 is 5mm; the absorption layer 3 is a polyester tape with adhesive, the thickness of the polyester tape is 150 microns, and the thickness of the adhesive is 10 microns; the constraint layer 2 is a flowing water film, the thickness is about 1.5mm, and the flow rate is 10cm / min. In this embodiment, 36 irradiation points are symmetrically and evenly set with the center of the connection hole 51 as the symmetry center, and the focused laser beam 1 is irradiated on the absorption layer 3 from the top of the constraint layer 2 through the constraint layer 2 by the above method to impact strengthen the connection hole 51. After strengthening, the accuracy of the position of the connection hole 51 is detected. After detection, the accuracy of the position of the connection hole 51 has not changed, and through XRD testing, the average residual compressive stress value of the hole surface is 257MPa. The hole is cut open and the residual compressive stress of the hole wall is measured. The results show that the average residual compressive stress value of the hole wall is 208MPa, and the surface layer around the hole is observed by TEM, and it is found that the material of the outermost layer is nanocrystalline. At the same time, under the same test conditions, 5 groups of sample tests were carried out, and it was found that the average fatigue life of the hole structure parts strengthened by the laser shock strengthening method for connecting holes of thin-walled structural parts disclosed in this application was 3.07 times the average fatigue life of the hole structure parts that were not strengthened.

[0042] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

[0043] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0044] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A laser shock strengthening method for connecting holes of thin-walled structural parts, characterized in that: include: Placing a thin-walled structural part with a connection hole on a cushion block, setting a rigid core shaft in the connection hole, and sequentially setting a constraint layer and an absorption layer from top to bottom on the top of the cushion block, wherein the constraint layer and the absorption layer at least cover the connection hole in the longitudinal direction; A plurality of irradiation points are symmetrically and evenly arranged at the edge of the connection hole with the center of the connection hole as the symmetry center. The focused laser beam passes through the constraint layer at the top of the constraint layer and is aligned with the two symmetrical irradiation points in sequence along the longitudinal direction to irradiate the absorption layer in sequence.

2. The laser shock peening method according to claim 1, characterized in that: The diameter of the rigid mandrel is 0.02-0.04 mm smaller than the diameter of the connecting hole, the height of the rigid mandrel is 0.1-0.15 mm greater than the thickness of the thin-walled structural part, and the lower surface of the rigid mandrel and the lower surface of the thin-walled structural part are located on the same horizontal plane.

3. The laser shock peening method according to claim 1, characterized in that: The wave impedance corresponding to the material of the cushion block is 0.2 to 1*10 lower than the wave impedance corresponding to the material of the thin-walled structural part. 7 kg·m -2 ·s -1 .

4. The laser shock peening method according to claim 3, characterized in that: The material of the thin-walled structural part is titanium alloy or aluminum alloy, and the thickness of the thin-walled structural part is 2-3 mm.

5. The laser shock peening method according to claim 3, characterized in that: The material of the pad is alumina ceramic or high-strength aluminum alloy.

6. The laser shock peening method according to claim 1, characterized in that: The material of the rigid core shaft is tungsten steel or high-strength titanium alloy.

7. The laser shock peening method according to claim 1, characterized in that: The constrained layer is a flowing water film, and the thickness of the water film is 1 to 1.5 mm, and the flow rate of the water film is 5 to 10 cm / min.

8. The laser shock peening method according to claim 1, characterized in that: The absorption layer is aluminum foil or polyester tape with adhesive, the thickness of the aluminum foil or polyester tape is 100-150 microns, and the thickness of the adhesive is 10 microns.

9. The laser shock peening method according to claim 1, characterized in that: The wavelength of the laser beam is 532nm or 1064nm, the pulse width is 15-25ns, and the power density is 2-4GW / cm 2 The spot diameter of the focused laser beam is 3 to 5 mm.

10. The laser shock peening method according to claim 8, characterized in that: The overlap rate between two adjacent light spots is 50-75%.

Citation Information

Patent Citations

  • Fastening hole machining strengthening method

    CN112593072A

  • Oblique angle laser shock processing

    US5911890A