Preparation method of platinum target material

Through powder metallurgy technology and hot isostatic sintering, forging and rolling treatment methods, the problems of high forming temperature and high cost of platinum targets are solved, effective control of grain size and density are achieved, and cracks are avoided and oxidation problems reduce production costs.

CN118932301AActive Publication Date: 2024-11-12HENAN DONGWEI ELECTRONIC EQUIPMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411041544.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

In the existing platinum target preparation methods, the molding temperature is high, the cost is expensive, and it is difficult to effectively control the grain size and density, and cracks and oxidation problems are prone to occur.

Method used

Powder metallurgy is adopted, and hot isostatic sintering, forging and rolling are carried out after vacuum welding to reduce the molding temperature, avoid cracks and oxidation, control grain size, and improve density.

Benefits of technology

It successfully reduces the forming temperature, saves energy consumption and raw materials, improves the density and grain control accuracy of the platinum target, is low in cost and easy to operate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932301A_ABST
    Figure CN118932301A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductors, in particular to a preparation method of a platinum target material. Comprising the following steps that 1, platinum powder raw materials are taken and put into a sheath, and welding sealing is conducted after vacuumizing; step 2, carrying out hot isostatic pressing sintering treatment on the package sleeve subjected to soldering sealing in the step 1; 3, the sheath treated in the step 2 is subjected to forging and pressing treatment, and then annealing treatment is conducted for the first time; 4, after a sheath of the platinum material subjected to the first annealing treatment is removed, rolling treatment is carried out, and then second annealing treatment is carried out; and 5, after secondary annealing treatment, the platinum target material is machined. According to the preparation method, through a powder metallurgy mode, vacuumizing treatment and then hot isostatic pressing sintering treatment, the forming temperature is effectively reduced, and energy consumption is saved; meanwhile, the platinum target material is wrapped by the sheath for forging and pressing, the problems of cracks and oxidation can be avoided, platinum material waste is reduced, and raw materials are saved; and through rolling treatment after forging and pressing, the grain size is well controlled, the compactness is improved, and the whole preparation process is low in cost and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, and in particular to a method for preparing a platinum target material. Background Art

[0002] The rapid development of new devices and new materials in the microelectronics industry, electronic, magnetic, optical, optoelectronic and superconducting films have been widely used in high-tech and industrial fields, which has led to the expansion of the sputtering target market. The sputtering deposition performance of the target is affected by the density, purity, grain size and size distribution range, grain orientation, texture, etc. of the target. Taking grain size and size distribution as an example, the sputtering rate of a target with fine grains is faster than that of a coarse grain. Because the smaller the grain, the more high free energy and high atomic dislocation grain boundaries of the target, and the easier it is to be bombarded by plasma in magnetron sputtering, resulting in a target with a small grain size having a higher sputtering deposition rate than a target with a large grain size. At the same time, the target with a smaller grain size difference has a more uniform thickness distribution of the deposited film. If the grain size variation is kept within 20%, the quality of the film obtained by sputtering the target will be significantly improved.

[0003] The grain size of different materials has different effects on the sputtering deposition performance of the target material, and the grain refinement process of different materials is also different. Even for the same material, the refinement process varies greatly depending on the purpose. The conventional preparation method of platinum target materials used in the semiconductor field is vacuum melting and then forming. The vacuum melting temperature is as high as 1700°C, the cost is also increased accordingly, and the grains are easy to grow; currently, there are few studies on the process of grain control and density of platinum targets. How to control the grains of platinum targets and improve the density of platinum targets is a problem that technicians in this field need to solve. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a platinum target material which can reduce the molding temperature and save costs while avoiding crack and oxidation problems, controlling the grain size and improving the density.

[0005] Based on the above purpose, the present invention adopts the following technical solutions:

[0006] A method for preparing a platinum target comprises the following steps:

[0007] Step 1, take the platinum powder raw material and put it into the bag, evacuate it and seal it with welding;

[0008] Step 2, subjecting the package sealed by welding in step 1 to hot isostatic pressing sintering;

[0009] Step 3, forging the sleeve processed in step 2, and then subjecting it to a first annealing treatment;

[0010] Step 4, after removing the sheath from the platinum material subjected to the first annealing treatment, rolling treatment is performed, followed by a second annealing treatment;

[0011] Step 5: After the second annealing treatment, the target is processed into a platinum target.

[0012] Preferably, in step 1, the diameter of the sheath is 80-150 mm and the thickness is 45-135 mm.

[0013] Preferably, in step 2, the hot isostatic pressing sintering treatment is performed at a temperature of 1050-1250° C., a pressure of 140-200 MPa, and a heat preservation time of 60-180 min.

[0014] Preferably, in step 3, the initial temperature of the forging process is not lower than 900°C, the end temperature is not lower than 300°C, and the diameter after forging is 108-200 mm and the thickness is 13-38 mm.

[0015] Preferably, the first annealing treatment temperature in step 3 is 750-900° C. and the heat preservation time is 60-120 min.

[0016] Preferably, in step 4, the rolling temperature is 300-500° C., the diameter after rolling is 160-300 mm, and the thickness is 5-15 mm.

[0017] Preferably, the second annealing treatment temperature in step 4 is 700-850° C., and the temperature is kept for 60-120 minutes.

[0018] Preferably, the platinum powder raw material in step 1 is platinum powder with a purity of 4N or above.

[0019] Preferably, the obtained platinum target has a purity of at least 4N, an oxygen content of less than 50 ppm, and an average grain size of less than 100 μm.

[0020] Preferably, the forging treatment in step 3 is to perform forging treatment multiple times in the height direction; and the rolling in step 4 is to remove the sheath of the platinum material and then roll it alternately in the vertical and horizontal directions.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The preparation method of the platinum target provided by the present invention uses a powder metallurgy method to perform a vacuum treatment to extract air, water vapor and impurities in a sheath, and then performs a hot isostatic pressing sintering treatment, thereby effectively reducing the molding temperature from more than 1800° C. to 1050-1250° C., thereby saving energy consumption; at the same time, the platinum target is wrapped in a sheath for forging, thereby avoiding the generation of cracks and oxidation problems, reducing the amount of platinum metal waste and saving raw materials; after forging, the grain size is well controlled by rolling treatment, thereby improving the density; the entire preparation process is low in cost, easy to operate, and the grain size of the platinum target is effectively controlled.

[0023] Forging is a processing method that uses a forging machine to apply pressure to a metal blank to cause it to undergo plastic deformation in order to obtain a forging with certain mechanical properties, a certain shape and size. Rolling is a pressure processing method in which a metal blank is passed through the gap between a pair of rotating rollers (in various shapes), and the material is compressed by the rollers to reduce its cross-section and increase its length. Forging is a highly longitudinal plastic deformation, while rolling is a transverse plastic deformation. The preparation method of the present invention, by first performing a forging process in the height direction, and then removing the sheath and rolling alternately in the longitudinal and transverse directions, can further control the grain size, making it difficult for the grains to grow, while also improving the overall density of the platinum target. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope photograph of the platinum target obtained in Example 1 of the present invention;

[0025] Figure 2 This is a grain size distribution diagram of the platinum target material obtained in Example 1 of the present invention;

[0026] Figure 3 This is a photo of the platinum target obtained in Example 2 of the present invention;

[0027] Figure 4 This is a grain size distribution diagram of the platinum target material obtained in Example 2 of the present invention;

[0028] Figure 5 This is a photo of the platinum target obtained in Example 3 of the present invention;

[0029] Figure 6 This is a grain size distribution diagram of the platinum target material obtained in Example 3 of the present invention; DETAILED DESCRIPTION

[0030] Refer to the following Figures 1 to 6 To describe a method for preparing a platinum target material according to an embodiment of the present invention. In the description of this embodiment, it should be understood that the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features, that is, include one or more of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. When a feature "includes or contains" one or some of the features it covers, unless otherwise specifically described, this indicates that other features are not excluded and may further include other features.

[0031] In the description of the present embodiment, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0032] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention is described in detail below, but the following embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by those skilled in the art without making creative work belong to the scope of protection of the present invention.

[0033] The present invention provides a method for preparing a platinum target, comprising the following steps:

[0034] Step 1, take the platinum powder raw material and put it into the bag, evacuate it and seal it with welding;

[0035] Step 2, subjecting the package sealed by welding in step 1 to hot isostatic pressing sintering;

[0036] Step 3, forging the sleeve processed in step 2, and then subjecting it to a first annealing treatment;

[0037] Step 4, after removing the sheath from the platinum material subjected to the first annealing treatment, rolling treatment is performed, followed by a second annealing treatment;

[0038] Step 5: After the second annealing treatment, the target is processed into a platinum target.

[0039] Preferably, in step 1, the diameter of the sheath is 80 to 150 mm, and the thickness is 45 to 135 mm.

[0040] Preferably, in step 2, the hot isostatic pressing sintering treatment is performed at a temperature of 1050-1250° C., a pressure of 140-200 MPa, and a heat preservation time of 60-180 min.

[0041] Preferably, in step 3, the initial temperature of the forging process is not lower than 900°C, the end temperature is not lower than 300°C, and the diameter after forging is 108-200 mm and the thickness is 13-38 mm.

[0042] Preferably, the first annealing treatment temperature in step 3 is 750-900° C. and the heat preservation time is 60-120 min.

[0043] Preferably, in step 4, the rolling temperature is 300-500° C., the diameter after rolling is 160-300 mm, and the thickness is 5-15 mm.

[0044] Preferably, the second annealing treatment temperature in step 4 is 700-850° C., and the temperature is kept for 60-120 minutes.

[0045] Preferably, the platinum powder raw material in step 1 is platinum powder with a purity of 4N or above.

[0046] Preferably, the obtained platinum target has a purity of at least 4N, an oxygen content of less than 50 ppm, and an average grain size of less than 100 μm.

[0047] Example 1

[0048] A method for preparing a platinum target comprises the following steps:

[0049] Step 1, taking platinum powder raw material with a purity of 4N or above and putting it into a steel ladle, and welding and sealing it after vibration and vacuuming; wherein the diameter of the ladle is 110 mm and the thickness is 80 mm;

[0050] Step 2, subjecting the package sealed in step 1 to hot isostatic pressing sintering treatment; wherein the hot isostatic pressing sintering treatment is performed at a temperature of 1150° C., a pressure of 170 MPa, and a heat preservation time of 120 minutes;

[0051] Step 3, forging the sheath after step 2, and then annealing for the first time; wherein the initial temperature of the forging process is not less than 900°C, the end temperature is not less than 300°C, the diameter of the sheath after forging is 150mm, and the thickness is 25m; the first annealing temperature is 820°C, and the heat preservation time is 90min;

[0052] Step 4, after removing the sheath from the platinum material after the first annealing treatment, rolling treatment is performed, and then a second annealing treatment is performed; wherein the rolling temperature is 400° C., and the diameter of the platinum material after rolling is 240 mm and the thickness is 10 mm; in step 4, the second annealing treatment temperature is 780° C. and the temperature is kept for 90 minutes.

[0053] Step 5: After the second annealing treatment, further processing is performed into a platinum target material. The purity of the obtained platinum target material is at least 4N and the oxygen content is 38 ppm.

[0054] like Figure 1 , Figure 2 As shown, the maximum grain size of the platinum target obtained in Example 1 is 170.05 μm, the minimum grain size is 34.51 μm, and the average grain size is 78.5 μm.

[0055] Example 2

[0056] A method for preparing a platinum target comprises the following steps:

[0057] Step 1, taking platinum powder raw material with a purity of 4N or above and putting it into a steel ladle, and welding and sealing it after vibration and vacuuming; wherein the diameter of the ladle is 80mm and the thickness is 45mm;

[0058] Step 2, subjecting the package sealed in step 1 to hot isostatic pressing sintering treatment; wherein the hot isostatic pressing sintering treatment is performed at a temperature of 1050° C., a pressure of 200 MPa, and a heat preservation time of 60 minutes;

[0059] Step 3, forging the sheath after step 2, and then annealing for the first time; wherein the initial temperature of the forging process is not less than 900°C, the end temperature is not less than 300°C, and the diameter of the sheath after forging is 108mm and the thickness is 13mm; the first annealing temperature is 900°C, and the heat preservation time is 60min;

[0060] Step 4, after removing the sheath of the platinum material subjected to the first annealing treatment, rolling treatment is performed, and then a second annealing treatment is performed; wherein the rolling temperature is 300° C., the diameter of the platinum material after rolling is 160 mm, and the thickness is 5 mm; in step 4, the second annealing treatment temperature is 700° C., and the heat preservation time is 120 minutes.

[0061] Step 5: After the second annealing treatment, further processing is performed into a platinum target material. The purity of the obtained platinum target material is at least 4N and the oxygen content is 35 ppm.

[0062] like Figure 3 , Figure 4 As shown, the maximum grain size of the platinum target obtained in Example 2 is 172.1 μm, the minimum grain size is 36.8 μm, and the average grain size is 86.5 μm.

[0063] Example 3

[0064] A method for preparing a platinum target comprises the following steps:

[0065] Step 1, taking platinum powder raw material with a purity of 4N or above and putting it into a steel ladle, and welding and sealing it after vibration and vacuuming; wherein the diameter of the ladle is 150mm and the thickness is 135mm;

[0066] Step 2, subjecting the package sealed in step 1 to hot isostatic pressing sintering treatment; wherein the hot isostatic pressing sintering treatment is performed at a temperature of 1250° C., a pressure of 140 MPa, and a heat preservation time of 180 minutes;

[0067] Step 3, forging the sheath after step 2, and then performing the first annealing treatment; wherein the initial temperature of the forging process is not less than 900°C, the end temperature is not less than 300°C, and the diameter of the sheath after forging is 200mm and the thickness is 38mm; the first annealing temperature is 750°C, and the heat preservation time is 120min;

[0068] Step 4, after removing the sheath of the platinum material subjected to the first annealing treatment, rolling treatment is performed, and then a second annealing treatment is performed; wherein the rolling temperature is 500° C., and the diameter of the platinum material after rolling is 300 mm and the thickness is 15 mm; in step 4, the second annealing treatment temperature is 850° C. and the temperature is kept for 60 minutes.

[0069] Step 5: After the second annealing treatment, further processing is performed into a platinum target material, and the purity of the obtained platinum target material is at least 4N and the oxygen content is less than 40 ppm.

[0070] like Figure 5 , Figure 6 As shown, the maximum grain size of the platinum target obtained in Example 3 is 169.1 μm, the minimum grain size is 37.2 μm, and the average grain size is 84.8 μm.

[0071] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a platinum target, characterized in that: The following steps are involved: Step 1, take the platinum powder raw material and put it into the bag, evacuate it and seal it with welding; Step 2, subjecting the package sealed by welding in step 1 to hot isostatic pressing sintering; Step 3, forging the sleeve processed in step 2, and then subjecting it to a first annealing treatment; Step 4, after removing the sheath from the platinum material subjected to the first annealing treatment, rolling treatment is performed, followed by a second annealing treatment; Step 5: After the second annealing treatment, the target is processed into a platinum target.

2. The method for preparing a platinum target according to claim 1, characterized in that: In step 1, the diameter of the sheath is 80-150 mm and the thickness is 45-135 mm.

3. The method for preparing a platinum target according to claim 1, characterized in that: In step 2, the hot isostatic pressing sintering treatment is carried out at a temperature of 1050-1250° C., a pressure of 140-200 MPa, and a heat preservation time of 60-180 min.

4. The method for preparing a platinum target according to claim 1, characterized in that: In step 3, the initial temperature of the forging process is not less than 900° C., the end temperature is not less than 300° C., and the diameter after forging is 108 to 200 mm and the thickness is 13 to 38 mm.

5. The method for preparing a platinum target according to claim 1, characterized in that: In step 3, the first annealing treatment temperature is 750-900° C. and the heat preservation time is 60-120 minutes.

6. The method for preparing a platinum target according to claim 1, characterized in that: In step 4, the rolling temperature is 300-500° C., the diameter after rolling is 160-300 mm, and the thickness is 5-15 mm.

7. The method for preparing a platinum target according to claim 1, characterized in that: In step 4, the second annealing treatment temperature is 700-850° C. and the heat preservation time is 60-120 minutes.

8. The method for preparing a platinum target according to claim 1, characterized in that: The platinum powder raw material in step 1 is platinum powder with a purity of 4N or above.

9. The method for preparing a platinum target according to claim 1, characterized in that: The obtained platinum target material has a purity of at least 4N, an oxygen content of less than 50 ppm, and an average grain size of less than 100 μm.

10. The method for preparing a platinum target according to claim 1, characterized in that: The forging process described in step 3 is to perform forging processes multiple times in the height direction; the rolling described in step 4 is to remove the sheath of the platinum material and then roll it alternately in the vertical and horizontal directions.

Citation Information

Patent Citations

  • Process for manufacturing high-density molybdenum-niobium alloy sputtering target material

    CN110257784A

  • Preparation method of nickel-platinum alloy target material

    CN115415523A

  • Preparation method of large-size and high-density molybdenum target material

    CN115502403A

  • Tantalum target material and preparation method and application thereof

    CN116970913A

  • PLATINUM GROUP ELEMENT - Mn BASED TARGET

    JP2001089850A