Copper foil and preparation method and application thereof

By using electrodeposition method and specific solution treatment in the preparation of copper foil, the problem of organic additives affecting the conductivity of the electrolyte is solved, the process stability and density of the copper foil are improved, and more accurate flow detection is achieved.

CN118932435AActive Publication Date: 2024-11-12江西江铜华东铜箔有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410997068.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

Smart Images

  • Figure CN118932435A_ABST
    Figure CN118932435A_ABST
Patent Text Reader

Abstract

The invention discloses a copper foil and a preparation method and application thereof, and relates to the technical field of copper foils, the preparation method of the copper foil comprises the following steps: dissolving copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution, and dissolving a complexing agent in a potassium hydroxide solution to obtain a complexing agent mixed solution; adding the copper-zinc mixed solution into the complexing agent mixed solution to obtain an electrolyte; providing an electro-deposition device, using a brass plate as an anode, using a titanium plate as a cathode, adopting a stabilized voltage direct current power supply, stirring at room temperature, adding a stabilizer and an additive, and electro-depositing electrolyte to obtain a copper-zinc alloy; the copper-zinc alloy is soaked in a sodium hydroxide solution and then soaked in a hydrochloric acid solution, and the copper foil is obtained.By means of the method, the problems that in the prior art, due to the fact that an organic additive is added, the conductivity of an electrolyte can be affected, the flow of an electromagnetic flowmeter cannot be detected, or the deviation between an actual value and a set flow value is large can be solved; the stability and the adjustment of the process are influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of copper foil, and in particular to a copper foil and a preparation method and application thereof. Background Art

[0002] Copper foil is mainly used as the negative electrode current collector of lithium batteries to improve the performance of the battery. Now, due to the porous setting, its structure is transformed from a planar structure to a three-dimensional structure, which increases the specific surface area, adjusts the nucleation site, and shortens the mass transfer distance, thereby reducing the local current, inhibiting the growth of dendrites, and improving the cycle performance and coulomb efficiency of lithium batteries. In addition, copper foil is also used in many fields such as the electronics industry, construction industry, and packaging industry, such as the production of electronic components such as printed circuit boards, integrated circuits, and capacitors, as well as architectural applications such as roofs, exterior walls, and interior walls to improve the durability and aesthetics of buildings.

[0003] Existing copper foil is generally prepared by hydrogen bubble template method under low copper, high acid and high current density. + , Cl - , PEG (polyethylene glycol), 3-mercapto-1-propanesulfonic acid (MPSA) and other additives can improve the density of copper foil, reduce roughness and enhance the overall performance of copper foil. However, the addition of organic additives will affect the conductivity of the electrolyte, resulting in the electromagnetic flowmeter failing to detect the flow or a large deviation between the actual value and the set flow value, affecting the stability and adjustment of the process. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a copper foil and a preparation method and application thereof, aiming to solve the technical problem that the addition of organic additives in the prior art will affect the conductivity of the electrolyte, resulting in the electromagnetic flowmeter being unable to detect the flow or the actual value deviating greatly from the set flow value, affecting the stability and adjustment of the process.

[0005] A first aspect of the present invention is to provide a method for preparing a copper foil, the method comprising:

[0006] Dissolving copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution, dissolving a complexing agent in a potassium hydroxide solution of a first preset concentration to obtain a complexing agent mixed solution;

[0007] Adding the copper-zinc mixed solution into the complexing agent mixed solution to obtain an electrolyte;

[0008] An electrodeposition device is provided, wherein a brass plate is used as an anode, a titanium plate is used as a cathode, a stabilized DC power supply is used, stirring is performed at room temperature, a stabilizer and an additive are added, and an electrolyte is electrodeposited at a preset deposition temperature and a preset current density for a first preset time to obtain a copper-zinc alloy;

[0009] The copper-zinc alloy is immersed in a sodium hydroxide solution of a second preset concentration for a second preset time, and then immersed in a hydrochloric acid solution of a third preset concentration for a third preset time to obtain a copper foil.

[0010] Compared with the prior art, the beneficial effect of the present invention is that the preparation method of the copper foil provided by the present invention can effectively improve the stability of the process, specifically, by coordinating with copper ions to form a stable complex, the cathode polarization of copper ions in electrolysis is improved, the deposition of copper ions is promoted, and then potassium hydroxide can react with zinc ions to form a Zn(OH) 4 2- It exists in the solution in the form of, and the deposition potential will also shift positively, which will further bring the deposition potentials of copper ions and zinc ions closer, achieve the purpose of co-deposition, improve the stability of the process, and by adding stability, it can effectively enhance the conductivity, improve the flow meter can not detect, the fluctuation value is large, improve the process stability, and then add additives, can effectively reduce the generation of cracks, accelerate ion migration, promote the crystallization nucleation of copper-zinc alloy, to achieve the effect of increasing density and refining grains, and further improve the stability of the process, thereby solving the problem that the addition of organic additives in the prior art will affect the conductivity of the electrolyte, resulting in the electromagnetic flowmeter flow can not be detected or the actual value and the set flow value deviate greatly, affecting the stability and adjustment of the process.

[0011] According to one aspect of the above technical solution, the step of dissolving copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution specifically includes:

[0012] Dissolve copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution, wherein the concentration of copper sulfate is 0.01 mol / L-1 mol / L, the concentration of zinc sulfate is 0.01 mol / L-1 mol / L, and the concentration ratio of copper sulfate to zinc sulfate is (0.5-3):1.

[0013] According to one aspect of the above technical solution, the first preset concentration is 2mol / L-4mol / L, the complexing agent is maltitol, and in the complexing agent mixture, the concentration of the complexing agent is 0.05mol / L-0.5mol / L.

[0014] According to one aspect of the above technical solution, the complexing agent is maltitol, and in the complexing agent mixed solution, the concentration of the complexing agent is 0.05 mol / L-0.5 mol / L.

[0015] According to one aspect of the above technical solution, the stabilizer is copper sulfate crystals, and the concentration of the stabilizer is 10g / L-50g / L.

[0016] According to one aspect of the above technical solution, the additive includes sodium hexametapolyphosphate and aminoacetic acid, the concentration of the sodium hexametapolyphosphate is 5 mg / L-12 mg / L, and the concentration of the aminoacetic acid is 1 mg / L-5 mg / L.

[0017] According to one aspect of the above technical solution, the preset deposition temperature is 30°C-50°C, and the preset current density is 1A / dm 2 -4A / dm 2 , the first preset time is 5min-20min.

[0018] According to one aspect of the above technical solution, the second preset concentration is 0.5mol / L-2mol / L, the second preset time is 4h-10h, the third preset concentration is 0.5mol / L-2mol / L, and the third preset time is 1min-5min.

[0019] A second aspect of the present invention is to provide a copper foil, wherein the copper foil is prepared by the above copper foil preparation method.

[0020] The third aspect of the present invention is to provide a use of the copper foil as described above in a lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0022] Figure 1 The present invention is a flow chart of the method for preparing the copper foil. DETAILED DESCRIPTION

[0023] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings. Several embodiments of the present invention are shown in the accompanying drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0024] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right", "upper", "lower" and similar expressions used herein are for illustrative purposes only and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0025] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be internal communication between two components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0026] See also Figure 1 , which shows a method for preparing a copper foil provided by the present invention, the preparation method comprises: steps S10-S13,

[0027] Step S10, dissolving copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution, dissolving a complexing agent in a potassium hydroxide solution of a first preset concentration to obtain a complexing agent mixed solution;

[0028] Among them, setting the ratio of copper sulfate and zinc sulfate can effectively improve the performance of the copper-zinc alloy, reduce the generation of cracks, and facilitate the subsequent formation of copper foil.

[0029] Preferably, in the copper-zinc mixed solution, the concentration of copper sulfate is 0.01mol / L-1mol / L, and the concentration of zinc sulfate is 0.01mol / L-1mol / L, for example, it can be 0.01mol / L, 0.05mol / L, 0.1mol / L, 0.2mol / L, 0.5mol / L, 0.7mol / L or 1mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0030] Furthermore, the concentration ratio of copper sulfate to zinc sulfate is (0.5-3):1.

[0031] In addition, the complexing agent is maltitol, which has a polyhydroxy structure and can coordinate with copper ions to form a stable complex, thereby increasing the cathode polarization of copper ions in electrolysis and promoting the deposition of copper ions.

[0032] Preferably, in the complexing agent mixture, the concentration of the complexing agent is 0.05mol / L-0.5mol / L, for example, it can be 0.05mol / L, 0.1mol / L, 0.2mol / L or 0.5mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Furthermore, potassium hydroxide can react with zinc ions to form Zn(OH) 42- exists in the solution in the form of, and the deposition potential will also shift positively, which will further bring the deposition potentials of copper ions and zinc ions closer, thus achieving the purpose of co-deposition.

[0034] Preferably, the first preset concentration is 2mol / L-4mol / L, for example, it can be 2mol / L, 2.5mol / L, 3mol / L, 3.5mol / L or 4mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Step S11, adding the copper-zinc mixed solution into the complexing agent mixed solution to obtain an electrolyte;

[0036] Step S12, providing an electrodeposition device, using a brass plate as an anode and a titanium plate as a cathode, using a stabilized DC power supply, stirring at room temperature, adding a stabilizer and an additive, and electrodepositing the electrolyte at a preset deposition temperature and a preset current density for a first preset time to obtain a copper-zinc alloy;

[0037] Among them, the stabilizer is copper sulfate crystals. In order to improve the performance of electrolytic copper-zinc alloy, complexing agents and additives will be added, but the organic matter or ions in the complexing agents and additives will affect the conductivity of the electrolyte, causing the electromagnetic flowmeter to fail to detect the flow or the actual value to deviate greatly from the set flow value, affecting the stability and adjustment of the process. Adding an appropriate amount of copper sulfate crystals can effectively enhance the conductivity and improve the problem that the flowmeter cannot detect and the fluctuation value is large. Secondly, the addition of copper sulfate crystals will not introduce new impurities and improve the purity of the copper-zinc alloy.

[0038] Preferably, the concentration of the stabilizer is 10 g / L-50 g / L, for example, it can be 10 g / L, 15 g / L, 20 g / L, 25 g / L, 30 g / L, 35 g / L, 40 g / L, 45 g / L or 50 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Further, the additive includes sodium hexametapolyphosphate and aminoacetic acid. Sodium hexametapolyphosphate is a surfactant, which can effectively reduce the surface tension of the electrolyte, reduce the potential of copper-zinc alloy deposition, accelerate ion migration, promote copper-zinc alloy crystallization nucleation, and improve the density and grain of copper-zinc alloy. Aminoacetic acid will reduce the stress in the electrolyte, and play the role of a brightener, reducing the cracks caused by stress during the deposition of copper-zinc alloy. Through the synergistic effect of the additive, the generation of cracks can be effectively reduced, ion migration can be accelerated, and copper-zinc alloy crystallization nucleation can be promoted, achieving the effect of improving density and refining grains.

[0040] Preferably, the concentration of the sodium hexametapolyphosphate is 5 mg / L-12 mg / L, for example, it can be 5 mg / L, 6 mg / L, 7 mg / L, 8 mg / L, 9 mg / L, 10 mg / L, 11 mg / L or 12 mg / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Preferably, the concentration of aminoacetic acid is 1 mg / L-5 mg / L, for example, 1 mg / L, 2 mg / L, 3 mg / L, 4 mg / L or 5 mg / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Step S13, soaking the copper-zinc alloy in a sodium hydroxide solution of a second preset concentration for a second preset time, and then soaking the copper-zinc alloy in a hydrochloric acid solution of a third preset concentration for a third preset time, to obtain a copper foil.

[0043] Among them, zinc in the copper-zinc alloy is removed by sodium hydroxide solution and hydrochloric acid solution.

[0044] The second preset concentration is 0.5mol / L-2mol / L, the second preset time is 4h-10h, the third preset concentration is 0.5mol / L-2mol / L, and the third preset time is 1min-5min. Zinc in the copper-zinc alloy is removed by low-concentration sodium hydroxide solution and low-concentration hydrochloric acid solution to reduce the generation of cracks in the copper-zinc alloy and reduce the collapse of the copper foil.

[0045] Correspondingly, the present invention provides a copper foil, which is prepared by the above copper foil preparation method. A preparation method for preparing the above copper foil.

[0046] Among them, the thickness of the copper foil is 2μm-5μm, and the specific surface area is 15m 2 / g-20m 2 / g, pore volume is 0.03cm 2 / g-0.05cm 2 / g, pore size is 120nm-170nm.

[0047] In addition, the present invention also provides an application of the copper foil in a lithium battery.

[0048] The present invention is further described below with specific embodiments:

[0049] Embodiment 1

[0050] The first embodiment of the present invention provides a method for preparing copper foil, the method comprising: steps S10-S13,

[0051] Step S10, dissolving copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution, dissolving a complexing agent in a potassium hydroxide solution of a first preset concentration to obtain a complexing agent mixed solution;

[0052] Among them, in the copper-zinc mixed solution, the concentration of copper sulfate is 0.2 mol / L, and the concentration of zinc sulfate is 0.09 mol / L.

[0053] Furthermore, the concentration ratio of copper sulfate to zinc sulfate is 2.22:1.

[0054] In addition, the complexing agent is maltitol, and in the complexing agent mixed solution, the concentration of the complexing agent is 0.2 mol / L, and the first preset concentration is 3 mol / L.

[0055] Step S11, adding the copper-zinc mixed solution into the complexing agent mixed solution to obtain an electrolyte;

[0056] Wherein, the copper-zinc mixed solution and the complexing agent mixed solution are mixed in equal volumes.

[0057] Step S12, providing an electrodeposition device, using a brass plate as an anode and a titanium plate as a cathode, using a stabilized DC power supply, stirring at room temperature, adding a stabilizer and an additive, and electrodepositing the electrolyte at a preset deposition temperature and a preset current density for a first preset time to obtain a copper-zinc alloy;

[0058] Wherein, the stabilizer is copper sulfate crystals, and the concentration of the stabilizer is 5g / L.

[0059] Furthermore, the additive includes sodium hexametapolyphosphate and aminoacetic acid, the concentration of the sodium hexametapolyphosphate is 10 mg / L, and the concentration of the aminoacetic acid is 3 mg / L.

[0060] Step S13, soaking the copper-zinc alloy in a sodium hydroxide solution of a second preset concentration for a second preset time, and then soaking the copper-zinc alloy in a hydrochloric acid solution of a third preset concentration for a third preset time, to obtain a copper foil.

[0061] Among them, the second preset concentration is 1 mol / L, the second preset time is 8 hours, the third preset concentration is 1 mol / L, and the third preset time is 2 minutes.

[0062] Embodiment 2

[0063] The second embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0064] In the copper-zinc mixed solution, the concentration of copper sulfate is 0.3 mol / L and the concentration of zinc sulfate is 0.09 mol / L.

[0065] Embodiment 3

[0066] The third embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0067] In the copper-zinc mixed solution, the concentration of copper sulfate is 0.2 mol / L and the concentration of zinc sulfate is 0.15 mol / L.

[0068] Embodiment 4

[0069] The fourth embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0070] The concentration of the complexing agent is 0.1 mol / L.

[0071] Embodiment 5

[0072] The fifth embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0073] The concentration of the complexing agent is 0.5 mol / L.

[0074] Embodiment 6

[0075] The sixth embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0076] The concentration of the stabilizer is 1 g / L.

[0077] Embodiment 7

[0078] The seventh embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0079] The concentration of the stabilizer is 10 g / L.

[0080] Embodiment 8

[0081] The eighth embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0082] The concentration of the sodium hexametapolyphosphate is 5 mg / L, and the concentration of the aminoacetic acid is 1 mg / L.

[0083] Embodiment 9

[0084] The ninth embodiment of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this embodiment is different from the method for preparing the copper foil in the first embodiment in that:

[0085] The concentration of the sodium hexametapolyphosphate is 12 mg / L, and the concentration of the aminoacetic acid is 5 mg / L.

[0086] Comparative Example 1

[0087] The first comparative example of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this example is different from the method for preparing the copper foil in the first example in that:

[0088] No complexing agent was added.

[0089] Comparative Example 2

[0090] The second comparative example of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this example is different from the method for preparing the copper foil in the first example in that:

[0091] No stabilizer was added.

[0092] Comparative Example 3

[0093] The third comparative example of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this example is different from the method for preparing the copper foil in the first example in that:

[0094] No additives are added.

[0095] Comparative Example 4

[0096] The fourth comparative example of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this example is different from the method for preparing the copper foil in the first example in that:

[0097] No sodium hexametapolyphosphate is added.

[0098] Comparative Example 5

[0099] The fifth comparative example of the present invention provides a method for preparing a copper foil. The method for preparing the copper foil in this example is different from the method for preparing the copper foil in the first example in that:

[0100] No glycine was added.

[0101] Please refer to the following Table 1, which shows the parameters corresponding to the above-mentioned Embodiments 1 to 9 and Comparative Examples 1 to 5 of the present invention.

[0102] Table 1

[0103]

[0104]

[0105] Combining the data of Examples 1 to 9 and Comparative Examples 1 to 5, it can be seen that the method for preparing the copper foil of the present invention can effectively increase the pore size and porosity and reduce the generation of cracks.

[0106] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0107] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing copper foil, It is characterized in that The preparation method comprises: Dissolving copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution, dissolving a complexing agent in a potassium hydroxide solution of a first preset concentration to obtain a complexing agent mixed solution; Adding the copper-zinc mixed solution into the complexing agent mixed solution to obtain an electrolyte; An electrodeposition device is provided, wherein a brass plate is used as an anode, a titanium plate is used as a cathode, a stabilized DC power supply is used, stirring is performed at room temperature, a stabilizer and an additive are added, and an electrolyte is electrodeposited at a preset deposition temperature and a preset current density for a first preset time to obtain a copper-zinc alloy; The copper-zinc alloy is immersed in a sodium hydroxide solution of a second preset concentration for a second preset time, and then immersed in a hydrochloric acid solution of a third preset concentration for a third preset time to obtain a copper foil.

2. The method for preparing the copper foil according to claim 1, It is characterized in that The step of dissolving copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution specifically comprises: Dissolve copper sulfate and zinc sulfate in deionized water to prepare a copper-zinc mixed solution, wherein the concentration of copper sulfate is 0.01 mol / L-1 mol / L, the concentration of zinc sulfate is 0.01 mol / L-1 mol / L, and the concentration ratio of copper sulfate to zinc sulfate is (0.5-3):

1.

3. The method for preparing the copper foil according to claim 1, It is characterized in that The first preset concentration is 2mol / L-4mol / L, the complexing agent is maltitol, and in the complexing agent mixture, the concentration of the complexing agent is 0.05mol / L-0.5mol / L.

4. The method for preparing the copper foil according to claim 1, It is characterized in that The complexing agent is maltitol, and in the complexing agent mixed solution, the concentration of the complexing agent is 0.05 mol / L-0.5 mol / L.

5. The method for preparing the copper foil according to claim 1, It is characterized in that The stabilizer is copper sulfate crystals, and the concentration of the stabilizer is 10g / L-50g / L.

6. The method for preparing the copper foil according to claim 1, It is characterized in that The additive comprises sodium hexametapolyphosphate and aminoacetic acid, the concentration of the sodium hexametapolyphosphate is 5mg / L-12mg / L, and the concentration of the aminoacetic acid is 1mg / L-5mg / L.

7. The method for preparing the copper foil according to claim 1, It is characterized in that The preset deposition temperature is 30°C-50°C, and the preset current density is 1A / dm 2 -4A / dm 2 , the first preset time is 5min-20min.

8. The method for preparing the copper foil according to claim 1, It is characterized in that The second preset concentration is 0.5mol / L-2mol / L, the second preset time is 4h-10h, the third preset concentration is 0.5mol / L-2mol / L, and the third preset time is 1min-5min.

9. A copper foil, It is characterized in that The copper foil is prepared by the method for preparing the copper foil according to any one of claims 1 to 8.

10. Use of the copper foil as claimed in claim 9 in a lithium battery.

Citation Information

Patent Citations

  • Cyanide-free electroplating brass liquid and application method thereof

    CN110592626A

  • Porous copper foil for lithium battery, preparation method and application thereof

    CN112635772A

  • Metal coated substrate

    CN114901866A

  • Aqueous zinc ion electrolyte additive containing maltitol and application thereof

    CN117080584A

  • Coated Metallic Substrates

    GB2605584A