Method for preparing Se-Sb semiconductor film through electro-deposition in deep eutectic solvent
By using pulse constant potential electrodeposition method in deep eutectic solvents, the problems of large deposition potential difference, poor stability of the plating solution and difficult to control the plating composition in traditional methods are solved, and high efficiency and low cost are achieved Se-Sb alloy film was prepared to obtain excellent photoelectric properties and uniform and dense films.
Patent Information
- Application Number
- CN202411198847.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
The preparation of Se-Sb alloy films in traditional aqueous solutions and traditional ionic liquids has problems such as large deposition potential difference, poor stability of the plating solution, high cost, low efficiency and difficult to control the plating composition. In the deep eutectic solvent, the electrodeposition efficiency and plating quality are low. Not good.
The Se-Sb semiconductor film was prepared in a choline chloride-ethylene glycol deep eutectic solvent by pulse constant potential electrodeposition method. By controlling the composition of the plating solution and the electrodeposition parameters, uniform co-deposition of Se and Sb is achieved, and the plating layer is improved. Component control accuracy and electrodeposition efficiency.
A high-quality Se-Sb semiconductor film with a band gap in the range of 1.15 to 1.20 eV was obtained, with the photoresponse current value between 0.08 and 0.15mA/cm2. The film was uniformly and dense, and the Se and Sb content was controllable, which reduced production costs. Improve the value of industrial applications.
Smart Images

Figure CN118932447A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a Se-Sb semiconductor film by electrodeposition in a deep eutectic solvent, which belongs to the field of electrodeposition and surface treatment technology, and particularly to the field of semiconductor preparation. The prepared Se-Sb semiconductor film has excellent semiconductor properties and can be applied to photovoltaics, solar cells, photoelectric conversion and other fields. Background Art
[0002] In recent years, with the rapid development of technologies such as photocatalysis, solar cells, photovoltaic materials, thermoelectric devices, hydrogen storage and lithium-ion batteries, semiconductor materials, as the basis of these technologies, have received widespread attention. Among many semiconductors, Se-Sb alloys are promising, but relatively speaking, they have not been fully developed. Among them, Se-Sb alloys with a Se content of about 60.00At% and a Sb content of about 40.00At% have a suitable band gap (band gap range of 1.10 to 1.20eV), which can absorb sunlight in a wider wavelength range (400nm to 1200nm); a large absorption coefficient (10 4 ~10 5 cm -1 It has the advantages of strong stability, high theoretical photoelectric conversion efficiency and environmental friendliness.
[0003] Traditional methods for preparing Se-Sb alloys include thermal evaporation, chemical vapor deposition (CVD), physical vapor deposition (PVD), magnetron sputtering, and electrodeposition. However, thermal evaporation has high requirements for equipment, is expensive, and has harsh operating conditions. The CVD and PVD methods are difficult to control the composition of the film and cannot accurately control the content of each element in the film. Magnetron sputtering requires high-energy ion sputtering, which is costly and inefficient, and it is also difficult to accurately control the composition of the film. Compared with other methods, the electrodeposition method is simple to operate, low cost, and can be industrialized. At the same time, the content of each element in the film can be easily controlled by adjusting the composition of the plating solution and the process parameters of the electrodeposition.
[0004] It is difficult to prepare Se-Sb alloy by electrodeposition in traditional aqueous solution because Sb in aqueous solution 3+ The standard electrode potential under acidic conditions is 0.15V, while SeO3 2-The standard electrode potential of is -0.37V, and the difference between the standard electrode potentials of the two is 0.52V, which is a large difference and makes co-deposition more difficult. Therefore, researchers have achieved co-deposition of Se and Sb by adding additives. For example, CN 115404466A discloses a method for preparing Sb2Se3 thin film, in which a Sb2Se3 precursor film is first prepared by electrodeposition in an aqueous solution, and then annealing is performed at 300-400°C to obtain a Sb2Se3 thin film. However, thiourea or selenourea is required as an additive to reduce the difference in deposition potential between the two. At the same time, the selection of selenium source and antimony source is relatively single and the concentration is only at the millimolar level, which is not conducive to industrial production. The method has a high annealing temperature, a narrow range, and a long time, which will result in a large loss of Se content in the film.
[0005] In the conventional aqueous solution, the electrodeposition of Se-Sb alloy still contains Sb 3+ The solubility is low, the stability of the plating solution is poor, and it is easy to produce SbOOH precipitation and other problems. Therefore, it is necessary to add a complexing agent and adjust the pH of the plating solution to increase the Sb 3+ The solubility and stability of the plating solution, and the environmental problems faced by the post-treatment of the plating solution have increased. These unfavorable factors limit the application of Se-Sb alloys prepared by electrodeposition in aqueous solution. For example, CN117845297A, a Se-Sb alloy negative electrode material and its preparation method, adds trisodium citrate, ethylenediamine hydrochloride and ethylene glycol as additives to the electrolyte to keep Sb 3+ Stability, reducing Se 4+ and Sb 3+ The potential difference.
[0006] At the same time, the selection of selenium and antimony sources in traditional aqueous solutions is relatively simple. The selenium and antimony sources used by researchers to prepare Se-Sb alloys by electrodeposition in aqueous solutions are sodium selenate / selenic acid and potassium antimony tartrate, which also limits the application of Se-Sb alloy thin films prepared by electrodeposition in aqueous solutions. In addition, Se-Sb alloy thin films have good catalytic properties. When deposited in aqueous solutions, a competitive reaction of Se-Sb alloy catalyzing water decomposition will occur, resulting in low electrodeposition efficiency and increased energy consumption.
[0007] Ionic liquids are considered to be a substitute for aqueous solutions. Ionic liquids contain a large number of anions and cations, which can be used as 3+ Provide a stable coordination environment to increase Sb 3+ In addition, ionic liquids do not contain water and OH - , avoiding the formation of SbOOH. However, traditional ionic liquids are sensitive to air, oxygen and water, have strict requirements on the operating environment, and most ionic liquids and their decomposition products are toxic, which limits their application range.
[0008] Deep eutectic solvent (DES) is the latest generation of ionic liquids. Compared with aqueous solutions and traditional ionic liquids, it has a wide electrochemical window, acts as a complexing agent, is stable to water and air, is green and biodegradable, and is an ideal solvent to replace traditional electrodeposition systems. Cyclic voltammetry was used to find that Se in DES 4+ The deposition potential of Sb is about -0.35V. 3+ The deposition potential of Se is about -0.40 V. 4+ , and Sb 3+ The potential difference is 0.05V, which shows great advantages in achieving the co-deposition of Se and Sb compared to the potential difference of 0.52V in aqueous solution.
[0009] However, when using DES as a solvent for electrodeposition, there are problems such as large system viscosity leading to large concentration polarization, slow ion migration rate, low electrodeposition efficiency, and poor coating quality. CN201510335144.7 A method for electrochemical co-deposition of CZTS (Se) thin film in a deep eutectic solvent adds deionized water as an additive to the electrolyte to reduce the viscosity of DES and increase the ion migration rate. Although the viscosity of the system is reduced, it will inevitably cause hydrogen and oxygen evolution problems, affecting the quality of the coating. At the same time, the constant current method will cause large fluctuations in the deposition potential, difficulty in deposition, and difficulty in controlling the coating composition due to the large viscosity of DES and the low ion migration rate. This method is annealed twice, the procedure is complicated, and additional selenium source / sulfur source needs to be added during annealing, which will make the Se / S composition in the film more difficult to control. CN202310137390.6 A self-assembled heterojunction catalyst, preparation method and application, the method uses an electron transfer method, selenium dioxide as a catalyst and a selenium source and oxygen source at the same time, to prepare a heterojunction catalyst. In this method, oxidation and reduction reactions occur simultaneously, which will lead to low deposition efficiency and loose coating. Oxidation and reduction occur simultaneously and compete with each other. The reduction rate is lower than the oxidation rate, and additional reducing agents need to be added. The process is complicated and the cost is increased. The increase in by-products affects the cycle life and long-term stability of the electrolyte. CN201810025092.7 A method for preparing nanoporous cobalt selenide by electrodeposition in a low-melting ionic liquid. This patent uses a constant potential electrodeposition method to prepare cobalt selenide compounds. Due to the large viscosity of DES, the low ion migration rate, and Se 4+ and Co 2+ The diffusion coefficients of Se 4+ and Co 2+ The ion concentration changes greatly. Under the influence of these factors, the deposition efficiency is reduced, the difficulty of coating thickening increases, the coating quality deteriorates, and the coating composition changes greatly.
[0010] The pulse constant potential electrodeposition method reduces the influence of concentration polarization by utilizing the relaxation of electric pulses, increases the cathode current density, accelerates the deposition rate, and reduces the influence of system viscosity on the coating. CN200910065147.8 A method for electrodepositing copper indium selenide or copper indium gallium selenide thin films using a special pulse power supply. This patent is a method for using high-frequency (26-400kHz) pulse electrodeposition in a water system. The water system has low viscosity, fast ion migration rate and small concentration polarization, so a higher frequency pulse electrodeposition method can be used. However, DES has problems such as high system viscosity, slow ion migration rate and large concentration polarization, and is not suitable for high-frequency pulse electrodeposition methods. In addition, this method uses cyanide as a complexing agent, and the pH needs to be adjusted to 1.0-2.0 during the electrodeposition process, and the process conditions are harsh. It is necessary to add an additional selenium source during the annealing process, which further increases the complexity of the operation. The film composition is difficult to control, which is not conducive to industrial production.
[0011] The problems of DES in the preparation of metals and their alloys by electrodeposition are slow ion migration rate, large concentration polarization, low coating quality, and difficult control of coating composition. The present invention creatively combines the low-frequency pulse electrodeposition method with the deep eutectic electrolyte system, which not only solves the problem of Sb in the traditional electrodeposition of Se-Sb alloy, but also solves the problem of Sb 3+ Ions cannot exist stably and Se 4+ and Sb 3+ The problem of large difference in deposition potential and difficulty in co-deposition is solved. The problem of slow ion migration rate and large concentration polarization caused by large viscosity of DES is solved, the electrodeposition efficiency is improved, the coating composition can be accurately controlled, and the coating quality can be improved, providing technical guarantee for obtaining high-quality Se-Sb semiconductor films. Summary of the invention
[0012] In view of the above problems, the present invention uses an electrochemical workstation and a pulsed constant potential method to prepare a Se-Sb semiconductor film with excellent optical and electrical properties in a choline chloride-ethylene glycol deep eutectic solvent. This invention is green and environmentally friendly. By using a deep eutectic solvent as a solvent and an electrolyte, the plating solution system does not need to add a complexing agent and a stabilizer. There is no hydrogen or oxygen evolution during the electrodeposition process, and the current efficiency is high. In addition, selenium sources and antimony sources are widely available. Ultimately, through the preparation of the plating solution system and the control of the electrodeposition process conditions, the obtained Se-Sb semiconductor film has excellent photoelectric properties, a band gap in the range of 1.15 to 1.20 eV, and a photoresponse current value of 0.08 to 0.15 mA / cm 2 In addition, the Se-Sb semiconductor film prepared in a deep eutectic solvent by pulse constant potential electrodeposition is uniform and dense, and the contents of Se and Sb are controllable.
[0013] The present invention provides a method for preparing a Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent, the specific steps of which are as follows:
[0014] (1) Substrate treatment: The substrate is first ultrasonically cleaned in acetone at a temperature of 25°C to 45°C for 20 to 30 minutes. Then the substrate is ultrasonically cleaned in anhydrous ethanol for 20 to 30 minutes. Finally, it is rinsed with deionized water, dried with cold air, and set aside.
[0015] (2) Preparation of deep eutectic solvent: choline chloride and ethylene glycol are stirred at a molar ratio of 1:1.5 to 1:3 at 60 to 90° C. (preferably 80° C.) for 3 to 6 hours to obtain the desired deep eutectic solvent.
[0016] (3) Plating solution: The plating solution is prepared by dissolving a certain proportion of a selenium source and an antimony source in a deep eutectic solvent.
[0017] (4) Plating: The plating solution is heated to the deposition temperature, and a constant potential pulse method is used in a three-electrode system to perform electrodeposition to prepare a Se-Sb semiconductor film. The working electrode is the pre-treated substrate, the counter electrode is a platinum mesh or platinum sheet, and the reference electrode is Ag / AgCl (the filling solution is a saturated NaCl ethylene glycol solution). Continuous plating is performed at a certain deposition potential and temperature.
[0018] (5) Post-plating treatment: After plating, the plated sheet is first ultrasonically cleaned with anhydrous ethanol for 1 to 3 minutes, then washed with deionized water for 1 to 3 minutes, blown dry with cold air, and set aside.
[0019] (6) Annealing treatment: The plated sheet obtained above is annealed in an argon or nitrogen atmosphere to obtain a Se-Sb semiconductor thin film.
[0020] Furthermore, the preparation method of the plating solution used for the electrodeposition in step (3) is to first completely dissolve the selenium source and the antimony source in the deep eutectic solvent respectively, and then mix the two uniformly in a certain molar ratio. The selenium source is any one of selenides such as selenium dioxide, selenium tetrachloride, sodium selenite, etc., and the concentration range is 0.05M to 0.30M. The antimony source is any one of antimony salts such as antimony trichloride, antimony sulfate, antimony acetate, antimony trioxide, antimony pentoxide, etc., and the concentration range is 0.10M to 0.60M.
[0021] Dissolving the selenium source and antimony source in the deep eutectic solvent separately first helps the selenium ions and antimony ions to fully dissolve and react with the Cl in the deep eutectic solvent. -After the two are completely dissolved separately and then mixed, the mutual influence between ions and the occurrence of redox reaction can be effectively prevented, thereby improving the stability of the plating solution. Deep eutectic solvents contain a large number of anions and cations, which can form stable complexes with metal ions, allowing the metal ions to exist stably in the solution and increase their solubility. The solubility of selenium and antimony sources can be increased to dozens of times that of traditional solvents, making the electrodeposition of Se-Sb semiconductor films in deep eutectic solvents lower in cost, more efficient, longer in service life, and more industrially valuable than traditional solvents.
[0022] Furthermore, the molar ratio of the selenium source to the antimony source in the electroplating solution in step (3) is 1:1 to 1:3. 4+ and Sb 3+ The deposition potential in the deep eutectic solvent is different. By controlling the main salt ratio of the plating solution, the co-deposition process of selenium and antimony is regulated to control the relative content of Se and Sb in the Se-Sb semiconductor film, thereby obtaining a Se-Sb semiconductor film with uniform and dense morphology and high photocurrent response value.
[0023] Further, in step (4), electrodeposition is carried out in a three-electrode system, the working electrode is one of FTO, ITO, Mo, Cu, Si, and stainless steel, the counter electrode is a platinum sheet or a platinum mesh, and the reference electrode is Ag / AgCl (the filling liquid is a saturated NaCl ethylene glycol solution). Compared with the two-electrode system, the three-electrode system can accurately control the potential and reduce the error in the deposition process. The diversity of the working electrode shows that the method of the present invention does not depend on a specific substrate and is easier to achieve large-scale preparation. For optoelectronic devices, FTO or ITO is preferably used as a substrate because the high light transmittance of FTO or ITO will not affect the optical and electrical properties of Se-Sb semiconductor films. The filling liquid of the reference electrode is a saturated NaCl ethylene glycol solution, which is more suitable for use in a choline chloride-ethylene glycol (DES) environment than the filling liquid of the traditional Ag / AgCl, which is a saturated KCl aqueous solution, so that the reference electrode is not affected by the electrolyte composition, the electrodeposition process, and the use time.
[0024] The present invention adopts a pulse constant potential electrodeposition method, with a duty cycle of 20% to 80%, a pulse frequency of 0.05Hz to 1.00Hz, and a deposition potential range of -0.30 to -1.00V. Due to the large viscosity of deep eutectic solvents, the electrodeposition process is greatly affected by concentration polarization using traditional constant potential or constant current methods, while the wide-amplitude low-frequency pulse constant potential electrodeposition method uses the relaxation of electric pulses to reduce the influence of concentration polarization, increase the cathode current density, and accelerate the deposition rate. In addition, the wide-amplitude low-frequency pulse constant potential electrodeposition method can more accurately control the element content of the coating, because the ion concentration near the electrode surface is in an approximately stable state during the electrodeposition process, so the element composition in the coating can be more accurately regulated by pulse parameters. The wide-amplitude low-frequency pulse constant potential method of the present invention can regulate the composition and structure of the coating by adjusting pulse parameters such as duty cycle and frequency. The method can refine the grains, and the obtained Se-Sb semiconductor alloy film is uniform and dense.
[0025] Furthermore, the deposition potential range of the present invention is -0.30 to -1.00V, which is wider than that of the water system. The present invention can prepare Se-Sb semiconductor films at larger underpotentials and higher overpotentials. In the deep eutectic system, due to the induced co-deposition of Se, Se and Sb can be co-deposited at a lower underpotential than their deposition potentials. Due to the catalytic properties of Se-Sb, hydrogen evolution will occur at around -0.5V in the water system, greatly affecting the quality of the coating and the efficiency of electrodeposition. The deep eutectic solvent has a wide electrochemical window (about 4.0V) due to its low volatility and high stability, low intrinsic redox potential and stability of the hydrogen bond network, so that a larger overpotential can be applied to deposit Se-Sb semiconductor films during the electrodeposition process, and the undesirable phenomena of hydrogen evolution and electrolyte decomposition will not occur, which can greatly improve the deposition rate and improve the preparation efficiency of Se-Sb semiconductor films.
[0026] Furthermore, the deposition temperature of pulse electrodeposition is 50-150°C, and the deposition time is 5-25min. Since the deep eutectic solvent prepared by the present invention has a low vapor pressure, is not easy to volatilize, has no hydrogen evolution side reaction during the deposition process, and has high deposition efficiency, the increase in temperature can reduce the viscosity of the deep eutectic solvent and increase the ion migration rate. The deep eutectic solvent has a eutectic effect, a rich hydrogen bond network, and a variety of molecular bond forces, so that it still maintains high stability when the temperature exceeds 100°C, giving full play to the characteristics of low-temperature molten salts, and improving deposition rate and efficiency.
[0027] Furthermore, in step (6), the annealing temperature in argon or nitrogen is 200-400°C, the heating rate is 5-20°C / min, the holding time is 1-10min, and the temperature is lowered at a rate of 5-15°C / min after the holding is completed. Appropriate annealing temperature and annealing time help to improve the crystallinity of the Se-Sb alloy without affecting the composition of the film. Too low annealing temperature and holding time are not conducive to the recrystallization process of the crystal. Too high annealing temperature and too long holding time will cause the Se element in the coating to volatilize, thereby causing changes in the composition of the coating and affecting the semiconductor properties of the film. Too fast heating and cooling rates will cause deformation or even cracking of the film. Only a suitable heating and cooling annealing procedure can avoid secondary growth of grains at high temperatures, reduce deformation, maintain the consistency of grain size and film morphology, and excellent semiconductor properties.
[0028] The Se-Sb semiconductor film obtained by the present invention has excellent semiconductor performance, fast light response speed, and high light response current value. Its band gap is in the range of 1.15 to 1.20 eV, P-type conductivity and light response current value are in the range of 0.08 to 0.15 mA / cm 2 Meanwhile, the selenium content in the film is between 57.00 and 63.00 at.%, the antimony content is between 37.00 and 43.00 at.%, and the main phase structure is Sb2Se3 phase.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] Compared with the traditional aqueous solution system, the deep eutectic solvent system has the advantages of wide electrochemical window and no hydrogen and oxygen evolution. At the same time, there are a large number of anions and cations in the deep eutectic solvent system, which can form complexes with metal ions, avoiding the use of additives.
[0031] Compared with the conventional Se-Sb alloy electrodeposited in aqueous solution, the present invention has Se 4+ With Sb 3+ The deposition potential difference is large and it is difficult to co-deposit Sb 3+ SbOOH precipitation is easily formed during the deposition process, causing the instability of the plating solution and the relatively single selection of selenium source and antimony source. However, the above problems can be avoided in deep eutectic solvents.
[0032] The present invention adopts a pulse constant potential electrodeposition method under a three-electrode system, which can more accurately control the electrodeposition potential of a high-viscosity non-aqueous system, significantly improve the quality of the coating, and obtain the advantages of a coating with a small grain size and uniform and dense coating. At the same time, the relaxation effect of the pulse constant potential electrodeposition can effectively reduce the influence of concentration polarization, increase the cathode current density, increase the deposition speed and efficiency, and more accurately control the element content of the coating.
[0033] The programmed annealing process of the present invention can avoid secondary growth of crystal grains at high temperatures, reduce deformation, and maintain the consistency of crystal grain size and film morphology as well as excellent semiconductor performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The figure (a) shows the surface morphology and composition of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing, and the figure (b) shows the photoresponse current curve.
[0035] Figure 2 FIG. 1 is a graph showing the surface morphology and composition of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing (a) and a graph showing the photoresponse current curve (b).
[0036] Figure 3 FIG. 1 is a graph showing the surface morphology and composition of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing (a) and a graph showing the photoresponse current curve (b).
[0037] Figure 4 FIG. 1 is a graph showing the surface morphology and composition of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing (a) and a graph showing the photoresponse current curve (b).
[0038] Figure 5 The surface morphology and composition diagram (a) and the photoresponse current curve diagram (b) of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing in Comparative Example 1 are shown.
[0039] Figure 6 Figure 2 shows the surface morphology and composition of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing (a) and the photoresponse current curve (b).
[0040] Figure 7 Figure 2 is the surface morphology and composition diagram (a) and the photoresponse current curve diagram (b) of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing in comparative example 3.
[0041] Figure 8 Figure 2 is a graph showing the surface morphology and composition of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-ethylene glycol deep eutectic solvent after annealing (a) and a graph showing the photoresponse current curve (b).
[0042] Fig. 9Figure 2 is a graph showing the surface morphology and composition of the Se-Sb semiconductor film prepared by electrodeposition in the choline chloride-urea deep eutectic solvent after annealing (a) and a graph showing the photoresponse current curve (b).
[0043] Fig.10 It is the surface morphology and composition diagram (a) and the photoresponse current curve diagram (b) of the Se-Sb semiconductor film prepared by constant potential electrodeposition in the choline chloride-urea deep eutectic solvent after annealing in comparative example seven. Specific implementation methods
[0045] Embodiment 1:
[0046] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0047] (2) Choline chloride and ethylene glycol are placed in a vacuum drying oven at 60° C. and dried for 2 h, respectively, and then cooled to 20° C. and mixed in a molar ratio of 1:2. The mixture is then heated and stirred at 80° C. for 3 h to form a clear and transparent deep eutectic solvent, which is then cooled for later use.
[0048] (3) Add selenium dioxide to the deep eutectic solvent (DES) in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly, and stirred for 1 hour to obtain electrolyte C, wherein the concentration of selenium dioxide is 0.20M, and the concentration of antimony trichloride is 0.40M.
[0049] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for pulse constant potential electrodeposition, the working electrode was FTO, the counter electrode was a Pt sheet, the reference electrode was Ag / AgCl (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.50 V, the duty cycle was 40%, the frequency was 0.10 Hz, the deposition temperature was 60°C, and the deposition time was 20 min.
[0050] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0051] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 300° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0052] Figure 1The surface morphology, composition and photoresponse current results of the Se-Sb semiconductor film obtained by annealing in the DES plating solution in Example 1 at a deposition potential of -0.50 V, a deposition temperature of 60°C and a deposition time of 20 min.
[0053] from Figure 1 From a, we can see that the microscopic morphology of the Se-Sb semiconductor film is linear. EDS results show that the Se content in the film is 59.49At%, and the Sb content is 40.51At%. The crystal structure shows the Sb2Se3 phase. Figure 1 It can be seen from b that the Se-Sb alloy film obtained by pulse constant potential electrodeposition has a rapid light response speed and good photoelectric properties. Its light response current value is 0.11mA / cm 2 At the same time, its band gap is 1.18eV, which is a p-type semiconductor.
[0054] Embodiment 2:
[0055] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0056] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0057] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, wherein the concentration of selenium dioxide is 0.20M and the concentration of antimony trichloride is 0.40M.
[0058] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for pulse constant potential electrodeposition, the working electrode was FTO, the counter electrode was a Pt sheet, the reference electrode was Ag / AgCl (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.70 V, the duty cycle was 60%, the frequency was 0.10 Hz, the deposition temperature was 60°C, and the deposition time was 20 min.
[0059] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0060] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 400° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0061] Figure 2 The surface morphology, composition and photoresponse current of the Se-Sb semiconductor film obtained by annealing in the DES plating solution of Example 2 at a deposition potential of -0.70 V, a deposition temperature of 60°C and a deposition time of 20 min. Figure 2 In a, it can be seen that the microscopic morphology of the Se-Sb semiconductor film is linear. EDS results show that the Se content in the film is 60.29At%, and the Sb content is 39.71At%. Figure 2 In b, it can be seen that the Se-Sb alloy film obtained by pulse constant potential electrodeposition has a fast light response speed and good photoelectric properties. Its light response current value is 0.09mA / cm 2 The crystal phase of the Se-Sb semiconductor film obtained in Example 2 is Sb2Se3 phase, a p-type semiconductor, and a band gap of 1.16 eV. Example 3:
[0062] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0063] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0064] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, wherein the concentration of selenium dioxide is 0.16M and the concentration of antimony trichloride is 0.48M.
[0065] (4) Electrodeposition: In the electrolyte C obtained in step (3), pulse constant potential electrodeposition was carried out using a three-electrode system, with FTO as the working electrode, Pt sheet as the counter electrode, Ag / AgCl as the reference electrode (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.70 V, the duty cycle was 60%, the frequency was 0.05 Hz, the deposition temperature was 120° C., and the deposition time was 10 min.
[0066] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0067] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 400° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0068] Figure 3 The surface morphology and composition of the Se-Sb semiconductor film obtained by annealing in the DES plating solution of Example 3, with a deposition potential of -0.70 V, a deposition temperature of 120°C, and a deposition time of 10 min, and the light response current curve obtained by testing in 0.5M H2SO4. Figure 3 From a, we can see that the microscopic morphology of the Se-Sb semiconductor film is linear. The Se content is 58.97At%, and the Sb content is 41.03At%. XRD analysis shows that the crystal phase of the film is Sb2Se3 phase. Figure 3 The results of b show that the Se-Sb semiconductor film has a fast response speed to light, and the photoresponse current value is 0.11mA / cm 2 The structure is p-type and the band gap is 1.17 eV. The Se-Sb semiconductor film has excellent photoelectric properties.
[0069] Embodiment 4:
[0070] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0071] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0072] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, wherein the concentration of selenium dioxide is 0.16M and the concentration of antimony trichloride is 0.48M.
[0073] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for pulse constant potential electrodeposition, the working electrode was FTO, the counter electrode was a Pt sheet, the reference electrode was Ag / AgCl (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.90 V, the duty cycle was 80%, the frequency was 1.00 Hz, the deposition temperature was 120°C, and the deposition time was 10 min.
[0074] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0075] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 400° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0076] Figure 4 The surface morphology and composition of the Se-Sb semiconductor film obtained by annealing in the DES plating solution of Example 4 at a deposition potential of -0.90 V, a deposition temperature of 120°C, and a deposition time of 10 min, and the photoresponse current curve obtained by testing in 0.5MH2SO4. Figure 4 From a, we can see that the microstructure of the Se-Sb semiconductor film is linear, the Se content is 60.69At%, and the Sb content is 39.31At%. Figure 4 b It can also be seen that the Se-Sb semiconductor film obtained by pulse constant potential electrodeposition has excellent light response speed and 0.10 mA / cm 2 The light response current value is 1.19 eV. The band gap value of the film is about 1.19 eV obtained by solid ultraviolet diffuse reflectance data. The Se-Sb semiconductor alloy film has p-type conductivity, and its main crystal phase structure is Sb2Se3 phase.
[0077] Comparative Example 1:
[0078] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0079] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0080] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, wherein selenium dioxide is 0.20M and antimony trichloride is 0.40M.
[0081] (4) Electrodeposition: In the electrolyte C obtained in step (3), pulse constant potential electrodeposition was carried out using a three-electrode system, with FTO as the working electrode, Pt sheet as the counter electrode, Ag / AgCl as the reference electrode (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.20 V, the duty cycle was 40%, the frequency was 0.10 Hz, the deposition temperature was 60°C, and the deposition time was 20 min.
[0082] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0083] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 300° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0084] The difference between Comparative Example 1 and Example 1 is that the applied deposition potential is changed to -0.2 V. The band gap of the Se-Sb semiconductor film obtained in Comparative Example 1 is 0.64 eV, and the crystal phase is mainly Se single phase and a small amount of Sb2Se3 phase. Figure 5 The surface morphology, composition and photoresponse current results of the Se-Sb semiconductor film obtained in Comparative Example 1 are shown in FIG. Figure 5 From a, we can see that the microstructure of the Se-Sb semiconductor film is mainly granular, with some short rods scattered. The EDS results show that the Se content in the film is 90.63At%, and the Sb content is 9.37At%. The deposition potential is relatively positive, which is not conducive to the deposition of Sb. Figure 5 It can be seen from the photoresponse current curve of b that the photoresponse current value of the Se-Sb semiconductor film obtained under the conditions of comparative example 1 is relatively low, which is 0.03 mA / cm 2 , the photoelectric performance is poor.
[0085] Comparative Example 2:
[0086] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0087] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0088] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, which contains 0.20M selenium dioxide and 0.40M antimony trichloride.
[0089] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for pulse constant potential electrodeposition, the working electrode was FTO, the counter electrode was a Pt sheet, the reference electrode was Ag / AgCl (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.70 V, the duty cycle was 90%, the frequency was 0.10 Hz, the deposition temperature was 60°C, and the deposition time was 20 min.
[0090] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0091] (6) The obtained coating was annealed in an argon atmosphere at a temperature of 400°C, an annealing time of 3 min, a heating rate of 10°C / min, a cooling rate of 10°C / min, and cooled to room temperature.
[0092] The difference between Comparative Example 2 and Example 2 is that the duty cycle set by the pulse constant potential electrodeposition method is changed to 90%. From the EDS results, it can be seen that the Se content in the film is 77.86At%, and the Sb content is 22.14At%. A larger duty cycle will promote excessive deposition of Se. From the XRD analysis, it can be seen that the crystal structure of the film is a single phase of Se and a small amount of Sb2Se3 phase, indicating that the excess Se in the film cannot be completely alloyed with Sb to transform into the Sb2Se3 phase. Figure 6 a The results show that the morphology of the film is mainly spherical and rod-shaped, indicating that a larger duty cycle will make the film morphology uneven. The band gap of the Se-Sb semiconductor film obtained in Comparative Example 2 is 0.81 eV. Figure 6 It can be seen from b that although the Se-Sb semiconductor film responds to light, the photoresponse current value is only 0.05 mA / cm 2 The photoelectric performance is poor.
[0093] Comparative Example 3:
[0094] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0095] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0096] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, which contains 0.16M selenium dioxide and 0.48M antimony trichloride.
[0097] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for pulse constant potential electrodeposition, the working electrode was FTO, the counter electrode was a Pt sheet, the reference electrode was Ag / AgCl (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.70 V, the duty cycle was 60%, the frequency was 0.01 Hz, the deposition temperature was 120°C, and the deposition time was 10 min.
[0098] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0099] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 400° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0100] The difference between Comparative Example 3 and Example 3 is that the frequency set in the pulse constant potential electrodeposition method is reduced to 0.01 Hz. The band gap of the Se-Sb semiconductor film obtained in Comparative Example 3 is 0.76 eV, and the crystal form is Se single phase and Sb2Se3 phase. The change in frequency affects the co-deposition ratio of Se and Sb, affects the alloying during the annealing process, affects the morphology and crystal structure of the coating, and affects the performance of the thin film semiconductor. Figure 7 It can be seen from a that the microscopic morphology of the Se-Sb semiconductor film is mainly rods of varying lengths. EDS results show that the Se content in the film is 82.97At%, and the Sb content is 17.03At%. At the same time, from the photocurrent curve, it can be obtained that the photoresponse current value of the Se-Sb semiconductor film is 0.04mA / cm 2 , which is much smaller than the light response current value of the third embodiment.
[0101] Comparative Example 4:
[0102] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0103] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0104] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, which contains 0.16M selenium dioxide and 0.64M antimony trichloride.
[0105] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for pulse constant potential electrodeposition, the working electrode was FTO, the counter electrode was a Pt sheet, the reference electrode was Ag / AgCl (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.90 V, the duty cycle was 80%, the frequency was 1.00 Hz, the deposition temperature was 120°C, and the deposition time was 10 min.
[0106] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0107] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 400° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0108] The difference between Comparative Example 4 and Example 4 is that Se in electrolyte C is 4+ With Sb 3+ The molar ratio changes from 1:3 to 1:4. Figure 8 The surface morphology, content and photoresponse current results of the Se-Sb semiconductor film obtained in Comparative Example 4 are as follows: Figure 8 From a, we can see that the microstructure of the film is agglomerated spheres. EDS results show that the Se content in the film is 49.41At%, and the Sb content is 50.59At%. XRD shows that the crystal structure of the film is Sb phase and Sb2Se3 phase. Figure 8b The photoresponse current curve shows that the photoresponse current value of the Se-Sb film obtained in Comparative Example 4 is 0.02 mA / cm 2 The band gap is 0.38eV. The increase in the proportion of antimony source in the electrolyte increases the Sb content in the film. Excessive Sb content is not conducive to the alloying of Se and Sb, affecting the microstructure and crystal structure of the film, resulting in the poor performance of the thin film semiconductor obtained in the fourth example.
[0109] Comparative Example 5:
[0110] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0111] (2) Choline chloride and urea were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0112] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, which contains 0.20M selenium dioxide and 0.40M antimony trichloride.
[0113] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for pulse constant potential electrodeposition, the working electrode was FTO, the counter electrode was a Pt sheet, the reference electrode was Ag / AgCl (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.50 V, the duty cycle was 40%, the frequency was 0.10 Hz, the deposition temperature was 60°C, and the deposition time was 20 min.
[0114] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0115] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 300° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0116] The difference between Comparative Example 5 and Example 1 is that the choline chloride-ethylene glycol deep eutectic solvent is replaced with a choline chloride-urea deep eutectic solvent. Fig. 9 In order to obtain the microscopic surface morphology, content and photoresponse current results of the Se-Sb semiconductor film in Comparative Example 5, Fig. 9 From a, we can see that the film has a spherical microstructure. EDS results show that the Se content in the film is 20.16At%, and the Sb content is 79.84At%. XRD analysis shows that the film's crystal structure is mainly Sb single phase and a small amount of Sb2Se3. Figure 8 b The photoresponse current curve shows that its photoresponse current value is 0.01mA / cm 2 The band gap of the semiconductor film is 0.25 eV. Compared with Example 1, choline chloride-urea DES is used as a solvent, in which urea reacts with Sb 3+ , Cl - The formation of complex ions promotes the deposition of Sb, resulting in an excessively high Sb content in the film and a small amount of Sb single-element impurity phase in the film after annealing, thereby reducing the semiconductor performance of the film.
[0117] Comparative Example 6:
[0118] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with toluene, acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0119] (2) Add selenium dioxide to deionized water and stir until the solution is clear and transparent to obtain electrolyte A. Add antimony trichloride to deionized water and stir until the solution is clear and transparent. Then add hydrochloric acid to the solvent to adjust the pH of the solvent to 2 to obtain electrolyte B. Then, mix electrolyte A and electrolyte B evenly, adjust the pH of the solvent to 2 with hydrochloric acid again, and stir well for 1 hour to obtain the final desired electrolyte C, wherein selenium dioxide is 0.015M and antimony trichloride is 0.030M.
[0120] (3) Electrodeposition: In the electrolyte C obtained in step (2), pulse constant potential electrodeposition was carried out using a three-electrode system, with FTO as the working electrode, Pt sheet as the counter electrode, Ag / AgCl as the reference electrode, the deposition potential being -0.50 V, the duty cycle being 40%, the frequency being 0.10 Hz, the deposition temperature being 60° C., and the deposition time being 20 min.
[0121] (4) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0122] (5) The coating obtained above was annealed in an argon atmosphere at a temperature of 300° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0123] The main difference between Comparative Example 6 and Example 1 is that the choline chloride-ethylene glycol deep eutectic solvent used is replaced with deionized water. Since water has a very low solubility in antimony salts, when water is used as the solvent, Sb in the plating solution 3+ The maximum concentration is 0.030M. In comparative example 6, the electrodeposition solution is unstable during the electrodeposition process, and SbOOH precipitates are produced. In addition, dense bubbles are generated on the surface of the working electrode during the electrodeposition process. After 20 minutes of electrodeposition, there are loose and discontinuous deposits on the surface of the FTO electrode. The EDS results show that the main components are Se and a small amount of Sb. The photoelectric properties are tested, and the coating has no photoresponse current to light.
[0124] Comparative Example 7:
[0125] (1) FTO was used as a substrate with a size of 20 mm × 10 mm × 0.03 mm. The organic matter remaining on the surface was washed away with acetone and anhydrous ethanol, and the surface moisture of the substrate was removed for later use.
[0126] (2) Choline chloride and ethylene glycol were placed in a vacuum drying oven at 60°C for 2 hours, respectively, and then cooled to 20°C and mixed in a molar ratio of 1:2. The mixture was then heated and stirred at 80°C for 3 hours to form a clear and transparent solution, which was then cooled for later use.
[0127] (3) Add selenium dioxide to the deep eutectic solvent in step (2), stir until the solution is clear and transparent, and obtain electrolyte A. Add antimony trichloride to DES, stir until the solution is clear and transparent, and obtain electrolyte B. Then, electrolyte A and electrolyte B are mixed evenly and stirred for 1 hour to obtain the final desired electrolyte C, wherein selenium dioxide is 0.20M and antimony trichloride is 0.40M.
[0128] (4) Electrodeposition: In the electrolyte C obtained in step (3), a three-electrode system was used for constant potential electrodeposition, with FTO as the working electrode, Pt sheet as the counter electrode, Ag / AgCl as the reference electrode (the filling liquid was a saturated NaCl solution in ethylene glycol), the deposition potential was -0.70 V, the deposition temperature was 60°C, and the deposition time was 20 min.
[0129] (5) After the electrodeposition is completed, rinse the plated sheet with anhydrous ethanol for 3 minutes, then rinse with deionized water for 3 minutes, blow dry with cold air, and store for later use.
[0130] (6) The coating obtained above was annealed in an argon atmosphere at a temperature of 400° C., an annealing time of 3 min, a heating rate of 10° C. / min, a cooling rate of 10° C. / min, and then cooled to room temperature.
[0131] The difference between Comparative Example 7 and Example 2 is that the electrodeposition method is changed to constant potential electrodeposition. Fig.10The surface morphology, composition and photoresponse current of the Se-Sb semiconductor film obtained in the DES plating solution in Comparative Example 7 when the deposition potential is -0.70V. Fig.10 From a, we can see that the microscopic morphology of the Se-Sb semiconductor film is uneven, mainly presenting granular, with some short rod-shaped substances as scattered impurities. EDS analysis results show that the Se content in the film is 85.27At%, and the Sb content is 14.73At%. Its crystal structure is mainly Se single phase and a small amount of Sb2Se3 phase. Fig.10 In b, the photoresponse current value of the Se-Sb semiconductor film obtained by constant potential electrodeposition is as low as 0.03 mA / cm 2 , the band gap is 0.69eV, and the photoelectric performance is poor.
[0132] The above embodiments and drawings are further explanations of the technical solutions of the present invention, but are not limited to the above embodiments and drawings. Any modification or equivalent replacement of the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent, characterized in that: The following steps are included (1) Preparation of deep eutectic solvent: mixing choline chloride and ethylene glycol to obtain a deep eutectic solvent; (2) Preparation of electrolyte: Selenium source and antimony source are added to the deep eutectic solvent respectively, stirred and dissolved, and then mixed evenly to obtain an electrolyte for electrodeposition of Se-Sb alloy film; (3) Electrodeposition: The working electrode, counter electrode and reference electrode are placed in an electrolyte and a Se-Sb semiconductor precursor film is prepared by a pulsed constant potential method; (4) Annealing treatment: The Se-Sb semiconductor precursor film obtained by pulse constant potential electrodeposition is annealed in an inert gas atmosphere to obtain a Se-Sb semiconductor film.
2. The method for preparing a Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent according to claim 1, characterized in that: Add choline chloride and ethylene glycol in a molar ratio of 1:1.5 to 1:3 and stir at 60 to 90°C for 3 to 6 hours to obtain a deep eutectic solvent.
3. The method for preparing Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent according to claim 1, characterized in that: The selenium source described in step (2) is any one of selenium dioxide, selenium tetrachloride, and sodium selenite; the antimony source is any one of antimony trichloride, antimony sulfate, antimony acetate, antimony trioxide, and antimony pentoxide.
4. The method for preparing a Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent according to claim 1, characterized in that: In step (2), the selenium source and antimony source in the electrolyte preparation are added to the deep eutectic solvent respectively, stirred at 50-100° C. until completely dissolved, and then the two are evenly mixed in a molar ratio of 1:1-1:3 to obtain a Se-Sb alloy thin film electrolyte with a selenium source concentration of 0.05M-0.30M and an antimony source concentration of 0.10M-0.60M.
5. The method for preparing Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent according to claim 1, characterized in that: In step (3), the working electrode substrate is any one of FTO, ITO, Si, Mo, Cu, and stainless steel.
6. The method for preparing Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent according to claim 1, characterized in that: Parameters of pulsed constant potential electrodeposition in step (3): pulse frequency is 0.05 Hz to 1.00 Hz; The duty cycle is 20% to 80%; the electrodeposition temperature is 50 to 150° C.; the deposition potential range is -0.30 to -1.00 V; and the deposition time is 5 to 25 minutes.
7. The method for preparing Se-Sb semiconductor thin film by electrodeposition in a deep eutectic solvent according to claim 1, characterized in that: In step (4), annealing is performed in an inert gas atmosphere, and the annealing procedure is as follows: a heating rate of 5 to 20°C / min, an annealing temperature of 200 to 400°C, an annealing time of 1 to 10 min, a cooling rate of 5 to 15°C / min, and cooling to room temperature.
8. A Se-Sb semiconductor thin film prepared by the method according to any one of claims 1 to 6, characterized in that: The microscopic morphology of the Se-Sb semiconductor film is dense and linear, and the selenium content is 57.00-63.00 At.%, and the antimony content is 37.00-43.00 At.%.
9. The use of the Se-Sb semiconductor thin film according to claim 7, characterized in that: The application of Se-Sb semiconductor film in semiconductors has a band gap of 1.15-1.20 eV and a P-type structure. The photoresponse current value is 0.08-0.15 mA / cm 2 The main phase structure is Sb2Se3 phase.
Citation Information
Patent Citations
Method for electrodepositing copper indium diselenide or copper indium gallium selenide film by special pulsing power source
CN101570871A
Method for electrochemical codeposition of CZTS (Se) films in deep eutectic solution
CN104962962A
Method of preparing nano porous cobalt selenide in low-eutectic ionic liquid via electrodeposition
CN108220991A
Preparation method of Sb2Se3 film and solar cell
CN115404466A
Self-assembled heterojunction catalyst, preparation method and application
CN116641090A
Cited By
GaS powder, GaS thin film electrode, preparation method of GaS powder and GaS thin film electrode, and photoelectric detector
CN120736558A
GaS powder, GaS thin film electrodes and their preparation methods, photodetectors
CN120736558B