Memory alloy-based deformable color-changing composite fabric and manufacturing method thereof

Through a composite fabric with a four-layer structure, combining memory alloy, resistive wire and elastic wire layer, a simple and easy-to-get color distortion effect is achieved, solving the complex structure problems in the prior art, and supporting reversible color distortion and deformation processes.

CN118932629AActive Publication Date: 2024-11-12TSINGHUA UNIVERSITY
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410990685.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing deformable fabrics have complex structures when achieving discoloration and deformation, and lack simple and feasible solutions, making it difficult to support discoloration and deformation at the same time.

Method used

Composite fabrics with four-layer structures include base fabric, memory alloy layer, resistive wire layer and elastic wire layer. The fabric is discolored and deformed through automatic embroidery technology and temperature-changing pigment. The memory alloy layer drives deformation when heated, and resistive wire The heating of the layer causes the fabric area to heat up and discolor, and the elastic silk layer returns to its initial form when the temperature drops.

Benefits of technology

It realizes a simple and easy-to-get discolored fabric, supports reversible discoloration and deformation processes, and adjusts the degree of deformation and discoloration by controlling the current magnitude to ensure that the fabric returns to its initial form at room temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932629A_ABST
    Figure CN118932629A_ABST
Patent Text Reader

Abstract

The invention provides a memory alloy-based deformable color-changing compound fabric and a manufacturing method thereof. The compound fabric comprises four layers, namely a bottom layer, a top layer and a bottom layer, the memory alloy layer is made of memory alloy; the resistance wire layer is composed of a conductive wire; the elastic silk layer is formed by silk threads; the bottom layer, the memory alloy layer, the resistance wire layer and the elastic wire layer are sequentially arranged from bottom to top. The composite fabric is simple in structure and supports color change and deformation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of fabrics, and in particular to a deformable and color-changing composite fabric based on a memory alloy and a manufacturing method thereof. Background Art

[0002] Fabric products are everywhere in our daily lives. In some situations, fabric products with dynamic color and deformation capabilities can better enhance the user interaction effect. For example, a textile flower decoration can have dynamic changes such as turning red and the petals unfolding to simulate the effect of blooming.

[0003] However, the current implementation of deformable fabric interfaces is often complex in structure, and there is no simple and feasible solution that can simultaneously support color change and deformation of fabrics. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a fabric that can change color and shape, and the manufacturing method of the fabric is relatively simple and the raw materials are relatively easy to obtain.

[0005] In a first aspect of the present invention, the present invention provides a composite fabric. According to an embodiment of the present invention, the composite fabric comprises four layers,

[0006] a bottom layer, the bottom layer being made of cloth;

[0007] A memory alloy layer, wherein the memory alloy layer is composed of a memory alloy;

[0008] A resistance wire layer, wherein the resistance wire layer is composed of conductive wires;

[0009] an elastic silk layer, wherein the elastic silk layer is composed of silk threads;

[0010] The four layers are respectively the bottom layer, the memory alloy layer, the resistance wire layer and the elastic wire layer in order from bottom to top. The composite fabric has a simple structure and can change color and deform, and the raw materials are relatively easy to obtain. The bottom layer can also be called the lower layer.

[0011] According to an embodiment of the present invention, the composite fabric may further include at least one of the following additional technical features:

[0012] According to an embodiment of the present invention, the composite fabric further comprises an upper layer.

[0013] According to an embodiment of the present invention, the upper layer is made of cloth.

[0014] According to an embodiment of the present invention, the upper layer is located above the elastic silk layer.

[0015] According to an embodiment of the present invention, the upper layer of fabric and the bottom layer of fabric are fixed together by sewing. The upper layer of fabric can be added or not according to whether both sides need to be fabric surfaces in actual conditions.

[0016] According to an embodiment of the present invention, the cloth is a thin cloth.

[0017] According to an embodiment of the present invention, the fabric has low elasticity.

[0018] According to an embodiment of the present invention, the fabric is easily dyeable.

[0019] According to an embodiment of the present invention, the fabric is selected to be relatively light, thin, less elastic, and easy to dye. The selected fabric is light and thin, so it has less damping when it is deformed; the fabric has less elasticity, so it can be automatically embroidered with specific patterns on it; and the fabric is easy to dye, and a specific area on it is dyed with a temperature-changing pigment, so that the dyed area can change color when heated.

[0020] According to an embodiment of the present invention, the memory alloy is a memory alloy wire.

[0021] According to an embodiment of the present invention, the diameter of the memory alloy wire is 0.1 mm-0.3 mm.

[0022] According to an embodiment of the present invention, the diameter of the memory alloy wire is 0.15 mm.

[0023] According to an embodiment of the present invention, the phase change temperature of the memory alloy wire is 40°C-45°C.

[0024] According to an embodiment of the present invention, the memory alloy layer is embroidered on the bottom fabric by using automatic embroidery technology.

[0025] According to an embodiment of the present invention, the memory alloy layer uses thinner memory alloy wire and is embroidered on the bottom fabric according to a specific pattern using automatic embroidery technology. When the memory alloy is heated, it undergoes a phase change, thereby driving the composite fabric to deform.

[0026] According to an embodiment of the present invention, the memory alloy layer is selected from memory alloy wires with a diameter ranging from 0.1mm to 0.3mm, and is embroidered on the bottom fabric according to a certain pattern. The memory alloy wire is similar to a general hard silk thread at room temperature and has a small elasticity; when it is heated, it undergoes a phase change, generates elastic force, and then drives the fabric to deform. The larger the diameter of the memory alloy wire, the greater the force generated by the phase change, and thus the stronger the ability to drive deformation.

[0027] According to an embodiment of the present invention, the electric wire is an enameled conductive wire.

[0028] According to an embodiment of the present invention, the diameter of the enameled conductive wire is 0.1 mm to 1 mm.

[0029] According to an embodiment of the present invention, the diameter of the enameled conductive wire is 0.1 mm to 0.5 mm.

[0030] According to an embodiment of the present invention, the heating temperature range of the resistance wire layer is 40°C-60°C.

[0031] According to an embodiment of the present invention, after the memory alloy layer is embroidered, the resistance wire layer is embroidered on the bottom fabric by using automatic embroidery technology.

[0032] According to an embodiment of the present invention, the resistance wire layer uses a thinner enameled conductive wire, and is embroidered on the bottom fabric according to a specific pattern using automatic embroidery technology after the memory alloy layer is embroidered. The outer layer of the enameled conductive wire has a thin insulating paint to ensure that there will be no short circuit during the embroidery process. When current is passed through the enameled conductive wire, it will generate heat, causing the composite fabric within the pattern coverage area to heat up, thereby causing the overlapping part of the memory alloy layer pattern to deform due to heat, and the overlapping part of the bottom / upper fabric dyeing range to change color due to heat.

[0033] According to an embodiment of the present invention, the resistance wire layer is selected from enameled conductive wires with diameters ranging from 0.1mm to 0.5mm, and is embroidered on the bottom fabric according to a certain pattern after the memory alloy layer is embroidered. When current is passed through the embroidered enameled conductive wire, it will generate heat, causing the composite fabric filled with the resistance wire layer pattern to heat up. The larger the diameter of the enameled conductive wire, the smaller the resistance per unit length, the stronger the heating capacity under a certain voltage, and the higher the temperature; at the same time, the smaller the diameter of the enameled conductive wire, the smaller its bending resistance. Generally, the heating temperature range of the resistance wire layer is between 40°C and 60°C.

[0034] According to an embodiment of the present invention, the wire is a wear-resistant wire.

[0035] According to an embodiment of the present invention, the wire is a hard wear-resistant wire.

[0036] According to an embodiment of the present invention, the diameter of the wire is 0.1 mm to 1 mm.

[0037] According to an embodiment of the present invention, after the resistance silk layer is embroidered, the elastic silk layer is embroidered on the bottom fabric by using automatic embroidery technology.

[0038] According to an embodiment of the present invention, the elastic silk layer first uses a thinner hard wear-resistant silk thread, and after the resistance silk layer is embroidered, it is embroidered on the bottom fabric using automatic embroidery technology according to a specific pattern to form an elastic silk fixed layer. There are jumps in the embroidery path, and some perforations are formed between the bottom fabric for the elastic silk to penetrate. Then the hard elastic silk is passed through the perforations and fixed in the composite fabric. The elastic silk forms a preset bending shape in the default state, so that the fabric material forms a preset structure by default. When the composite fabric is deformed by heat and the temperature drops, the elastic silk will pull the composite fabric back to the default structure.

[0039] According to an embodiment of the present invention, the elastic silk layer is firstly made of thin, hard, and wear-resistant silk thread, and is embroidered on the bottom fabric as a fixed thread according to a certain pattern after the resistance silk layer is embroidered. There are jumps on the embroidery path of the embroidered fixed thread, forming perforations that can be used to insert the elastic thread. After the fixed thread is embroidered, the hard elastic thread with a certain initial bending shape is passed through the perforations and fixed on the fabric. The elastic force of the elastic thread needs to be between the bending resistance of the resistance silk layer and the memory alloy layer at room temperature and the elastic force of the memory alloy layer after phase change. The above conditions ensure that the fabric at room temperature recovers the shape formed by the pulling of the elastic thread, and the memory metal wire undergoes a phase change after heating, overcoming the elastic force of the elastic thread and deforming the fabric.

[0040] According to an embodiment of the present invention, the bottom layer and (optionally) the upper layer of fabric are dyed with temperature-variable pigments, and the dyed area contained in the filling area of ​​the resistance wire layer will heat up and change color after the resistance wire is energized and heated. The temperature-variable pigment needs to ensure that its color-changing temperature range is between the designed normal temperature and the highest temperature that the resistance wire can maintain after heating up after energizing, so that the color changes when the resistance wire layer heats up and cools down.

[0041] According to an embodiment of the present invention, the cloth includes temperature-changing pigments.

[0042] According to an embodiment of the present invention, the temperature-changing pigment is a fuel that changes color at 40°C.

[0043] According to an embodiment of the present invention, the temperature-changing pigment is a vinyl blending liquid.

[0044] According to an embodiment of the present invention, the memory alloy is composed of a nickel-chromium memory alloy wire with a wire diameter of 0.15 mm and a phase change temperature of about 40°C.

[0045] According to an embodiment of the present invention, the conductive wire is 34AWG, 180°C temperature-resistant Litz wire.

[0046] According to an embodiment of the present invention, the wire is a 34AWG, 180°C temperature-resistant Litz wire.

[0047] According to an embodiment of the present invention, the fabric is a white-bottomed fabric made of cotton and linen.

[0048] According to the embodiment of the present invention, when the fabric resistance wire layer is powered on, it will heat up, causing the memory alloy layer to change phase, resulting in fabric deformation; at the same time, the temperature-changing pigment changes color; when the current is different, the degree of fabric deformation and discoloration is different. When the fabric resistance wire layer is powered off, it slowly cools down, and the elastic wire drives the fabric to return to its original shape. Therefore, the composite fabric can support reversible discoloration and deformation processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0050] Figure 1 It is a general structural diagram of the present invention;

[0051] Figure 2 is a schematic diagram of a flower structure according to a specific embodiment of the present invention;

[0052] Figure 3 A real picture of a flower according to a specific embodiment of the present invention (including blooming and closed states);

[0053] Figure 4 A schematic diagram of a single petal structure according to a specific embodiment of the present invention;

[0054] Figure 5 It is an expanded diagram of a single petal structure according to a specific embodiment of the present invention (an embroidery pattern designed by Rhino7 software);

[0055] Figure 6 This is a real picture of petals according to a specific embodiment of the present invention. DETAILED DESCRIPTION

[0056] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0057] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0058] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0059] Example 1

[0060] like Figure 2 As shown in the figure, this embodiment is a flower structure with four color-changing and deformable fabric petals. When the power is turned on, the petals can open and turn red; when the power is turned off, the petals will close and return to white, so as to reversibly simulate the effect of opening and closing. For specific effect pictures, please refer to Figure 3 .

[0061] The structure of this embodiment includes: a flower central stigma, a flower base, and four color-changing and deformable fabric petals based on the principles of the present disclosure.

[0062] In this embodiment, the flower center stigma and the flower base are both static structures. Figure 2 , Figure 3 As shown, it is made of 3D printed ABS material.

[0063] In this embodiment, the four petals have the same structure and are all composite fabrics as described in the present disclosure. The structural diagram is shown in FIG. Figure 4 The petal shape parameters are as follows. Figure 5 As shown, the petal shape structure, the specific design scheme of each layer and the manufacturing method are described in detail as follows.

[0064] In this embodiment, the petal shape, structure and technical parameters such as the selection of different layered wire materials are as follows, which can be referred to Figure 5:The petal shape is wide at the top and narrow at the bottom, similar to the shape of magnolia petals, with a maximum width of 41.6mm and a petal length of 80.2mm. The outer contour of the elastic wire layer is similar to the outer contour of the petals, and its maximum width is 40.5mm. The maximum width of the resistance wire layer is 40.0mm, which approximately fills the entire petal range. The memory alloy layer is arranged in a serpentine line to fill a rectangular area, with a width of 14.1mm and a length of about 50mm to support the expansion and deformation of the petals. The fabrics for the upper and bottom layers of the petals are made of thin cotton and linen white fabrics; the elastic wire layer and the resistance wire layer are both made of 34AWG, 180℃ heat-resistant Litz wire, and the wire diameter range is 0.1mm to 1.0mm; the memory alloy layer is made of nickel-chromium memory alloy wire with a wire diameter of 0.15mm and a phase change temperature of about 40℃, and the wire diameter range is 0.1mm to 1.0mm; the upper and bottom temperature-changing pigments are made of colorless red toner dissolved in vinyl blending liquid at 40℃. Each layered wiring design is exported as a .pes format file using Rhino7 software drawing programming, and embroidered by a Brother M370 sewing and embroidery machine. The above technical parameters and material selection are all feasible solutions, and any technical parameters or material selections with the same or similar characteristics can be used as alternatives to this embodiment.

[0065] In this embodiment, reference Figure 5 As shown, the memory alloy layer pattern uses closely arranged parallel serpentine lines, which are arranged along the center line of the petals. The center spacing of the parallel part of the serpentine line is 0.82mm, and there are 19 parallel lines side by side. The selected memory alloy is a nickel-titanium memory alloy wire with a wire diameter of 0.15mm, a phase change temperature of 40-45°C, and a phase change morphology of a straight line. When it is heated and the temperature rises to produce a phase change, the memory alloy wire will tend to straighten, overcome the elastic force of the elastic wire, and make the petal structure unfold. It should be noted that the memory alloy layer pattern and wire selection used in this embodiment are only a feasible solution. In theory, the larger the diameter of the memory alloy wire, the more parallel lines are arranged side by side, the greater the force generated by its straightening, and the larger the unfolding angle. The selectable wire diameter can range from 0.1mm to 1.0mm.

[0066] In this embodiment, reference Figure 5As shown, the resistance wire layer uses two filling schemes to fill the petal range, and there is repetition in a certain area to ensure the stability of the petal structure. The selected resistance wire is 34AWG enameled Litz wire, with a temperature tolerance of 180℃. When a current of 1.2-1.5V is passed, the temperature of the petals can reach between 45-55℃. At the root of the petals, the resistance wire layer adopts a parallel serpentine line arrangement perpendicular to the arrangement direction of the memory alloy layer. The center spacing of the parallel part of the serpentine line is 1.0mm, filling the petal area and extending 49.0mm in the vertical direction (along the center line of the petals). The serpentine line arrangement perpendicular to the center line of the petals can ensure that the resistance generated by the deformation of the resistance wire layer is small when the petals are unfolded and bent. In the upper part of the petals, the resistance wire layer adopts a serpentine arrangement along the equally divided transition curves on both sides of the petals. The number of equal divisions is 25 times, so that the spacing between adjacent equally divided transition curves is about 1.0mm. At the same time, the upper and lower arrangements of the resistance wire layer overlap in the middle of the petals, making the structure of the upper and middle parts of the petals (the area corresponding to the non-memory alloy layer) stable and not easy to deform, while the overlapping area of ​​the lower memory alloy layer is easy to bend. It should be noted that the resistance wire layer pattern, resistance wire material selection and input current used in this embodiment are only one feasible solution. In theory, the denser the arrangement of the resistance wire layer pattern, the greater the wire resistance, the greater the input current, and the more obvious the heating effect. The optional wire diameter can range from 0.1mm to 1.0mm.

[0067] In this embodiment, reference Figure 5 As shown, the elastic silk layer fixed silk adopts the corresponding pattern to be embroidered. The selected fixed silk is the same as the resistance silk layer. It should be noted that in this embodiment, the fixed silk can be selected as any hard wear-resistant silk thread as a substitute. Figure 4 , Figure 5 It shows that there are jumps in the embroidery process of the fixed silk, forming perforations for fixing the elastic silk.

[0068] In this embodiment, reference Figure 5 As shown, the elastic wire is made of 0.1 mm hard 304 stainless steel elastic wire, which is inserted into the perforation formed by the fixed wire. It should be noted that the hard elastic wire used in this embodiment is only a feasible solution, and other wires with the same or similar properties can be used as an implementation of the elastic wire described in the present disclosure.

[0069] In this embodiment, there is an upper layer of fabric, and both the upper layer and the bottom layer of fabric are cut into petal shapes.

[0070] In this embodiment, both the upper layer of fabric and the bottom layer of fabric are dyed with temperature-changing pigments. The selected temperature-changing pigments are temperature-changing color powders that change from colorless to red at 40°C. After being dissolved by a vinyl blending liquid, the fabrics are dyed. It should be noted that the temperature-changing pigments in this embodiment are only one feasible solution, and other temperature-changing pigments with the same or similar properties can be used as an implementation of the temperature-changing pigments described in the present invention.

[0071] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0072] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A composite fabric, It is characterized in that It consists of four floors. a bottom layer, the bottom layer being made of cloth; A memory alloy layer, wherein the memory alloy layer is composed of a memory alloy; A resistance wire layer, wherein the resistance wire layer is composed of conductive wires; an elastic silk layer, wherein the elastic silk layer is composed of silk threads; The four layers are respectively the bottom layer, the memory alloy layer, the resistance wire layer and the elastic wire layer in order from bottom to top.

2. The composite fabric according to claim 1, It is characterized in that The composite fabric further comprises an upper layer; Optionally, the upper layer is composed of cloth; Optionally, the upper layer is located above the elastic silk layer; Optionally, the upper layer of fabric and the bottom layer of fabric are fixed together by sewing.

3. The composite fabric according to claim 1 or 2, It is characterized in that The fabric is a light and thin fabric; Optionally, the fabric has low elasticity; Optionally, the fabric is susceptible to dyeing.

4. The composite fabric according to any one of claims 1 to 3, It is characterized in that The memory alloy is a memory alloy wire; Optionally, the diameter of the memory alloy wire is 0.1 mm-0.3 mm; Optionally, the diameter of the memory alloy wire is 0.15 mm; Optionally, the phase change temperature of the memory alloy wire is 40°C-45°C; Optionally, the memory alloy layer is embroidered on the bottom fabric by using automatic embroidery technology.

5. The composite fabric according to any one of claims 1 to 4, It is characterized in that The electric wire is an enameled conductive wire; Optionally, the diameter of the enameled conductive wire is 0.1 mm to 1 mm; Optionally, the diameter of the enameled conductive wire is 0.1 mm to 0.5 mm; Optionally, the heating temperature range of the resistance wire layer is 40°C-60°C; Optionally, after the memory alloy layer is embroidered, the resistance wire layer is embroidered on the bottom fabric using automatic embroidery technology.

6. The composite fabric according to any one of claims 1 to 5, It is characterized in that The silk thread is a wear-resistant silk thread; Optionally, the wire is a hard wear-resistant wire; Optionally, the diameter of the wire is 0.1 mm to 1 mm; Optionally, after the resistance silk layer is embroidered, the elastic silk layer is embroidered on the bottom fabric by using automatic embroidery technology.

7. The composite fabric according to any one of claims 1 to 6, It is characterized in that The fabric includes a temperature-changing pigment; Optionally, the temperature-changing pigment is a fuel that changes color at 40°C; Optionally, the temperature-changing pigment is a vinyl blending liquid.

8. The composite fabric according to any one of claims 1 to 7, It is characterized in that The memory alloy is composed of a nickel-chromium memory alloy wire with a wire diameter of 0.15 mm and a phase change temperature of about 40°C.

9. The composite fabric according to any one of claims 1 to 8, It is characterized in that The conductive wire is 34AWG, 180°C temperature-resistant Litz wire; Optionally, the wire is 34AWG, 180°C temperature-resistant Litz wire.

10. The composite fabric according to any one of claims 1 to 9, It is characterized in that The fabric is a white-bottomed fabric made of cotton and linen.

Citation Information

Patent Citations

  • Composite fabric with flexible wire

    CN107932999A

  • Artware capable of achieving flexible dynamic deformation

    CN108189609A

  • 3D background wall cloth

    CN110847531A

  • Method for orthopedy of foot and shoe with clamping plate

    CN1119093A

  • Fabric interface manufacturing process based on thermochromic embroidery

    CN114318705A