Method for rapidly identifying lithium iron phosphate battery cell with failure of liquid injection

CN118937374APending Publication Date: 2024-11-12WUHAN RIKOMAY NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065298.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

但在回收厂家回收过程中,无法做到完整的失效电芯追溯,从而导致回收到的电芯种类多样,品质参差不齐,大大增加了回收厂家的处理难度,导致了时间成本和经济成本较高

Benefits of technology

[0018] The beneficial effects of the present invention are: The principle of ICP identification is: The ICP testing principle is to detect the content of each element in the sample, and the main elements of the lithium iron phosphate battery positive electrode black powder are Li, Fe, and P, and the ternary battery positive electrode black powder The main elements of the powder are Ni, Co, and Mn, so according to the N in the I CP results i, Co, and Mn content can be used to determine whether this batch of batteries is a ternary battery or a ternary battery is mixed into the battery. Then, based on the atomic ratio of Li, Fe, and P, the structure of Fe and P can be determined, that is, It can be identified as lithium iron phosphate battery. The principle of XRD identification is: the main reason for the failure of lithium iron phosphate is the lack of lithium content, that is, lithium vacancies are generated in the structure, but the olivine structure still exists, and the material can be repaired, so the XRD pattern of the repairable failed lithium iron phosphate should be Similar to standard cards, there are four diffraction peaks (101), (140), (112), and (042). If not, it means that the olivine structure has been damaged and the material must be irreparable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937374A_ABST
    Figure CN118937374A_ABST
Patent Text Reader

Abstract

The invention relates to a method for quickly identifying liquid injection failure lithium iron phosphate battery cells, which comprises the following steps: randomly selecting n battery cells from the liquid injection failure lithium iron phosphate battery cells to be identified, and disassembling to obtain positive plates; performing high-temperature calcination and stripping on the positive plate obtained in the step S1 to obtain black powder, and testing black powder I CP; and analyzing an I CP result, and identifying whether the to-be-identified liquid injection failure lithium iron phosphate battery cell is a lithium iron phosphate battery cell or not. According to the contents of N , Co and Mn in an I < CP > result, whether the batch of battery cells are ternary battery cells or the ternary battery cells are mixed in the battery cells can be judged, then structures of Fe and P are determined according to the atomic ratio of L , Fe and P, and the battery cells can be identified as the lithium iron phosphate battery cells. The XRD spectrum of repairable failed lithium iron phosphate should be similar to that of a standard card, four diffraction peaks (101), (140), (112) and (042) exist, and if not, it is indicated that the olivine structure is damaged, and the material must not be repaired.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of energy materials and engineering technology, and in particular to a method for quickly identifying a lithium iron phosphate battery cell with injection failure. Background Art

[0002] With the increasing emphasis on sustainable energy development, people's attention has gradually shifted from traditional fossil energy to new clean energy, and lithium-ion batteries are one of them. Lithium-ion batteries (LI B) have dominated the portable electronics market in the past 20 years. Compared with other rechargeable batteries, lithium-ion batteries have higher energy per unit weight or volume.

[0003] At present, the application of lithium-ion batteries in transportation fields such as hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), and electric vehicles (EV) is widely pursued, and they are also seriously considered in the stationary storage and utilization of intermittent renewable energy such as solar energy and wind energy. With the expansion of production capacity, the number of waste lithium-ion batteries is also increasing. Waste lithium-ion batteries not only contain rich precious metal elements, but also retain residual energy. If improperly handled, waste lithium-ion batteries will increase the risk and pollution of the living environment. In this sense, the recycling of lithium-ion batteries is crucial to maintain the continuous supply of raw materials and prevent potential environmental pollution and hazards. Among various batteries, LiFePO4 (LFP) power batteries are mainly used in the fields of electric vehicles and smart grids. Their cost, safety and durability are superior to layered lithium transition metal oxides, and they have an indispensable market and lasting prosperity.

[0004] With the rapid growth of electric vehicles worldwide, millions of tons of waste LFP power batteries are waiting to be properly handled. In recent years, a lot of research has been conducted on the recycling of waste LFP power batteries, focusing on the recovery of valuable elements and the re-synthesis of new LFP positive electrode materials. Direct regeneration is a promising strategy developed in recent years. Its purpose is to repair the structure of cathode particles through a simple process without destroying the bulk phase. The new active materials regenerated through this process can be directly used to assemble new batteries. According to previous studies, direct regeneration has great potential in reducing greenhouse gas emissions. It is expected to achieve certain economic benefits by forming a closed-loop cycle through a simple process.

[0005] At present, LFP recycling mainly involves recycling retired cells from battery manufacturers, which are then processed by recycling manufacturers. However, during the recycling process, it is impossible to fully trace the failed cells, resulting in a variety of recycled cells with varying quality, which greatly increases the difficulty of processing for recycling manufacturers and leads to high time and economic costs. Summary of the invention

[0006] The technical problem to be solved by the present invention is to study a method for quickly identifying failed lithium iron phosphate battery cells due to injection, efficiently identifying failed lithium iron phosphate battery cells from unknown battery cells and judging their repairability, thereby reducing the time and economic costs of the battery cell classification and screening process.

[0007] The technical solution of the present invention to solve the above technical problems is as follows:

[0008] A method for quickly identifying a lithium iron phosphate battery cell with injection failure comprises the following steps:

[0009] S1, randomly selecting n cells from the lithium iron phosphate cells to be identified as having failed injection, and disassembling them to obtain the positive electrode sheets;

[0010] S2, calcining and peeling the positive electrode sheet obtained in S1 at high temperature to obtain black powder, and testing the I CP of the black powder;

[0011] S3. Analyze the ICP result to identify whether the lithium iron phosphate battery cell with injection failure to be identified is a lithium iron phosphate battery cell.

[0012] Based on the above technical solution, the present invention can also be improved as follows.

[0013] Further, if S3 identifies that the lithium iron phosphate battery cell with failed injection to be identified is a lithium iron phosphate battery cell, execute step S4;

[0014] S4. Test the black powder obtained in S1 with XRD. If the black powder has four diffraction peaks (101), (140), (112), and (042), the lithium iron phosphate battery cell that has failed injection can be repaired. Otherwise, it cannot be repaired.

[0015] Furthermore, in S1, n=3-10.

[0016] Furthermore, the temperature of high temperature calcination in S2 is 350-500°C, the holding time is 0.5-5h, the calcination atmosphere is one of N2 or Ar, and the gas flow rate is 5-10L / min.

[0017] Further, S3 specifically includes: if Ni, Co, Mn<100ppm, Li, Fe, P>10000ppm, and the atomic ratio of Fe and P is Fe:P=1:0.9~1:1.1, it can be identified as a lithium iron phosphate battery.

[0018] The beneficial effects of the present invention are as follows: the principle of ICP identification is: the principle of ICP testing is to detect the content of each element in the sample, and the main elements of the positive black powder of the lithium iron phosphate battery are Li, Fe, and P, and the main elements of the positive black powder of the ternary battery are Ni, Co, and Mn. Therefore, according to the content of Ni, Co, and Mn in the ICP result, it can be judged whether this batch of batteries are ternary batteries or ternary batteries are mixed in the batteries. Then, according to the atomic ratio of Li, Fe, and P, the structure of Fe and P can be determined, and it can be identified as a lithium iron phosphate battery. The principle of XRD identification is: the main reason for the failure of lithium iron phosphate is the lack of lithium content, that is, lithium vacancies are generated in the structure, but the olivine structure still exists, and the material can be repaired. Therefore, the XRD spectrum of the repairable failed lithium iron phosphate should be similar to the standard card, and there are four diffraction peaks of (101), (140), (112), and (042). Otherwise, it means that the olivine structure is damaged and the material cannot be repaired.

[0019] This identification method is convenient and easy to repeat. The lithium iron phosphate batteries sorted by this identification method were repaired and regenerated, and the gram capacity of the button batteries reached more than 150mAh / g, showing a 100% identification accuracy rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a flow chart of a method for quickly identifying a lithium iron phosphate battery cell with injection failure according to the present invention;

[0021] Figure 2 is the XRD diagram of specific embodiment 1 of the present invention;

[0022] Figure 3 is the XRD diagram of specific embodiment 2 of the present invention;

[0023] Figure 4 This is the XRD diagram of specific embodiment 3 of the present invention. DETAILED DESCRIPTION

[0024] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0025] like Figure 1 As shown, a method for quickly identifying a lithium iron phosphate battery cell with injection failure according to embodiment 1 of the present invention comprises the following steps:

[0026] S1, randomly selecting n cells from the lithium iron phosphate cells to be identified as having failed injection, and disassembling them to obtain the positive electrode sheets;

[0027] S2, calcining and peeling the positive electrode sheet obtained in S1 at high temperature to obtain black powder, and testing the I CP of the black powder;

[0028] S3. Analyze the ICP result to identify whether the lithium iron phosphate battery cell with injection failure to be identified is a lithium iron phosphate battery cell.

[0029] Embodiment 2 of the present invention provides a method for quickly identifying a lithium iron phosphate battery cell with a failed injection. Based on Embodiment 1, if S3 identifies that the lithium iron phosphate battery cell with a failed injection to be identified is a lithium iron phosphate battery cell, then executing step S4;

[0030] S4. Test the black powder obtained in S1 with XRD. If the black powder has four diffraction peaks (101), (140), (112), and (042), the lithium iron phosphate battery cell that has failed injection can be repaired. Otherwise, it cannot be repaired.

[0031] Embodiment 3 of the present invention is a method for quickly identifying a lithium iron phosphate battery cell with injection failure. Based on Embodiment 1, in S1, n=3-1.

[0032] Embodiment 4 of the present invention is a method for quickly identifying a lithium iron phosphate battery cell that has failed injection. Based on Embodiment 1, the temperature of high temperature calcination in S2 is 350-500°C, the insulation time is 0.5-5h, the calcination atmosphere is one of N2 or Ar, and the gas flow rate is 5-10L / min.

[0033] Embodiment 5 of the present invention is a method for quickly identifying a lithium iron phosphate battery cell with failed injection. Based on Embodiment 1, S3 specifically includes: if Ni, Co, Mn<100ppm, Li, Fe, P>10000ppm, and the atomic ratio of Fe and P is Fe:P=1:0.9~1:1.1, it can be identified as a lithium iron phosphate battery cell.

[0034] The principle of ICP identification is as follows: The principle of ICP testing is to detect the content of each element in the sample. The main elements of the positive black powder of lithium iron phosphate batteries are Li, Fe, and P, and the main elements of the positive black powder of ternary batteries are Ni, Co, and Mn. Therefore, according to the content of Ni, Co, and Mn in the ICP results, it can be judged whether this batch of batteries is a ternary battery or a ternary battery is mixed in the battery. Then, according to the atomic ratio of Li, Fe, and P, the structure of Fe and P can be determined, and it can be identified as a lithium iron phosphate battery. The principle of XRD identification is as follows: The main reason for the failure of lithium iron phosphate is the lack of lithium content, that is, lithium vacancies are generated in the structure, but the olivine structure still exists, and the material can be repaired. Therefore, the XRD spectrum of the repairable failed lithium iron phosphate should be similar to the standard card, with four diffraction peaks of (101), (140), (112), and (042). Otherwise, it means that the olivine structure is damaged and the material cannot be repaired.

[0035] This identification method is convenient and easy to repeat. The lithium iron phosphate batteries sorted by this identification method were repaired and regenerated, and the gram capacity of the button batteries reached more than 150mAh / g, showing a 100% identification accuracy rate. Specific embodiment 1

[0037] S1. Randomly select 5 cells from a batch of failed injection cells and manually disassemble them to obtain the positive electrode sheets;

[0038] S2. Place the positive electrode sheet into a box furnace, keep it at 500°C for 3 hours in a 5L / min nitrogen atmosphere to obtain black powder, and test the I CP of the black powder;

[0039] S3, analyzing the I CP results to identify whether the battery cell is lithium iron phosphate;

[0040] S4. Test the black powder obtained in S1 by XRD to identify the repairability of the failed lithium iron phosphate.

[0041] In the specific example 1, the I CP result is: Li: 30701.43ppm, Fe: 349157.41ppm, P: 199156.80ppm, Ni: 9.29ppm, Co: 2.28ppm, Mn: 9.91ppm, Fe:P=1:1.03, which identifies the battery cells as lithium iron phosphate batteries. The XRD results are as follows Figure 2 As shown, (101), (140), (112), and (042) all exist, and this batch of materials can be repaired. The repaired material was tested with a button battery, and its gram capacity was 150.6 mAh / g. The repair capacity was greater than 150.0 mAh / g, indicating that the repair was successful.

[0042] The above test results show that lithium iron phosphate batteries can be successfully repaired after identification, which greatly avoids material uncertainties and thus saves time and economic costs. Specific embodiment 2

[0044] S1, randomly select 3 cells from a batch of failed injection cells and manually disassemble them to obtain the positive electrode sheets;

[0045] S2. Place the positive electrode sheet into a box furnace and keep it at 450°C for 3 hours in a 5L / min nitrogen atmosphere to obtain black powder, and test the I CP of the black powder;

[0046] S3, analyzing the I CP results to identify whether the battery cell is lithium iron phosphate;

[0047] S4. Test the black powder obtained in S1 by XRD to identify the repairability of the failed lithium iron phosphate.

[0048] In specific Example 2, the I CP results are: Li: 35879.41ppm, Fe: 306021.60ppm, P: 186747.80ppm, Ni: 14.75ppm, Co: 10.33ppm, Mn: 58.62ppm, Fe:P=1:1.1, and the battery cells are identified as lithium iron phosphate batteries. The XRD results are as follows Figure 3 As shown, (101), (140), (112), and (042) all exist, and this batch of materials can be repaired. The repaired material was tested with a button battery, and its gram capacity was 151.7 mAh / g. The repair capacity was greater than 150.0 mAh / g, indicating that the repair was successful.

[0049] The above test results show that lithium iron phosphate batteries can be successfully repaired after identification, which greatly avoids material uncertainties and thus saves time and economic costs.

[0050] Specific implementation 3

[0051] S1, randomly select 3 cells from a batch of failed injection cells and manually disassemble them to obtain the positive electrode sheets;

[0052] S2. Place the positive electrode sheet into a box furnace and keep it at 450°C for 2 hours in a 5L / min nitrogen atmosphere to obtain black powder, and test the I CP of the black powder;

[0053] S3, analyzing the I CP results to identify whether the battery cell is lithium iron phosphate;

[0054] S4. Test the black powder obtained in S1 by XRD to identify the repairability of the failed lithium iron phosphate.

[0055] The I CP results in Example 2 are: Li: 44992.03ppm, Fe: 334156.01ppm, P: 183447.88ppm, Ni: 51.67ppm, Co: 23.30ppm, Mn: 62.25ppm, Fe:P=1:0.99, which identifies this batch of batteries as lithium iron phosphate batteries. The XRD results are as follows Figure 4 As shown, (101), (140), (112), and (042) do not exist, and this batch of materials cannot be repaired. After the materials are repaired, button battery tests are performed to verify their repairability. After multiple attempts, the final gram capacity is 145.2 mAh / g. The repair capacity is less than 150.0 mAh / g, indicating that the repair is not successful.

[0056] The above test results show that the lithium iron phosphate battery cell cannot be successfully repaired after identification, and the button battery test also verifies this, which greatly avoids material uncertainty and saves time and economic costs.

[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for quickly identifying a lithium iron phosphate battery cell with injection failure, characterized in that: The steps include: S1. Randomly select n cells from the lithium iron phosphate cells to be identified as having failed injection, and disassemble them to obtain the positive electrode sheets; S2, calcining and peeling the positive electrode sheet obtained in S1 at high temperature to obtain black powder, and testing the ICP of the black powder; S3. Analyze the ICP result to identify whether the lithium iron phosphate battery cell with injection failure to be identified is a lithium iron phosphate battery cell.

2. According to the method of claim 1, the method is characterized in that: If S3 identifies that the to-be-identified lithium iron phosphate battery cell with injection failure is a lithium iron phosphate battery cell, then execute step S4; S4. The black powder obtained in S1 is tested by XRD. If the black powder has four diffraction peaks (101), (140), (112), and (042), the failed lithium iron phosphate battery cell to be identified can be repaired, otherwise it cannot be repaired.

3. A method for quickly identifying a lithium iron phosphate battery cell with injection failure according to claim 1, characterized in that: In the S1, n=3-10.

4. The method for quickly identifying a lithium iron phosphate battery cell with injection failure according to claim 1, characterized in that: The temperature of the high temperature calcination in S2 is 350-500°C, the insulation time is 0.5-5h, the calcination atmosphere is one of N2 or Ar, and the gas flow rate is 5-10L / min.

5. The method for quickly identifying a lithium iron phosphate battery cell with injection failure according to claim 1, characterized in that: The S3 specifically includes: if Ni, Co, Mn<100ppm, Li, Fe, P>10000ppm, and the atomic ratio of Fe and P is Fe:P=1:0.9~1:1.1, it can be identified as a lithium iron phosphate battery cell.