Test method and test equipment for temperature resistance consistency of pressure-sensitive adhesive

By continuously pressing the standard sample of the pressure-sensitive adhesive and the sample to be tested, comparing the maximum or final rebound force, combining segmented pressing and temperature gradient processing, the problem of large error in the temperature resistance consistency evaluation of pressure-sensitive adhesive in the prior art is solved, and the problem of large error in the evaluation of temperature resistance consistency of pressure-sensitive adhesives is realized. Higher test accuracy and accuracy.

CN118937393APending Publication Date: 2024-11-12SHENZHEN MOMA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411013700.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art has a large error and low accuracy when evaluating the temperature resistance consistency of pressure-sensitive adhesives, which cannot accurately reflect the binding state and cross-linking degree of the molecular chains inside the pressure-sensitive adhesives.

Method used

By providing the standard sample of pressure-sensitive adhesive and the sample to be tested, the maximum rebound force or final rebound force is obtained by continuous pressing method, and the force value changes of the standard sample and the sample to be tested are compared. If 90% ≤ T1/T0 ≤ 110% or 90% ≤H1/H0≤110%, then the temperature resistance consistency of the sample to be tested is good. Use segmented pressing and different temperature gradient treatment to detect the force rebound curve of the pressure-sensitive adhesive, analyze the curve overlap to determine the temperature resistance consistency .

Benefits of technology

The accuracy of the temperature resistance consistency test of pressure-sensitive adhesives is improved, and the cohesion and crosslinking degree is intuitively reflected through specific force value data, and the temperature resistance is accurately quantified, error is reduced and testing efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937393A_ABST
    Figure CN118937393A_ABST
Patent Text Reader

Abstract

The invention relates to a method and equipment for testing the temperature resistance consistency of a pressure-sensitive adhesive. In the process of continuously pressing the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive sample to be tested, the maximum resilience force or the final resilience force of the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive sample to be tested can be tested, so that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is evaluated. The temperature resistance of the pressure-sensitive adhesive can be directly quantified through the change of the pressure value generated by pressing the pressure-sensitive adhesive, the difference between the pressure-sensitive adhesive sample to be tested and the pressure-sensitive adhesive standard sample is shown through the specific force value data, and the accuracy is higher. Moreover, the change of the force value can reflect the internal structure, cohesion strength and crosslinking degree of the molecular chain of the pressure-sensitive adhesive. The pressure-sensitive adhesive is treated at different temperature gradients and time gradients, so that the influence of different experimental environments on the mechanical property and cohesion property of the pressure-sensitive adhesive is finally obtained, and the temperature-resistant consistency of the pressure-sensitive adhesive can be intuitively judged according to the coincidence degree of different gradient curves.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of pressure-sensitive adhesive testing, and in particular to a method and equipment for testing the temperature resistance consistency of a pressure-sensitive adhesive. Background Art

[0002] Temperature resistance is a very important technical parameter for evaluating pressure-sensitive adhesives. For example, high-temperature adhesion is an important indicator for evaluating the temperature resistance of pressure-sensitive adhesives. By detecting the bonding force between the molecular chains of the pressure-sensitive adhesive layer under high temperature, the cohesion of the pressure-sensitive adhesive can be judged, thereby inferring whether the pressure-sensitive adhesive is resistant to high temperatures. It is also possible to infer whether the pressure-sensitive adhesive is resistant to high temperatures by bonding it to the object being adhered, testing the adhesion value to the object being adhered at different temperatures, and whether there is residual adhesive on the surface of the object being adhered after tearing it off. However, the above are all evaluations of the high-temperature resistance of pressure-sensitive adhesives by evaluating the viscosity changes of pressure-sensitive adhesives, and cannot accurately reflect the bonding state and degree of cross-linking of the molecular chains inside the pressure-sensitive adhesive. Therefore, there are large errors and low accuracy when evaluating the temperature resistance consistency of pressure-sensitive adhesives. Summary of the invention

[0003] The embodiments of the present application provide a method and equipment for testing the temperature resistance consistency of a pressure-sensitive adhesive, which are intended to improve the problem of large errors and low accuracy when evaluating the temperature resistance consistency of a pressure-sensitive adhesive.

[0004] In the first aspect, an embodiment of the present application provides a method for testing the temperature resistance consistency of a pressure-sensitive adhesive, including: providing a standard sample of a pressure-sensitive adhesive, pressing the standard sample of the pressure-sensitive adhesive to a first preset depth, and pressing at the first preset depth for a first preset time. Obtaining the maximum rebound force T0 of the standard sample of the pressure-sensitive adhesive, or obtaining the final rebound force H0 of the standard sample of the pressure-sensitive adhesive. Providing a pressure-sensitive adhesive sample to be tested, pressing the pressure-sensitive adhesive sample to be tested to a second preset depth, and pressing at the second preset depth for a second preset time. Obtaining the maximum rebound force T1 of the pressure-sensitive adhesive sample to be tested, or obtaining the final rebound force H1 of the pressure-sensitive adhesive sample to be tested. Determine the temperature resistance consistency of the pressure-sensitive adhesive based on the maximum rebound force T0 of the standard sample of the pressure-sensitive adhesive and the maximum rebound force T1 of the pressure-sensitive adhesive sample to be tested. If 90%≤T1 / T0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good; alternatively, the temperature resistance consistency of the pressure-sensitive adhesive is determined based on the final rebound force H0 of the pressure-sensitive adhesive standard sample and the final rebound force H1 of the pressure-sensitive adhesive sample to be tested; if 90%≤H1 / H0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good.

[0005] In some embodiments, the step of pressing the pressure-sensitive adhesive standard sample to a first preset depth and pressing at the first preset depth for a first preset time includes: pressing the pressure-sensitive adhesive standard sample to a first preset depth by means of segmented pressing and pressing at the first preset depth for a first preset time. The step of pressing the pressure-sensitive adhesive sample to be tested to a second preset depth and pressing at the second preset depth for a second preset time includes: pressing the pressure-sensitive adhesive standard sample to a second preset depth by means of segmented pressing and pressing at the second preset depth for a second preset time.

[0006] In some embodiments, the pressure-sensitive adhesive standard sample is pressed to a first preset depth by a segmented pressing method, and is pressed at the first preset depth for a first preset time, including a first stage: the first speed of pressing the pressure-sensitive adhesive standard sample is 4mm / min to 6mm / min, the first depth is 0.2mm to 0.3mm, and the first time of pressing at the first depth is 20s to 30s. The second stage: the second speed of pressing the pressure-sensitive adhesive standard sample is 4mm / min to 6mm / min, the second depth is 0.35mm to 0.5mm, and the second time of pressing at the second depth is 20s to 30s. The third stage: the third speed of pressing the pressure-sensitive adhesive standard sample is 4mm / min to 6mm / min, the third depth is 0.45mm to 0.65mm, and the third time of pressing at the third depth is 20s to 30s.

[0007] In some embodiments, providing a pressure-sensitive adhesive standard sample includes providing a pressure-sensitive adhesive layer and a first protective film, wherein the pressure-sensitive adhesive layer has a first surface and a second surface disposed opposite to each other, and the first surface and the second surface are respectively provided with the first protective film, to obtain a first sample. The first sample is placed under a pressing block for pressing, the pressing temperature is 20° C. to 25° C., and the pressing time is 10 h to 14 h, to obtain the pressure-sensitive adhesive standard sample.

[0008] In some embodiments, providing a pressure-sensitive adhesive sample to be tested includes placing a plurality of the first samples in a baking device, baking them at a preset temperature for a preset time, cooling the baked first samples in an environment at a temperature of 20°C to 25°C, placing the cooled first samples under a pressing block for pressing, the pressing temperature is 20°C to 25°C, and the pressing time is 10h to 14h, to obtain the pressure-sensitive adhesive sample to be tested. The preset temperature includes any temperature between -40°C and 200°C. The preset time includes one or more of 24h, 48h, 72h, 96h, 120h, 144h, and 168h.

[0009] In some embodiments, the first protective film includes any one of a PI film, a PEEK film, a LCP film, a PPS film, or a PSF film.

[0010] In some embodiments, the first protection film has a thickness ranging from 1 μm to 10 μm.

[0011] In some embodiments, the pressure-sensitive adhesive includes at least one of silicone, acrylic adhesive, polyurethane adhesive or rubber.

[0012] In some embodiments, in the first stage, the first speed of pressing the standard pressure-sensitive adhesive sample is 5 mm / min, the first depth is 0.3 mm, and the first duration of pressing at the first depth is 30 s. In the second stage, the second speed of pressing the standard pressure-sensitive adhesive sample is 5 mm / min, the second depth is 0.45 mm, and the second duration of pressing at the second depth is 30 s. In the third stage, the third speed of pressing the standard pressure-sensitive adhesive sample is 5 mm / min, the third depth is 0.6 mm, and the third duration of pressing at the third depth is 30 s.

[0013] In the second aspect, an embodiment of the present application provides a test device for the temperature resistance consistency of a pressure-sensitive adhesive, which is applicable to the test method described in any one of the first aspects, and includes a universal tensile testing machine including a base, and a clamping member arranged opposite to the base along a first direction. A fixed table is arranged on the base, and the fixed table has a third surface facing the clamping member. A sample placement table is arranged on the third surface, and along the second direction, the sample placement table includes a first part and a second part arranged opposite to each other, and a first spacing space is provided between the first part and the second part, and the first part and the second part are used to support the test sample. A pressing member is clamped on the clamping member, and the pressing member is used to press the test sample toward the first spacing space.

[0014] Different from the related art, the embodiment of the present application provides a test method for the temperature resistance consistency of a pressure-sensitive adhesive. In the process of continuously pressing the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive sample to be tested, the pressure-sensitive adhesive will experience continuous changes in pressure value, and the strength of the cohesive force of the pressure-sensitive adhesive can be reflected according to the continuous changes in pressure value. By comparing the maximum resilience or final resilience of the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive sample to be tested, the quality of the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested can be evaluated. The present application can directly quantify the temperature resistance of the pressure-sensitive adhesive by the change in pressure value generated by pressing the pressure-sensitive adhesive, and show the difference between the pressure-sensitive adhesive sample to be tested and the pressure-sensitive adhesive standard sample through specific force value data, with higher accuracy. In addition, the change in force value can directly reflect the internal structure, cohesive strength and cross-linking degree of the pressure-sensitive adhesive molecular chain. By subjecting the pressure-sensitive adhesive to different temperature gradients and time gradients and using segmented compression methods, the force rebound curve of the pressure-sensitive adhesive is detected. Through analysis and comparison of the curves, the influence of the environment of "same temperature but different time or different temperatures but same time" on the mechanical properties and cohesive properties of the pressure-sensitive adhesive is finally obtained. The temperature resistance consistency of the pressure-sensitive adhesive can also be intuitively judged from the degree of overlap of different gradient curves. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] One or more embodiments are exemplarily described by corresponding drawings, which do not constitute limitations on the embodiments. Elements with the same reference numerals in the drawings represent similar elements, and the figures in the drawings do not constitute proportional limitations unless otherwise stated.

[0016] Figure 1 It is a flow chart of some test methods for the temperature resistance consistency of pressure-sensitive adhesives provided in the embodiments of the present application;

[0017] Figure 2 It is a schematic diagram of the structure of some pressure-sensitive adhesive temperature resistance consistency testing equipment provided in the embodiments of the present application;

[0018] Figure 3 It is a schematic diagram of the change of the resilience of the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive test sample with the pressing time in Example 1 of the present application;

[0019] Figure 4 It is a schematic diagram showing the change in the resilience of the medium pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive test sample with the pressing time in comparative example 1 of the present application. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0021] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "several" and "multiple" is more than two, unless otherwise clearly and specifically defined.

[0022] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0023] Reference to "embodiment" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. In addition, the technical features involved in the different embodiments of the present application described below may be combined with each other as long as they do not conflict with each other.

[0024] Pressure sensitive adhesive is a type of adhesive that is sensitive to pressure. It is mainly used to prepare pressure sensitive tapes. The main feature of pressure sensitive adhesive is that it can quickly and durably adhere to the surface of various objects under slight pressure. It does not need to be cured by solvent volatilization, chemical reaction or heating like traditional adhesives to achieve bonding. Pressure sensitive adhesive has the characteristics of strong initial adhesion, long-lasting adhesion, and sensitivity to pressure. It is widely used in the medical field, industrial field and daily necessities.

[0025] The temperature consistency of a pressure-sensitive adhesive refers to the ability of the pressure-sensitive adhesive to maintain stable and consistent initial performance under different temperature conditions. Specifically, when the pressure-sensitive adhesive is used in a high temperature environment or a low temperature environment, if the temperature consistency is good, the viscosity will not fluctuate greatly, and the effective adhesion effect can be maintained within the usable temperature range. The good temperature consistency of a pressure-sensitive adhesive is also reflected in the stable cohesion, and the internal separation or flow of the adhesive layer will not easily occur due to temperature changes. Good temperature consistency is very important for pressure-sensitive adhesives in practical applications. For example, in the automotive manufacturing industry, pressure-sensitive adhesives may face temperature changes in hot summers and cold winters. If the temperature consistency is poor, it may cause problems such as loosening and failure of parts. In electronic equipment, pressure-sensitive adhesives may experience temperature changes due to the heat generated when the equipment is working. If the temperature consistency of the pressure-sensitive adhesive is poor, it may affect the fixation and normal operation of electronic components.

[0026] In the first aspect, the present application embodiment provides a method for testing the temperature resistance consistency of a pressure-sensitive adhesive, please refer to Figure 1 , the test method specifically includes the following steps:

[0027] Step S1: providing a standard sample of a pressure-sensitive adhesive, pressing the standard sample of the pressure-sensitive adhesive to a first preset depth, and pressing at the first preset depth for a first preset time.

[0028] The pressure-sensitive adhesive standard sample is used as a benchmark for measuring the quality of pressure-sensitive adhesive products. In particular, in the embodiments of the present application, the pressure-sensitive adhesive prepared at room temperature is used as the pressure-sensitive adhesive standard sample, because the chemical and physical properties of the pressure-sensitive adhesive at room temperature are relatively stable and not prone to drastic changes, which helps the performance of the sample to remain consistent over a long period of time.

[0029] The first preset depth may be the first preset depth obtained after multiple pressings. For example, the pressure-sensitive adhesive standard sample may be pressed once, twice, three times, four times, etc. to reach the first preset depth.

[0030] In some embodiments, providing a pressure-sensitive adhesive standard sample includes: providing a pressure-sensitive adhesive layer and a first protective film. The pressure-sensitive adhesive layer has a first surface and a second surface that are arranged opposite to each other, and the first surface and the second surface are respectively provided with a first protective film to obtain a first sample. For example, the size of the first sample can be set to 25 mm×25 mm. The prepared first sample needs to be flat without obvious bubbles and wrinkles, the first protective film has no curling, and the edge of the first sample after cutting has no cracks and burrs visible to the naked eye.

[0031] Since the pressure-sensitive adhesive layer tends to become soft and thinner in a high temperature environment, the adhesion is reduced, and the shape retention ability is deteriorated. The support of the first protective film on the pressure-sensitive adhesive can maintain the shape of the pressure-sensitive adhesive layer to a certain extent, so that the experiment can proceed normally and reduce the pollution of the pressure-sensitive adhesive to the equipment. The first protective film needs to have high temperature resistance. During the test, the first protective film will not shrink or change other properties at the experimental temperature. For example, the first protective film includes PI film, PI film is the full name of polyimide film (Polyimide Film); PEEK film, PEEK film is the full name of polyetheretherketone film (Polyetheretherketone Film); LCP film, LCP film is the full name of liquid crystal polymer film (Liquid Crystal Polymer Film); PPS film, PPS film is the full name of polyphenylene sulfide film (Polyphenylene Sulfide Film) or PSF film, PSF film is the full name of polysulfone film (Polysulphone membrane).

[0032] In some embodiments, the first protection film has a thickness ranging from 1 μm to 10 μm.

[0033] In some embodiments, the pressure sensitive adhesive includes at least one of silicone, acrylic, polyurethane or rubber.

[0034] In some embodiments, the pressure-sensitive adhesive layer includes at least one of a silicone layer, an acrylic adhesive layer, a polyurethane adhesive layer, or a rubber layer.

[0035] The first sample is placed under a pressing block for pressing at a temperature of 20°C to 25°C for a time of 10h to 14h to obtain a standard sample of a pressure-sensitive adhesive. The weight of the pressing block may be 2kg to 4kg. During the preparation of the standard sample of the pressure-sensitive adhesive, the preparation environment temperature is maintained at 20°C to 25°C.

[0036] Step S2: obtaining the maximum resilience T0 of the standard sample of the pressure-sensitive adhesive, or obtaining the final resilience H0 of the standard sample of the pressure-sensitive adhesive.

[0037] By pressing the pressure-sensitive adhesive standard sample to a first preset depth, the maximum resilience T0 of the pressure-sensitive adhesive standard sample can be measured. By pressing at the first preset depth for a first preset time, the final resilience H0 of the pressure-sensitive adhesive standard sample can be measured.

[0038] Step S3: providing a pressure-sensitive adhesive sample to be tested, pressing the pressure-sensitive adhesive sample to be tested to a second preset depth, and pressing at the second preset depth for a second preset time.

[0039] During the production process of the pressure-sensitive adhesive test sample, the pressure-sensitive adhesive needs to be placed at a set temperature or time for heating or baking. For example, several pressure-sensitive adhesive test samples may have the same baking temperature but different baking times, or several pressure-sensitive adhesive test samples may have different baking temperatures but the same baking time. The performance and internal structure of the pressure-sensitive adhesive test sample may change to a certain extent at different baking times or temperatures. By comparing the test results of the pressure-sensitive adhesive test sample with the pressure-sensitive adhesive standard sample, the temperature resistance consistency of the pressure-sensitive adhesive can be judged.

[0040] The second preset depth may be the second preset depth obtained after multiple pressings. For example, the pressure-sensitive adhesive sample to be tested may be pressed once, twice, three times, four times, etc. to reach the second preset depth.

[0041] In some embodiments, providing a pressure-sensitive adhesive sample to be tested includes: placing a plurality of first samples in a baking device, baking at a preset temperature for a preset time, cooling the baked first samples in an environment at a temperature of 20°C to 25°C, placing the cooled first samples under a pressing block for pressing, the pressing temperature is 20°C to 25°C, and the pressing time is 10h to 14h, to obtain the pressure-sensitive adhesive sample to be tested. The preset temperature includes any temperature between -40°C and 200°C. The preset time includes one or more of 24h, 48h, 72h, 96h, 120h, 144h, and 168h.

[0042] Exemplarily, several first samples can be placed in a baking device with a temperature of 100°C and a preset baking time of 24h, 48h, 72h, 96h, 120h, 144h, and 168h to obtain several pressure-sensitive adhesive samples to be tested. The aging cycle of the pressure-sensitive adhesive is usually 7 days at room temperature, and the pressure-sensitive adhesive basically tends to be stable, mature or in the best performance state in 7 days. At a baking temperature of 100°C, the test data of each day for 7 consecutive days is obtained, and the temperature resistance consistency of the pressure-sensitive adhesive can be more accurately evaluated. Within the tolerance range of the pressure-sensitive adhesive, multiple temperatures can also be set, for example, at a baking temperature of 80°C, bake for 24h, 48h, 72h, 96h, 120h, 144h, and 168h respectively. At a baking temperature of 120°C, bake for 24h, 48h, 72h, 96h, 120h, 144h, and 168h respectively. By obtaining pressure-sensitive adhesive test samples at multiple baking temperatures and baking times, the temperature resistance consistency of the pressure-sensitive adhesive can be tested more accurately.

[0043] Step S4: obtaining the maximum resilience T1 of the pressure-sensitive adhesive sample to be tested, or obtaining the final resilience H1 of the pressure-sensitive adhesive sample to be tested.

[0044] The maximum resilience T1 of the pressure-sensitive adhesive sample can be measured by pressing the sample to be tested to a second preset depth. The final resilience H1 of the pressure-sensitive adhesive sample can be measured by pressing the sample to be tested to a second preset depth for a second preset time.

[0045] Step S5: Determine the temperature resistance consistency of the pressure-sensitive adhesive based on the maximum resilience T0 of the pressure-sensitive adhesive standard sample and the maximum resilience T1 of the pressure-sensitive adhesive sample to be tested; if 90%≤T1 / T0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good. Alternatively, determine the temperature resistance consistency of the pressure-sensitive adhesive based on the final resilience H0 of the pressure-sensitive adhesive standard sample and the final resilience H1 of the pressure-sensitive adhesive sample to be tested; if 90%≤H1 / H0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good.

[0046] The change in the force generated by the pressure-sensitive adhesive when it is pressed is closely related to the bonding state and cross-linking degree of the molecular chains inside the pressure-sensitive adhesive. When the molecular chains inside the pressure-sensitive adhesive are loosely bonded and the degree of cross-linking is low, the force generated by pressing the pressure-sensitive adhesive can easily cause the molecular chains to shift and rearrange. This will cause the pressure-sensitive adhesive to produce a large deformation under a small pressure, showing a low resistance to compression, that is, low resilience and poor temperature resistance. When the molecular chains inside the pressure-sensitive adhesive are tightly bonded and the degree of cross-linking is high, the movement of the molecular chains is restricted, and a greater force is required to cause significant displacement and deformation. When the pressure-sensitive adhesive can withstand a large pressing force without obvious structural damage, it has strong cohesion and strong compressive resistance, that is, a large resilience and better temperature resistance. The pressure-sensitive adhesive is set to be tested under different temperature conditions, and the temperature resistance consistency of the pressure-sensitive adhesive is evaluated by comparing the size of the resilience under different temperature conditions.

[0047] It should be noted that when evaluating the heat resistance consistency of the pressure-sensitive adhesive, the present application may evaluate only the maximum resilience of the pressure-sensitive adhesive sample to be tested, or the final resilience of the pressure-sensitive adhesive standard sample, or may evaluate both in combination. In the process of continuously pressing the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive sample to be tested, the curve graph of the continuous force value change of the pressure-sensitive adhesive will be intuitively displayed in the embodiment of the present application. By observing the curve graphs of the pressure-sensitive adhesive sample to be tested and the pressure-sensitive adhesive standard sample, the overlap of the two curves can be roughly judged, and the heat resistance consistency of the pressure-sensitive adhesive can be intuitively judged.

[0048] The embodiment of the present application provides a test method for the temperature resistance consistency of a pressure-sensitive adhesive. In the process of continuously pressing a pressure-sensitive adhesive standard sample and a pressure-sensitive adhesive sample to be tested, the pressure-sensitive adhesive will have a continuous change in pressure value, and the strength of the cohesive force of the pressure-sensitive adhesive can be reflected according to the continuous change in pressure value. By comparing the maximum resilience or final resilience of the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive sample to be tested, the quality of the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested can be evaluated. The present application can directly quantify the temperature resistance of the pressure-sensitive adhesive by the change in force value generated by pressing the pressure-sensitive adhesive, and show the difference between the pressure-sensitive adhesive sample to be tested and the pressure-sensitive adhesive standard sample through specific pressure value data, with higher accuracy. When testing, multiple samples can be tested simultaneously, which is simple to operate and improves test efficiency. In addition, the change in force value can directly reflect the internal structure, cohesive strength and cross-linking degree of the pressure-sensitive adhesive molecular chain. By subjecting the pressure-sensitive adhesive to different temperature gradients and time gradients and using segmented compression methods, the force rebound curve of the pressure-sensitive adhesive is detected. Through analysis and comparison of the curves, the influence of the environment of "same temperature but different time or different temperatures but same time" on the mechanical properties and cohesive properties of the pressure-sensitive adhesive is finally obtained. The temperature resistance consistency of the pressure-sensitive adhesive can also be intuitively judged from the degree of overlap of different gradient curves.

[0049] In some embodiments, pressing the pressure-sensitive adhesive standard sample to a first preset depth and pressing at the first preset depth for a first preset time includes: pressing the pressure-sensitive adhesive standard sample to a first preset depth by means of segmented pressing, and pressing at the first preset depth for a first preset time. Pressing the pressure-sensitive adhesive sample to be tested to a second preset depth and pressing at the second preset depth for a second preset time includes: pressing the pressure-sensitive adhesive standard sample to a second preset depth by means of segmented pressing, and pressing at the second preset depth for a second preset time. In the embodiments of the present application, different first preset depths and first preset time can be set for different pressure-sensitive adhesives.

[0050] Pressing the pressure-sensitive adhesive in sections can observe the changes in force values ​​at different stages, and find that the pressure-sensitive adhesive has unstable mutations or unstable conditions within a specific range. In particular, a single press is greatly affected by the outside world, which will reduce the accuracy of the measurement. Pressing in sections can reduce measurement errors and improve measurement accuracy.

[0051] Specifically, pressing the pressure-sensitive adhesive standard sample to a first preset depth by means of segmented pressing, and pressing at the first preset depth for a first preset duration include: the first stage: the first speed of pressing the pressure-sensitive adhesive standard sample is 4mm / min to 6mm / min, the first depth is 0.2mm to 0.3mm, and the first duration of pressing at the first depth is 20s to 30s. The second stage: the second speed of pressing the pressure-sensitive adhesive standard sample is 4mm / min to 6mm / min, the second depth is 0.35mm to 0.5mm, and the second duration of pressing at the second depth is 20s to 30s. The third stage: the third speed of pressing the pressure-sensitive adhesive standard sample is 4mm / min to 6mm / min, the third depth is 0.45mm to 0.65mm, and the third duration of pressing at the third depth is 20s to 30s.

[0052] By using the three-stage pressing method, the pressing error is reduced while saving operating procedures. When the number of pressings is small, such as one press, the pressing process is easily affected by the external environment, which can easily lead to inaccurate measurement results. When pressing more than three times, the pressing process is complicated, and the first preset depth is divided into too many stages, which will result in a small change in the pressure value at each stage, and the change in the pressure value cannot be well observed.

[0053] In some embodiments, in the first stage, the first speed of pressing the standard sample of the pressure-sensitive adhesive is 5 mm / min, the first depth is 0.3 mm, and the first duration of pressing at the first depth is 30 seconds. In the second stage, the second speed of pressing the standard sample of the pressure-sensitive adhesive is 5 mm / min, the second depth is 0.45 mm, and the second duration of pressing at the second depth is 30 seconds. In the third stage, the third speed of pressing the standard sample of the pressure-sensitive adhesive is 5 mm / min, the third depth is 0.6 mm, and the third duration of pressing at the third depth is 30 seconds.

[0054] In a second aspect, an embodiment of the present application provides a pressure-sensitive adhesive temperature resistance consistency testing device 100, which is applicable to the testing method of any embodiment of the first aspect. Figure 2 As shown, the testing device 100 includes a universal tensile testing machine 10 , a fixing table 20 , a sample placing table 30 and a pressing member 40 .

[0055] For the universal tensile testing machine 10, the universal tensile testing machine 10 includes a base 11 and a clamping member 12 arranged opposite to the base 11 along a first direction X. The universal tensile testing machine 10 can be connected to a computer, and an operator can control the operation state of the universal tensile testing machine 10 by inputting relevant parameters on the computer, and the test result data of the universal tensile testing machine 10 can also be displayed on the computer.

[0056] Regarding the fixing platform 20 , the fixing platform 20 is disposed on the base 11 , and the fixing platform 20 has a third surface 21 facing the clamping member 12 .

[0057] For the above-mentioned sample placement table 30, the sample placement table 30 is arranged on the third surface 21, along the second direction Y, the sample placement table includes a first part 31 and a second part 32 arranged opposite to each other, and there is a first spacing space 33 between the first part 31 and the second part 32, and the first part 31 and the second part 32 are used to support the test sample. Optionally, the sample placement table 30 can be arranged at the center position of the fixed table 20 to facilitate pressing by the pressing member 40. Among them, the test sample needs to cover the first spacing space 33, and the two sides of the test sample need to be fixed on the sample placement table 30.

[0058] Regarding the pressing member 40 , the pressing member 40 is clamped by the clamping member 12 , and the pressing member is used to press the test sample toward the first compartment 33 .

[0059] The test method for the temperature resistance consistency of pressure-sensitive adhesive is described below in conjunction with specific embodiments:

[0060] Example 1

[0061] (1) Preparation of a standard sample of a pressure-sensitive adhesive: Provide an acrylic adhesive layer and a PI film, and use a laminating machine to laminate the PI film onto the first surface and the second surface of the acrylic adhesive layer to prepare a first sample. Check the surface of the first sample, which must be flat and free of bubbles and curling at the edges. Place the first sample under a 2kg pressing block at 25°C for 12 hours to obtain a standard sample of a pressure-sensitive adhesive. The raw material of the acrylic adhesive layer is commercially available acrylic adhesive, to which an auxiliary reagent is added.

[0062] (2) Preparing pressure-sensitive adhesive samples to be tested: numbering a number of first samples, placing the numbered first samples in a baking device at a temperature of 130° C. for baking times of 48 h, 96 h, and 168 h, respectively; placing the baked first samples in an environment at a temperature of 25° C. to cool; placing the cooled first samples under a 2 kg pressing block at a temperature of 25° C. for 12 h, to obtain a number of pressure-sensitive adhesive samples to be tested.

[0063] (3) Setting parameters: Turn on the test equipment, connect the universal tensile testing machine to the computer, and set the pressing parameters of the universal tensile testing machine. The pressing process is divided into three stages. Stage 1: The first speed of pressing is 5 mm / min, the first depth is 0.3 mm, and the first duration of pressing at the first depth is 30 s. Stage 2: The second speed of pressing is 5 mm / min, the second depth is 0.45 mm, and the second duration of pressing at the second depth is 30 s. Stage 3: The third speed of pressing is 5 mm / min, the third depth is 0.6 mm, and the third duration of pressing at the third depth is 30 s.

[0064] (4) Testing the standard sample of pressure-sensitive adhesive: fix the standard sample of pressure-sensitive adhesive on the sample placement table, start the testing equipment, obtain the maximum rebound force T0 of the standard sample of pressure-sensitive adhesive, and obtain the final rebound force H0 of the standard sample of pressure-sensitive adhesive.

[0065] (5) Testing the pressure-sensitive adhesive samples: placing a number of pressure-sensitive adhesive samples on a sample placement table, starting the testing equipment, obtaining the maximum resilience T1 of the pressure-sensitive adhesive samples, and obtaining the final resilience H1 of the pressure-sensitive adhesive samples.

[0066] (6) Determine the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested: determine the temperature resistance consistency of the pressure-sensitive adhesive based on the maximum rebound force T0 of the pressure-sensitive adhesive standard sample and the maximum rebound force T1 of the pressure-sensitive adhesive sample to be tested; if 90%≤T1 / T0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good; or, determine the temperature resistance consistency of the pressure-sensitive adhesive based on the final rebound force H0 of the pressure-sensitive adhesive standard sample and the final rebound force H1 of the pressure-sensitive adhesive sample to be tested; if 90%≤H1 / H0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good.

[0067] The test results in Example 1 are as follows Figure 3 As shown in Table 1:

[0068] Table 1 shows the test results of the maximum resilience and final resilience of the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive test sample in Example 1.

[0069]

[0070] According to Table 1 and Figure 3It can be seen that the average value of the maximum resilience T0 of the standard sample in Example 1 is 0.0051N, and the average value of the maximum resilience T1 of the sample 1 to be tested at 130°C and a baking time of 48h is 0.0050N, 90%≤T1 / T0=98%≤110%, indicating that the cohesion of the sample 1 to be tested at 130°C and a baking time of 48h changes little, and the properties are relatively stable. The average value of the maximum resilience T1 of the sample 2 to be tested at 130°C and a baking time of 96h is 0.0049N, 90%≤T1 / T0=96%≤110%, indicating that the cohesion of the sample 2 to be tested at 130°C and a baking time of 96h changes little, and the properties are relatively stable. The average value of the maximum resilience T1 of the sample 3 under 130°C and a baking time of 168h is 0.00515N, and 90%≤T1 / T0=101%≤110%, indicating that the cohesive force of the sample 3 under 130°C and a baking time of 168h changes little and the properties are relatively stable. The pressure-sensitive adhesive tested in Example 1 is acrylic adhesive, and the ratios of the sample 1, the sample 2, and the sample 3 to the standard sample are all within the range of 90% to 110%, indicating that the acrylic adhesive has good temperature resistance consistency.

[0071] It should be noted that the temperature resistance consistency of the acrylic adhesive can also be judged by calculating the ratio of the final resilience of the test samples 1, 2 and 3 to the standard sample.

[0072] Comparative Example 1

[0073] (1) Preparation of a standard sample of a pressure-sensitive adhesive: Provide an acrylic adhesive layer and a PI film, and use a laminating machine to laminate the PI film onto the first surface and the second surface of the acrylic adhesive layer to prepare a first sample. Check the surface of the first sample, which must be flat and free of bubbles and curling at the edges. Place the first sample under a 2kg pressing block at 25°C for 12 hours to obtain a standard sample of a pressure-sensitive adhesive. The raw material of the acrylic adhesive layer is acrylic adhesive, and no auxiliary reagents are added to the acrylic adhesive.

[0074] (2) Preparing pressure-sensitive adhesive samples to be tested: numbering a number of first samples, placing the numbered first samples in a baking device at a temperature of 130° C. for baking times of 48 h, 96 h, and 168 h, respectively; placing the baked first samples in an environment at a temperature of 25° C. to cool; placing the cooled first samples under a 2 kg pressing block at a temperature of 25° C. for 12 h, to obtain a number of pressure-sensitive adhesive samples to be tested.

[0075] (3) Setting parameters: Turn on the test equipment, connect the universal tensile testing machine to the computer, and set the pressing parameters of the universal tensile testing machine. The pressing process is divided into three stages. Stage 1: The first speed of pressing is 5 mm / min, the first depth is 0.3 mm, and the first duration of pressing at the first depth is 30 s. Stage 2: The second speed of pressing is 5 mm / min, the second depth is 0.45 mm, and the second duration of pressing at the second depth is 30 s. Stage 3: The third speed of pressing is 5 mm / min, the third depth is 0.6 mm, and the third duration of pressing at the third depth is 30 s.

[0076] (4) Testing the standard sample of pressure-sensitive adhesive: fix the standard sample of pressure-sensitive adhesive on the sample placement table, start the testing equipment, obtain the maximum rebound force T0 of the standard sample of pressure-sensitive adhesive, and obtain the final rebound force H0 of the standard sample of pressure-sensitive adhesive.

[0077] (5) Testing the pressure-sensitive adhesive samples: placing a number of pressure-sensitive adhesive samples on a sample placement table, starting the testing equipment, obtaining the maximum resilience T1 of the pressure-sensitive adhesive samples, and obtaining the final resilience H1 of the pressure-sensitive adhesive samples.

[0078] (6) Determine the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested: determine the temperature resistance consistency of the pressure-sensitive adhesive based on the maximum rebound force T0 of the pressure-sensitive adhesive standard sample and the maximum rebound force T1 of the pressure-sensitive adhesive sample to be tested; if 90%≤T1 / T0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good; or, determine the temperature resistance consistency of the pressure-sensitive adhesive based on the final rebound force H0 of the pressure-sensitive adhesive standard sample and the final rebound force H1 of the pressure-sensitive adhesive sample to be tested; if 90%≤H1 / H0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good.

[0079] The test results in Comparative Example 1 are as follows Figure 4 As shown in Table 2:

[0080] Table 2 shows the test results of the maximum resilience and final resilience of the pressure-sensitive adhesive standard sample and the pressure-sensitive adhesive test sample in Comparative Example 1.

[0081]

[0082]

[0083] According to Table 2 and Figure 4It can be seen that the average value of the final resilience H0 of the standard sample in comparative example 1 is 0.0047N. The average value of the final resilience H1 of the sample 1 to be tested at 130°C and a baking time of 48h is 0.00635N, H1 / H0=135%≥110%, indicating that the cohesion of the sample 1 to be tested changes greatly under the environment of 130°C and a baking time of 48h, and the properties are unstable. The average value of the final resilience H1 of the sample 2 to be tested at 130°C and a baking time of 96h is 0.00805N, H1 / H0=171%≥110%, indicating that the cohesion of the sample 2 to be tested changes greatly under the environment of 130°C and a baking time of 96h, and the properties are unstable. The average value of the final resilience H1 of the sample 3 under 130°C and 168h baking time is 0.011N, H1 / H0=234%≥110%, indicating that the cohesion of the sample 3 under 130°C and 168h baking time changes greatly and the property is extremely unstable. The pressure-sensitive adhesive tested in Comparative Example 1 is acrylic original adhesive, and the ratios of the samples 1, 2 and 3 to the standard sample are all greater than 110%, indicating that the temperature resistance consistency of the acrylic original adhesive is poor.

[0084] It should be noted that by calculating the ratio of the maximum resilience of the test samples 1, 2 and 3 to the standard sample, the temperature resistance consistency of the acrylic rubber can also be judged.

[0085] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Under the concept of the present application, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present application as described above, which are not provided in detail for the sake of simplicity. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for testing the temperature resistance consistency of a pressure-sensitive adhesive, characterized in that: include: Providing a pressure-sensitive adhesive standard sample, pressing the pressure-sensitive adhesive standard sample to a first preset depth, and pressing at the first preset depth for a first preset time; Obtaining the maximum resilience T0 of the pressure-sensitive adhesive standard sample, or obtaining the final resilience H0 of the pressure-sensitive adhesive standard sample; Providing a pressure-sensitive adhesive sample to be tested, pressing the pressure-sensitive adhesive sample to be tested to a second preset depth, and pressing at the second preset depth for a second preset time; Obtaining the maximum resilience T1 of the pressure-sensitive adhesive sample to be tested, or obtaining the final resilience H1 of the pressure-sensitive adhesive sample to be tested; The temperature resistance consistency of the pressure-sensitive adhesive is determined based on the maximum resilience T0 of the pressure-sensitive adhesive standard sample and the maximum resilience T1 of the pressure-sensitive adhesive sample to be tested; if 90%≤T1 / T0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good; or, The temperature resistance consistency of the pressure-sensitive adhesive is determined based on the final resilience H0 of the pressure-sensitive adhesive standard sample and the final resilience H1 of the pressure-sensitive adhesive sample to be tested; if 90%≤H1 / H0≤110%, it is determined that the temperature resistance consistency of the pressure-sensitive adhesive sample to be tested is good.

2. The testing method according to claim 1, characterized in that: The pressing of the pressure-sensitive adhesive standard sample to a first preset depth and pressing at the first preset depth for a first preset time comprises: pressing the pressure-sensitive adhesive standard sample to a first preset depth and pressing at the first preset depth for a first preset time in a segmented pressing manner; The pressing of the pressure-sensitive adhesive sample to be tested to a second preset depth and pressing at the second preset depth for a second preset time comprises: pressing the pressure-sensitive adhesive standard sample to a second preset depth by segmented pressing and pressing at the second preset depth for a second preset time.

3. The testing method according to claim 2, characterized in that: Pressing the pressure-sensitive adhesive standard sample to a first preset depth by a segmented pressing method, and pressing at the first preset depth for a first preset time, comprises: The first stage: the first speed of pressing the standard pressure-sensitive adhesive sample is 4 mm / min to 6 mm / min, the first depth is 0.2 mm to 0.3 mm, and the first duration of pressing at the first depth is 20 s to 30 s; The second stage: the second speed of pressing the standard pressure-sensitive adhesive sample is 4 mm / min to 6 mm / min, the second depth is 0.35 mm to 0.5 mm, and the second duration of pressing at the second depth is 20 s to 30 s; The third stage: the third speed of pressing the standard pressure-sensitive adhesive sample is 4 mm / min to 6 mm / min, the third depth is 0.45 mm to 0.65 mm, and the third duration of pressing at the third depth is 20 s to 30 s.

4. The testing method according to claim 1, characterized in that: The standard sample of pressure-sensitive adhesive provided includes: Providing a pressure-sensitive adhesive layer and a first protective film, wherein the pressure-sensitive adhesive layer has a first surface and a second surface arranged opposite to each other, and the first surface and the second surface are respectively provided with the first protective film, to obtain a first sample; The first sample is placed under a pressing block for pressing at a pressing temperature of 20° C. to 25° C. for a pressing time of 10 h to 14 h to obtain the pressure-sensitive adhesive standard sample.

5. The testing method according to claim 4, characterized in that: The method of providing a pressure-sensitive adhesive sample to be tested comprises: Placing a plurality of the first samples in a baking device respectively, and baking them at a preset temperature for a preset time, cooling the baked first samples in an environment at a temperature of 20° C. to 25° C., placing the cooled first samples under a pressing block for pressing at a pressing temperature of 20° C. to 25° C. for a pressing time of 10 h to 14 h, to obtain the pressure-sensitive adhesive test sample; The preset temperature includes any temperature between -40°C and 200°C; The preset time includes one or more of 24h, 48h, 72h, 96h, 120h, 144h, and 168h.

6. The testing method according to claim 4, characterized in that: The first protective film includes any one of a PI film, a PEEK film, a LCP film, a PPS film or a PSF film.

7. The testing method according to claim 4, characterized in that: The first protection film has a thickness of 1 μm to 10 μm.

8. The testing method according to any one of claims 1 to 7, characterized in that: The pressure-sensitive adhesive includes at least one of silicone, acrylic adhesive, polyurethane adhesive or rubber.

9. The testing method according to claim 3, characterized in that: The first stage: the first speed of pressing the standard pressure-sensitive adhesive sample is 5 mm / min, the first depth is 0.3 mm, and the first duration of pressing at the first depth is 30 s; The second stage: the second speed of pressing the standard pressure-sensitive adhesive sample is 5 mm / min, the second depth is 0.45 mm, and the second duration of pressing at the second depth is 30 s; The third stage: the third speed of pressing the standard pressure-sensitive adhesive sample is 5 mm / min, the third depth is 0.6 mm, and the third duration of pressing at the third depth is 30 s.

10. A test device for the temperature resistance consistency of a pressure-sensitive adhesive, suitable for the test method according to any one of claims 1 to 9, characterized in that: include: The universal tensile testing machine comprises a base, and a clamping member arranged opposite to the base along a first direction; A fixing platform, disposed on the base, the fixing platform having a third surface facing the clamping member; A sample placement platform is arranged on the third surface, along the second direction, the sample placement platform comprises a first part and a second part which are arranged opposite to each other, a first interval space is provided between the first part and the second part, and the first part and the second part are used to support the test sample; A pressing member is clamped on the clamping member, and the pressing member is used to press the test sample toward the first spacing space.