O3 type sodium ion battery positive electrode material and preparation method and application thereof

By introducing sodium vacancy and Mg double-site doping in O3 type nickel manganese sodium ferromanganate positive electrode material, the problems of voltage hysteresis and slow sodium ion diffusion kinetics are solved, and efficient cycling stability and rate performance are achieved, suitable for the improvement of the Mass production.

CN118943359AActive Publication Date: 2024-11-12CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410990576.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

O3 type nickel sodium ferromanganate cathode material has serious voltage hysteresis and slow sodium ion diffusion kinetics, which limits its application in sodium ion batteries.

Method used

By introducing sodium vacancy in the Na layer, the sodium-depleted component design is used to achieve double-site doping of Mg and transition metal-position. The positive electrode material of O3-type sodium-ion battery is prepared by a one-step high-temperature solid phase method. The chemical formula is NaβMgγ [NixFeyMnzMgaXb] O2, X is Ti or Sn, and the preparation process is simplified by combining ball milling and high-temperature calcining processes.

Benefits of technology

It significantly improves cyclic stability and rate performance, alleviates the problems of voltage hysteresis and slow sodium ion diffusion kinetics, is simple in process and low in cost, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943359A_ABST
    Figure CN118943359A_ABST
Patent Text Reader

Abstract

The invention provides an O3-type sodium-ion battery positive electrode material and a preparation method and application thereof. The chemical formula of the positive electrode material is Na [beta] Mg [gamma] [Ni < x > Fe < y > Mn < z > Mg X ] O < 2 >, wherein 0.8 < = beta < lt >; 1, 0lt; gamma + a < = 0.1, 0 < = b < = 0.1, 0.8 < = x + y + z < = 1, and X is at least one of Ti or Sn. According to the preparation method disclosed by the invention, sodium vacancy is introduced into a Na layer through the design of a sodium-poor component during preparation, so that double-site doping of the sodium site and the transition metal site of Mg is realized, the phase change can be relieved, and the cycling stability and the rate capability of the system material are remarkably improved; furthermore, the problems of serious voltage lag, slow diffusion kinetics of sodium ions and the like of the existing O3 type sodium nickel manganese ferrite can be effectively solved. The preparation method provided by the invention is simple in process, can be obtained by adopting a one-step high-temperature solid-phase method, does not need special atmosphere protection, is high in production efficiency and low in cost, and is suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to an O3 type sodium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] In the past decade, electrochemical energy storage technology has been closely related to our lives, and lithium-ion batteries are widely used in consumer electronics and electric vehicles. However, the continuous growth of market demand has led to a rapid shortage of lithium resources and rising costs, which has limited the further development of lithium-ion batteries and their application in large-scale energy storage. Therefore, it is crucial to find secondary batteries with low costs and abundant resources to fill the gap in the application of lithium-ion batteries. Sodium-ion batteries naturally come into the field of vision of battery researchers. As a homologous element of lithium, sodium has very similar properties and the working mechanism of the battery is exactly the same; secondly, sodium is abundant and widely distributed, and its development will not be restricted by cost and region, creating opportunities for reducing costs and achieving large-scale energy storage. However, sodium ions have a larger ionic radius and slower ion diffusion kinetics, which limits the development of sodium storage materials. Therefore, it is of great significance to develop cathode materials with low cost, high energy density, good cycle stability and rate performance.

[0003] O3-phase sodium nickel manganese ferrite layered oxide has the advantages of high initial sodium content, stable structure, strong controllability of sample ratio and easy preparation, and is considered to be one of the ideal cathode material systems. However, low-nickel sodium nickel manganese ferrite cathode materials have serious voltage hysteresis and slow sodium ion kinetics, which limit their practical application. Element doping modification is currently one of the most widely used methods to improve material properties.

[0004] CN117476917A discloses a positive electrode material with dual-site doping and surface coating of metal phosphate, and its preparation method and application. The positive electrode material comprises a core and a coating layer arranged on the surface of the core, wherein the coating layer comprises at least one of AlPO4, Mg3(PO4)2 or Ca3(PO4)2, and the layered transition metal oxide core material has a general formula of Na α A β Fe x Mn y M z O2, different doping sites can be controlled by controlling the order of adding Mg source, but the co-precipitation preparation process is relatively complicated and not conducive to large-scale production. Summary of the invention

[0005] The purpose of the present invention is to provide an O3 type sodium ion battery positive electrode material and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art. By designing a sodium-poor component, sodium vacancies are introduced into the Na layer, thereby realizing dual-site doping of Mg at the sodium site and the transition metal site, which can effectively solve the problems of severe voltage hysteresis and slow sodium ion diffusion kinetics in the existing O3 type sodium nickel manganese ferrite.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The first object of the present invention is to provide an O3 type sodium ion battery positive electrode material, the chemical formula of the O3 type sodium ion battery positive electrode material is: Na β Mg γ [Ni x Fe y Mn z Mg a X b ]O2; wherein 0.8≤β<1, 0<γ+a≤0.1, 0≤b≤0.1, 0.8≤x+y+z≤1, and X is at least one of Ti or Sn.

[0008] Furthermore, the crystal structure of the O3 phase sodium ion battery positive electrode material includes a hexagonal phase R-3m space group, a unit cell parameter

[0009] The second object of the present invention is to provide a method for preparing the above-mentioned O3 type sodium ion battery positive electrode material, comprising the following specific steps:

[0010] S1. ball-milling and mixing solid compounds containing a sodium source, a nickel source, an iron source, a manganese source, a magnesium source and a titanium source in a certain proportion to obtain a uniformly mixed powder;

[0011] S2, the mixed powder of S1 is pressed into tablets and placed in a muffle furnace for high-temperature calcination, and then taken out and ground to obtain sodium ion battery positive electrode material powder.

[0012] Furthermore, the sodium source is one or more of sodium carbonate, sodium hydroxide, sodium acetate or sodium peroxide; the nickel source is one or more of nickel nitrate, nickel carbonate, nickel acetate, nickel hydroxide or nickel oxide; the iron source is one or more of iron nitrate, iron carbonate, iron acetate, iron hydroxide, ferric oxide or ferroferric oxide; the manganese source is one or more of manganese nitrate, manganese carbonate, manganese acetate, manganese hydroxide, manganese oxide or manganese dioxide; the magnesium source is one or more of corresponding magnesium nitrate, magnesium carbonate, magnesium hydroxide or magnesium oxide; the titanium source is one or more of titanium dioxide, titanium oxalate or titanium hydroxide.

[0013] Furthermore, in step S1, a planetary ball mill is used, the ball milling aid is isopropanol, ethanol or a mixture of isopropanol and ethanol, and the ball milling beads are of two different sizes, with a large ball: small ball mass ratio of 1:2 and a ball mill: raw material mass ratio of 10:1.

[0014] Furthermore, the ball milling beads have diameters of 5 mm and 10 mm, the mass of the ball milling beads is 10 times the mass of the powder, the speed of the ball mill is 250-400 rpm, and the ball milling time is 8-10 h.

[0015] Furthermore, in step S2, the pressure applied during the tableting operation is 10 to 20 MPa.

[0016] Furthermore, the drying temperature of the drying process is 70-100°C CAHNZ, and the drying time is 10-15 hours; the treatment temperature of the heat treatment is 850-950°C, and the treatment time is 10-15 hours.

[0017] The third object of the present invention is to provide a positive electrode comprising the above-mentioned O3 type sodium ion battery positive electrode material.

[0018] A fourth object of the present invention is to provide a sodium ion battery, which comprises the above-mentioned O3 type sodium ion battery positive electrode material or the above-mentioned positive electrode.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The present invention provides an O3 type sodium ion battery positive electrode material, the chemical formula of the O3 type sodium ion battery positive electrode material is: Na β Mg γ [Ni x Fe y Mn z Mg a X b ]O2; wherein 0.8≤β<1, 0<γ+a≤0.1, 0≤b≤0.1, 0.8≤x+y+z≤1, X is at least one of Ti or Sn, and sodium vacancies are introduced into the Na layer through the sodium-poor component design, which helps Mg to enter the sodium site and the transition metal site at the same time, alleviates the phase change of the material during the charge and discharge process, significantly improves the cycle stability and rate performance, and thus alleviates the problems of severe voltage hysteresis and slow sodium ion diffusion kinetics in the existing O3 type sodium nickel manganese ferrite.

[0021] (2) The preparation method provided by the present invention has a simple process and adopts a one-step high-temperature solid phase method to prepare the sodium ion battery positive electrode material with O3 phase Mg dual-site doping, which does not require special atmosphere protection and has high production efficiency. In addition, the raw materials required by the present invention are abundant in reserves, low in cost, non-toxic and environmentally friendly, and suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The SEM image and EDS spectrum of Example 1;

[0023] Figure 2 XRD comparison diagram of Examples 1, 2 and Comparative Example 2;

[0024] Figure 3 This is the XRD structure refinement diagram of Example 1;

[0025] Figure 4 In Example 1, the voltage range is 2.0-4.0V, 1C (160mA g -1 ) 500-cycle long cycle performance test result diagram under current density;

[0026] Figure 5 The first three charge and discharge curves of Example 1 at a voltage range of 2.0 to 4.0 V and a current density of 1 C are shown;

[0027] Figure 6 This is a graph showing the rate performance test results of Example 1. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0029] Example 1

[0030] This embodiment provides an O3 type sodium ion battery positive electrode material (Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.1 O2) preparation method.

[0031] The specific steps are as follows:

[0032] S1: According to the stoichiometric ratio of the design target product, 1.1129g Na2CO3 (excess 5%), 0.2801gNiO, 0.5988g Fe2O3, 1.0058g MnCO3, 0.1458g Mg(OH)2, 0.1997g TiO2 were weighed and placed in an agate ball milling jar, and two kinds of agate ball milling beads were added according to the ball milling bead: raw material mass ratio of 10:1, and the small ball and large ball mass ratio of 2:1. In order to improve the ball milling efficiency and make the raw material mixing more uniform, a certain amount of isopropanol was added as a grinding aid, and the grinding aid was operated at room temperature at a speed of 250rpm for 8h, and stopped for 5min every 30min during the period, and the rotation direction was changed. The grinding aid can also be ethanol or a mixture of isopropanol and ethanol.

[0033] S2: The ball-milled slurry was transferred to a clean petri dish and dried overnight in a forced air drying oven at 70°C. The obtained powder was then pressed into a disc with a diameter of 20 mm and a thickness of 2 mm to obtain an intermediate material.

[0034] S3: The intermediate material is placed in a muffle furnace and sintered at 900 °C for 12 h at a heating rate of 5 °C min -1 , and then cooled to room temperature with the furnace to obtain O3-Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.1 O2 and immediately transferred to an argon-filled glove box for later use.

[0035] Example 2

[0036] This embodiment provides an O3 type sodium ion battery positive electrode material Na 0.8 Ni 0.15 Fe 0.3 Mn 0.4 Mg 0.05 Ti 0.1 O2,

[0037] The specific steps are as follows:

[0038] The operation steps are the same as those in Example 1, except that: the raw material feed ratio in step (S1) is changed to 1.1129 g Na2CO3 (5% excess), 0.2801 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, 0.0729 g Mg(OH)2, 0.1997 g TiO2, and the chemical formula of the obtained positive electrode material is: Na 0.8 Ni 0.15 Fe 0.3 Mn 0.4 Mg 0.05 Ti0.1 O2.

[0039] Example 3

[0040] The operation steps are the same as those in Example 1, except that: the raw material feed ratio in step (S1) is changed to 1.1129 g Na2CO3 (5% excess), 0.2801 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, 0.1458 g Mg(OH)2, 0.0998 g TiO2, and the chemical formula of the obtained positive electrode material is: Na 0.8 Ni 0.15 Fe 0.3 Mn 0.4 Mg 0.1 Ti 0.05 O2.

[0041] Example 4

[0042] This embodiment provides an O3 type sodium ion battery positive electrode material Na 0.8 Ni 0.15 Fe 0.3 Mn 0.4 Mg 0.05 Ti 0.1 O2

[0043] The operation steps are the same as those in Example 1, except that: the raw material feed ratio in step (S1) is changed to 1.2520 g Na2CO3 (5% excess), 0.2801 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, 0.1458 g Mg(OH)2, 0.1997 g TiO2, and the chemical formula of the obtained positive electrode material is: Na 0.9 Ni 0.15 Fe 0.3 Mn 0.4 Mg 0.1 Ti 0.05 O2.

[0044] Example 5

[0045] This embodiment provides an O3 type sodium ion battery positive electrode material Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.09 Sn 0.0 1O2

[0046] The operation steps are the same as those in Example 1, except that: the raw material feeding ratio in step (S1) is changed to 1.1129 g Na2CO3 (5% excess), 0.2801 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, 0.1458 g Mg(OH)2, 0.1797 g TiO2, and 0.0517 g SnC2O4, and the chemical formula of the obtained positive electrode material is: Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.09 Sn 0.01 O2.

[0047] Example 6

[0048] This embodiment provides an O3 type sodium ion battery positive electrode material Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.08 Sn 0.0 2O2.

[0049] The operation steps are the same as those in Example 1, except that: the raw material feeding ratio in step (S1) is changed to 1.1129 g Na2CO3 (5% excess), 0.2801 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, 0.1458 g Mg(OH)2, 0.1597 g TiO2, 0.1034 g SnC2O4, and the chemical formula of the obtained positive electrode material is: Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.08 Sn 0.02 O2.

[0050] Example 7

[0051] This embodiment provides an O3 type sodium ion battery positive electrode material Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.08 Sn 0.0 2O2.

[0052] The operation steps are the same as those in Example 1, except that: the raw material feed ratio in step (S1) is changed to 1.1129 g Na2CO3 (5% excess), 0.2801 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, 0.1458 g Mg(OH)2, 0.1398 g TiO2, and 0.1551 g SnC2O4. The chemical formula of the obtained positive electrode material is: Na 0.8 Ni 0.15 Fe 0.3 Mn 0.35 Mg 0.1 Ti 0.07 Sn 0.03 O2.

[0053] Comparative Example 1

[0054] The operation steps are the same as those in Example 1, except that: the raw material feed ratio in step (S1) is changed to 1.3911 g Na2CO3 (5% excess), 0.2801 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, 0.1458 g Mg(OH)2, 0.1997 g TiO2, and the chemical formula of the obtained positive electrode material is: NaNi 0.15 Fe 0.3 Mn 0.4 Mg 0.1 Ti 0.05 O2.

[0055] Comparative Example 2

[0056] The operation steps are the same as those in Example 1, except that: the raw material feed ratio in step (S1) is changed to 1.1129 g Na2CO3 (5% excess), 0.4668 g NiO, 0.5988 g Fe2O3, 1.0058 g MnCO3, and 0.1997 g TiO2. The chemical formula of the obtained positive electrode material is: Na 0.8 Ni 0.25 Fe 0.3 Mn 0.35 Ti 0.1 O2.

[0057] In order to better illustrate the electrochemical performance of the sodium ion battery positive electrode material prepared by the present invention, the applicant conducted the following research:

[0058] Performance characterization:

[0059] Scanning electron microscope characterization: A scanning electron microscope model SU-3500 produced by HITACHI was used with an accelerating voltage of 15 kV to observe the morphology of the sodium ion battery electrode materials prepared in each implementation case.

[0060] X-ray diffraction (XRD) test: The test was carried out using a D8 Focus X-ray powder diffractometer from Bruker, Japan and Germany, using Cu-Kα as the radiation source with a wavelength of A Ni filter was used, the tube current was 40 mA, the tube voltage was 40 kV, the scanning range was 5° to 90°, the scanning speed was 5° / min, and the step length was 0.05°. The material was placed in a glass slide and flattened, and the glass slide was embedded in the center of the instrument experimental slot for testing; the identification of the phase and the crystal structure information were analyzed by JADE 6.0 software.

[0061] The positive electrode material of the sodium ion battery was characterized by scanning electron microscopy (SEM) and XRD. Examples 1 to 7 all had similar microscopic morphology and structure. Figure 1 As can be seen from the figure, the doped positive electrode material is composed of elliptical grains ranging from several hundred nanometers to several micrometers, with relatively uniform particle size, smooth grain surface, and no residual alkali attached. Moreover, the EDS results show that each element is uniformly doped.

[0062] The X-ray diffraction patterns of the positive electrode materials obtained in Examples 1, 2 and Comparative Example 2 are as follows: Figure 1 The XRD refinement results of Examples 1 and 2 are shown in Table 1, the atomic position information of Example 1 is shown in Table 2, and the XRD structure refinement diagram is shown in Figure 2 shown.

[0063] Table 1. Statistics of unit cell parameters

[0064]

[0065] Table 2. Atomic occupancy information statistics of Example 1

[0066]

[0067] The Mg undoped sample (Comparative Example 2) is a P2 / O3 composite phase, and the Mg doped samples (Examples 1 and 2) are pure O3 phases. In addition, as the doping ratio increases, the unit cell parameters a and b increase, indicating that Mg occupies the transition metal site, while the unit cell parameter c decreases, indicating that Mg occupies the sodium site.

[0068] The ICP results are shown in Table 3. The sodium contents of the samples of Examples 1, 2, 3, 5, 6 and 7 (β=0.8) are all lower than the designed ratio, providing evidence for the sodium-doped Mg occupying the Na site.

[0069] Table 3. Statistics of the content of each element obtained by ICP test

[0070]

[0071]

[0072] refer to Figure 2 The XRD comparison before and after Mg doping and the structure refinement results prove that Mg occupies both the sodium site and the transition metal site.

[0073] In order to better illustrate the electrochemical performance of the sodium ion battery positive electrode material of the present invention, the applicant also conducted the following research:

[0074] Preparation of electrode samples:

[0075] The slurry was prepared with a mass ratio of active material, conductive agent and binder of 7:2:1. 0.07 g of the sodium ion battery positive electrode material sample powder of the present invention and 0.02 g of Ketjen black were weighed and placed in an agate mortar. The powders were ground to make them uniformly mixed, and then 200 μL of polyvinylidene fluoride (PVDF) solution (PVDF and N-methylpyrrolidine (NMP) solution) was added. The concentration of the PVDF solution was 0.05 g mL -1 , then add 200-400μL of NMP, grind and mix thoroughly into slurry, transfer to clean aluminum foil and scrape into a uniform film with a manual applicator. Then dry in a 70-100℃ forced air drying oven for 1h (NMP initially evaporates), transfer to a 110-130℃ vacuum drying oven and dry for 10-15h. Cut into Φ=10mm circular slices with a slicer, finally weigh each electrode and transfer to a glove box for storage.

[0076] The prepared cathode film was assembled into a battery for conventional cycle testing. Metallic sodium was used as the negative electrode, glass fiber membrane (GE Whatman) was used as the separator, and 1.0 mol·L -1 NaClO4 / ethylene carbonate (EC) + propylene carbonate (PC) + 5% fluoroethylene carbonate (FEC) solution (EC: PC = 1: 1 vol% with 5% FEC) was used as the electrolyte and button cells were assembled in an argon glove box. The assembled battery was tested using a battery tester under the following test conditions: the charge and discharge voltage range was 2.0 to 4.0 V, and the current density was 1C for constant current charge and discharge tests.

[0077] The positive electrode materials prepared in the embodiment and the comparative example were respectively used to prepare electrode plates according to the above method, and then the electrochemical performance was tested. The test results are shown in Table 4.

[0078] Table 4. Discharge specific capacity and capacity retention rate after 100 cycles

[0079] Cathode Materials <![CDATA[Discharge specific capacity (mAh g -1 )]]> Capacity retention rate after 100 cycles (%) Example 1 115.8 93.0 Example 2 110.8 84.7 Example 3 116.5 73.0 Example 4 124.1 83.0 Example 5 128.1 96.5 Example 6 129.2 88.4 Example 7 110.9 87.3 Comparative Example 1 132.0 80.0

[0080] The capacity retention rate is the ratio of the 100-cycle discharge capacity to the first-cycle discharge capacity.

[0081] From the comparison of the electrochemical performance data of each embodiment and comparative example 1 in Table 4, it can be seen that Mg dual-site doping can effectively improve the long-cycle performance of the positive electrode material. For example, the capacity retention rate of embodiment 1 is 93%, while that of comparative example 1 is only 80.0%. It is worth noting that the type and content of doping elements have a great influence on the performance of the positive electrode material. The capacity retention rate of embodiment 3 with a low Ti content is even lower than that of comparative example 1, which is only 73.0%. In addition, after replacing a small amount of Ti with Sn (Example 5), the discharge specific capacity increases to 128.1 mAh g -1 , the capacity retention rate increased to 96.5%, but this kind of replacement does not mean the more the better. As the replacement ratio increases, the capacity retention rate decreases slightly.

[0082] refer to Figure 4 The long cycle performance of the sodium ion battery prepared in Example 1 at a current density of 1C is 76.7% after 500 cycles. Figure 1-Figure 3 It can be seen that the Mg dual-site doped cathode material has excellent long-cycle performance, which benefits from the stabilized O3 phase cathode material structure after Mg dual-site doping and the elimination of surface residual alkali.

[0083] refer to Figure 5 As can be seen from the charge and discharge curve of Example 1 in the figure, Mg dual-site doping can effectively alleviate the complex phase transition of the material during the charge and discharge process and smooth the charge and discharge curve.

[0084] refer to Figure 6 , is the rate performance test of Example 1 in the present invention, indicating that Mg dual-site doping can effectively improve the rate performance of the material.

[0085] The present invention provides the above-mentioned O3 phase Mg dual-site doped sodium ion battery positive electrode material and its preparation method and application. The contribution to the prior art lies in adopting a simple one-step high-temperature solid-phase method, through the sodium-poor component design, to obtain a Mg dual-site doped layered oxide positive electrode material, which significantly improves the cycle stability and rate performance of the system material.

[0086] The present invention simultaneously meets the current demand for low cost and long cycle life of positive electrode materials, and is expected to achieve large-scale production.

[0087] For matters not mentioned above, the prior art applies.

[0088] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. An O3 type sodium ion battery positive electrode material, It is characterized in that The chemical formula of the positive electrode material of the O3 type sodium ion battery is: Na β Mg γ [Ni x Fe y Mn z Mg a X b ]O 2 ; wherein 0.8≤β<1, 0<γ+a≤0.1, 0≤b≤0.1, 0.8≤x+y+z≤1, and X is at least one of Ti or Sn.

2. The O3 type sodium ion battery positive electrode material according to claim 1, It is characterized in that The crystal structure of the O3 phase sodium ion battery positive electrode material is a hexagonal phase R-3m space group, and the unit cell parameter parameters 3. A method for preparing an O3 type sodium ion battery positive electrode material as claimed in any one of claims 1 to 2, It is characterized in that The specific steps include: S1. ball-milling and mixing solid compounds containing a sodium source, a nickel source, an iron source, a manganese source, a magnesium source and a titanium source in a certain proportion to obtain a uniformly mixed powder; S2, the mixed powder of S1 is pressed into tablets and placed in a muffle furnace for high-temperature calcination, and then taken out and ground to obtain sodium ion battery positive electrode material powder.

4. The preparation method according to claim 3, It is characterized in that The sodium source is one or more of sodium carbonate, sodium hydroxide, sodium acetate or sodium peroxide; the nickel source is one or more of nickel nitrate, nickel carbonate, nickel acetate, nickel hydroxide or nickel oxide; the iron source is one or more of iron nitrate, iron carbonate, iron acetate, iron hydroxide, ferric oxide or ferroferric oxide; the manganese source is one or more of manganese nitrate, manganese carbonate, manganese acetate, manganese hydroxide, manganese oxide or manganese dioxide; the magnesium source is one or more of corresponding magnesium nitrate, magnesium carbonate, magnesium hydroxide or magnesium oxide; the titanium source is one or more of titanium dioxide, titanium oxalate or titanium hydroxide.

5. The preparation method according to claim 3, It is characterized in that In step S1, a planetary ball mill is used for ball milling and mixing. The ball milling aid is isopropanol, ethanol or a mixture of isopropanol and ethanol. The ball milling beads are of two different sizes, and the mass ratio of large balls to small balls is 1:

2.

6. The preparation method according to claim 5, It is characterized in that The sizes of ball milling beads are 5 mm and 10 mm in diameter, the mass of ball milling beads is 10 times the mass of powder, the speed of ball mill is 250-400 rpm, and the ball milling time is 8-10 h.

7. The preparation method according to claim 3, It is characterized in that In step S2, the pressure applied during the tableting operation is 10 to 20 MPa.

8. The preparation method according to claim 3, It is characterized in that The drying temperature of the drying process is 70-100° C., and the drying time is 10-15 hours; the treatment temperature of the heat treatment is 850-950° C., and the treatment time is 10-15 hours.

9. A positive electrode, It is characterized in that Contains the O3 type sodium ion battery positive electrode material as described in claim 1 or 2.

10. A sodium ion battery, It is characterized in that The sodium ion battery comprises the sodium ion battery positive electrode material according to any one of claims 1 to 2 or the positive electrode according to claim 9.

Citation Information

Patent Citations

  • Positive electrode material and preparation method and application thereof

    CN117476917A

  • Coated oxygen-doped modified sodium ion battery positive electrode material and preparation method thereof

    CN117133906A

  • Double-site metal ion doped nickel iron sodium manganate positive electrode material and preparation method thereof, positive electrode plate and sodium ion battery