Prussian blue positive electrode material and preparation method thereof, positive electrode plate, secondary battery and electric device

By introducing Mn-C coordination and Mn, Fe-Co-N coordination into Prussian blue cathode materials, a manganese-iron-cobalt coexistence structure is formed, which solves the capacity and cycle performance problems of Prussian blue cathode materials and achieves a balance between high voltage and excellent rate performance, making it suitable for sodium-ion batteries.

CN118943360APending Publication Date: 2024-11-12湖州超钠新能源科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410991795.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing Prussian blue cathode materials have lower actual capacity and compaction density than lithium iron phosphate, and manganese-based Prussian blue cathode materials have lower rate performance and cycle performance.

Method used

By introducing Mn and C coordination into Prussian blue-type cathode materials, and using Mn, Fe, and Co coordination with N at the P site, a cathode material with coexisting manganese, iron, and cobalt is formed, which improves structural stability and voltage plateau, and enhances the discharge capacity and cycle performance of the material.

Benefits of technology

It achieves a balance between high voltage, excellent rate performance and cycle performance. The initial discharge capacity at 0.1C is above 212.4 mAh/g, the initial discharge capacity at 1C is above 182.7 mAh/g, and the cycle retention at 1C after 100 cycles is above 84.9%. The preparation method is simple and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943360A_ABST
    Figure CN118943360A_ABST
Patent Text Reader

Abstract

The invention provides a Prussian blue positive electrode material and a preparation method thereof, a positive electrode plate, a secondary battery and an electric device, the molecular formula of the Prussian blue positive electrode material is AxM1-a-b-cCocFeaMnb [Mn (CN) 6] y.zH2O, A is alkali metal, 0 < x < = 2, 0 < y < = 1, 0 < z < = 2, 0 < a < 1, 0 < b < 1, 0 < c < 0.1, and 0.9 < a + b + c < = 1. The preparation method comprises the following steps: carrying out a co-precipitation reaction on cobalt salt, manganese salt, ferric salt, manganous cyanide alkali metal salt and a complexing agent, aging, washing and drying to obtain the Prussian blue positive electrode material. Mn is coordinated with C (R position), Mn, Fe and Co are coordinated with N (P position), the advantage of high capacity of R position Mn is achieved, and structural stability and a voltage platform can be improved by doping P position Fe and Co.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium batteries, and in particular to a Prussian blue positive electrode material and a preparation method thereof, a positive electrode sheet, a secondary battery and an electric device. Background Art

[0002] Sodium-ion batteries are expected to partially replace lithium-ion batteries in the field of large-scale energy storage due to their advantages such as abundant sodium resources, wide distribution and low cost. They are one of the important research directions of the next generation of battery technology. However, sodium ions are larger than lithium ions and diffuse slowly in positive electrode materials. Prussian blue is a sodium-ion positive electrode material with a distinct three-dimensional open structure. Its Na ion channels and lattice gaps are large, which can achieve rapid Na ion deintercalation. It also has the advantages of high charge and discharge platform, high energy density and low cost, which can meet the requirements of large-scale energy storage applications.

[0003] At present, the mainstream Prussian blue cathode material is iron-based cyanide Na x M[Fe(CN)6] has a theoretical capacity of 171 mAh / g, but its actual capacity and compaction density are inferior to those of lithium iron phosphate.

[0004] Therefore, improving the capacity of Prussian blue-based positive electrode materials has become an important direction to solve the pain points of their application. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a Prussian blue-based positive electrode material and a preparation method thereof, a positive electrode plate, a secondary battery and an electrical device. By adopting Mn and C coordination (R position), and simultaneously adopting Mn, Fe and Co and N coordination (P position), it not only has the advantage of high capacity of R-site Mn, but also can improve the structural stability and voltage platform of the positive electrode material by doping with Fe and Co at the P position, and has broad application prospects.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a Prussian blue positive electrode material, wherein the molecular formula of the Prussian blue positive electrode material is A x M 1-a-b-c Co c Fe a Mn b [Mn(CN)6] y ·zH2O, wherein A is an alkali metal, 0<x≤2, 0<y≤1, 0<z≤2, 0<a<1, 0<b<1, 0<c<0.1, 0.9<a+b+c≤1.

[0008] In the present invention, Mn is coordinated with C (R position) to replace the Fe element in the traditional Prussian blue ferrocyanide, and the unit cell volume becomes larger, which is more conducive to Na+ deintercalation, and can achieve three Na + The reversible deintercalation of manganese greatly improves the discharge capacity of the material; however, the introduction of manganese into the R position leads to a decrease in the rate performance and cycle performance of Prussian blue cathode materials. For this reason, the present invention uses Mn, Fe and Co to coordinate with N at the P position, wherein the manganese element can ensure high voltage, iron doping improves conductivity and structural stability, and cobalt doping can cause charge-spin-lattice coupling effect, increase oxidation voltage, and the three work together to achieve the effect of weakening structural distortion during charging and discharging. The present invention realizes a Prussian blue cathode material that can take into account high voltage, excellent rate performance and cycle performance through the specific selection of R and P position elements.

[0009] Specifically, 0<x≤2, for example, it can be 0.01, 0.24, 0.46, 0.68, 0.9, 1.12, 1.34, 1.56, 1.78 or 2, etc.

[0010] 0<y≤1, for example, it can be 0.01, 0.12, 0.23, 0.34, 0.45, 0.56, 0.67, 0.78, 0.89 or 1, etc.

[0011] 0<z≤2, for example, it can be 0.01, 0.24, 0.46, 0.68, 0.9, 1.12, 1.34, 1.56, 1.78 or 2, etc.

[0012] 0<a<1, for example, it can be 0.01, 0.12, 0.23, 0.34, 0.45, 0.56, 0.67, 0.78, 0.89 or 0.9, etc.

[0013] 0<b<1, for example, it can be 0.01, 0.12, 0.23, 0.34, 0.45, 0.56, 0.67, 0.78, 0.89 or 0.9, etc.

[0014] 0<c<0.1, for example, it can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1, etc.

[0015] 0.9<a+b+c≤1, for example, it can be 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99 or 0.99, etc.

[0016] Preferably, the ratio of a to b is a:b=1:99-99:1, for example, it can be 1:99, 1:98, 1:97, 1:96, 1:95, 1:92, 1:90, 1:89, 1:88, 1:87, 1:85, 1:80, 1:70, 1:50, 1:40, 1:30, 1:20, 1:10, 1:5, 1:1, 2:1, 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1, 90:1 or 99:1, etc., preferably a:b=1:9-9:1.

[0017] The present invention preferably has a molar ratio of iron to manganese in the range of 1:9 to 9:1, which can be more conducive to ensuring high voltage while improving conductivity and structural stability of the positive electrode material.

[0018] Preferably, the ratio of c to the sum of a+b is c:(a+b)=(0.005-0.3):1, for example, it can be 0.005:1, 0.01:1, 0.02:1, 0.03:1, 0.05:1, 0.1:1, 0.15:1, 0.2:1, 0.22:1, 0.26:1, 0.28:1 or 0.3:1, etc.

[0019] The present invention preferably has a molar ratio of cobalt to the sum of iron and manganese within the above range, which can better cooperate with iron and manganese to comprehensively improve the electrochemical performance of the positive electrode material.

[0020] Preferably, said A comprises Na and / or K.

[0021] Preferably, M comprises any one of Ni, Cu, Zn, V or Cr or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of Ni and Cu, a combination of Zn and Cu, a combination of Ni and Zn, a combination of V and Cu, a combination of Ni and V, a combination of Cr and V, and a combination of Ni and Cr.

[0022] The present invention further preferably dopes the Prussian blue positive electrode material with a metal element M, thereby further improving the electrochemical performance of the positive electrode material.

[0023] In a second aspect, the present invention provides a method for preparing the Prussian blue positive electrode material according to the first aspect, the preparation method comprising:

[0024] The cobalt salt, manganese salt, iron salt, manganese cyanide alkali metal salt and complexing agent are subjected to coprecipitation reaction, and then aged, washed and dried to obtain the Prussian blue positive electrode material.

[0025] The present invention prepares the Prussian blue positive electrode material by means of a coprecipitation reaction, the preparation process is simple, and the prepared product has excellent performance and broad application prospects.

[0026] Preferably, the alkali metal manganocyanide salt comprises sodium manganocyanide and / or potassium manganocyanide.

[0027] Preferably, the iron salt is a ferrous iron salt and / or a hydrate of a ferrous iron salt.

[0028] Preferably, the ferrous iron salt comprises any one of ferrous acetate, ferrous sulfate, ferrous chloride or ferrous nitrate, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of ferrous acetate and ferrous sulfate, a combination of ferrous chloride and ferrous sulfate, a combination of ferrous acetate and ferrous chloride, and a combination of ferrous nitrate and ferrous sulfate.

[0029] Preferably, the manganese salt comprises a divalent manganese salt and / or a hydrate of a divalent manganese salt.

[0030] Preferably, the divalent manganese salt includes any one of manganese sulfate, manganese nitrate, manganese chloride or manganese acetate, or a combination of at least two of them.

[0031] Preferably, the cobalt salt comprises a divalent cobalt salt and / or a hydrate of a divalent cobalt salt.

[0032] Preferably, the divalent cobalt salt comprises any one of cobalt acetate, cobalt sulfate, cobalt nitrate or cobalt chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of cobalt acetate and cobalt sulfate, a combination of cobalt nitrate and cobalt sulfate, a combination of cobalt acetate and cobalt nitrate, and a combination of cobalt chloride and cobalt sulfate.

[0033] Preferably, the complexing agent comprises any one of sodium hexametaphosphate, triethanolamine, sodium citrate, ascorbic acid, tartaric acid, glucose or ethylenediaminetetraacetic acid, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of sodium hexametaphosphate and triethanolamine, a combination of sodium citrate and triethanolamine, a combination of sodium hexametaphosphate and sodium citrate, a combination of ascorbic acid and triethanolamine, a combination of tartaric acid and triethanolamine, a combination of glucose and triethanolamine, and a combination of tartaric acid and ethylenediaminetetraacetic acid.

[0034] Preferably, a dopant is also added into the coprecipitation reaction.

[0035] Preferably, the dopant comprises any one of nickel salt, copper salt, zinc salt, vanadium salt or chromium salt, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of nickel salt and copper salt, a combination of zinc salt and copper salt, a combination of nickel salt and zinc salt, a combination of vanadium salt and copper salt, a combination of nickel salt and vanadium salt, a combination of chromium salt and copper salt, and a combination of nickel salt and chromium salt.

[0036] Preferably, the nickel salt comprises any one of nickel acetate, nickel sulfate, nickel nitrate or nickel chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of nickel acetate and nickel sulfate, a combination of nickel nitrate and nickel sulfate, a combination of nickel acetate and nickel nitrate, a combination of nickel chloride and nickel sulfate, and a combination of nickel acetate and nickel chloride.

[0037] Preferably, the copper salt comprises any one of copper acetate, copper sulfate, copper nitrate or copper chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of copper acetate and copper sulfate, a combination of copper nitrate and copper sulfate, a combination of copper acetate and copper nitrate, and a combination of copper chloride and copper sulfate.

[0038] Preferably, the zinc salt comprises any one of zinc acetate, zinc sulfate, zinc nitrate or zinc chloride, or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of zinc acetate and zinc sulfate, a combination of zinc nitrate and zinc sulfate, a combination of zinc acetate and zinc nitrate, or a combination of zinc chloride and zinc sulfate.

[0039] Preferably, the vanadium salt comprises any one of vanadium acetate, vanadium sulfate, vanadium nitrate or vanadium chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of vanadium acetate and vanadium sulfate, a combination of vanadium nitrate and vanadium sulfate, a combination of vanadium acetate and vanadium nitrate, and a combination of vanadium chloride and vanadium sulfate.

[0040] Preferably, the chromium salt comprises any one of chromium acetate, chromium sulfate, chromium nitrate or chromium chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of chromium acetate and chromium sulfate, a combination of chromium nitrate and chromium sulfate, a combination of chromium acetate and chromium nitrate, and a combination of chromium chloride and chromium sulfate.

[0041] The present invention has no special limitation on the aging in the above process, and any device and method known to those skilled in the art for aging may be used, and may also be adjusted according to the actual process.

[0042] Preferably, the temperature of the coprecipitation reaction is 0-100°C, for example, it can be 0°C, 12°C, 23°C, 34°C, 45°C, 56°C, 67°C, 78°C, 89°C or 100°C.

[0043] Preferably, the coprecipitation reaction comprises: dissolving an alkali metal manganese cyanide salt in water to obtain a solution A; dissolving a cobalt salt, a manganese salt, an iron salt, a dopant and a complexing agent in water to obtain a solution B; and mixing solution A and solution B in an inert atmosphere to perform a coprecipitation reaction.

[0044] Preferably, the concentration of the alkali metal manganese cyanide salt in the solution A is 0.1-5 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.5 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, 3.5 mol / L, 4.0 mol / L, 4.5 mol / L or 5 mol / L, etc.

[0045] Preferably, the inert atmosphere comprises any one of nitrogen, helium or argon or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of nitrogen and helium, a combination of argon and helium, a combination of nitrogen and argon, and a combination of hydrogen and argon.

[0046] The present invention has no special limitation on the drying in the above process. Any drying device and method known to those skilled in the art can be used, and can also be adjusted according to the actual process, for example, it can be air drying, vacuum drying or oven drying, or a combination of different methods.

[0047] Preferably, the drying temperature is 80-250°C, for example, it can be 80°C, 90°C, 100°C, 120°C, 140°C, 150°C, 162°C, 173°C, 184°C, 195°C, 206°C, 217°C, 228°C, 239°C or 250°C.

[0048] Preferably, the molar ratio of the complexing agent to the alkali metal manganese cyanide is (0.1-10):1, for example, it can be 0.1:1, 1:1, 1.2:1, 1.5:1, 2:1, 2.2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, etc.

[0049] Preferably, the molar ratio of cobalt in the cobalt salt, manganese in the manganese salt and iron in the iron salt is c:b:a, wherein 0<a<1, 0<b<1, 0<c<0.1, 0.9<a+b+c≤1.

[0050] Preferably, the molar ratio of the metal in the dopant to the sum of cobalt in the cobalt salt, manganese in the manganese salt and iron in the iron salt is (0.001-0.1):1, for example, it can be 0.001:1, 0.002:1, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1 or 0.1:1, etc.

[0051] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0052] (1) dissolving an alkali metal salt of manganese cyanide in water to obtain solution A; dissolving a cobalt salt, a manganese salt, an iron salt, a dopant and a complexing agent in water to obtain solution B;

[0053] (2) In an inert atmosphere, solution A and solution B are mixed and subjected to a coprecipitation reaction at 0 to 100° C. to obtain a coprecipitation reaction system;

[0054] (3) The coprecipitation reaction system is aged, the aged system is subjected to solid-liquid separation, and the obtained solid phase is washed and dried at 80-250° C. to obtain the Prussian blue positive electrode material.

[0055] In a third aspect, the present invention provides a positive electrode plate, which includes the Prussian blue positive electrode material described in the first aspect, or the Prussian blue positive electrode material prepared by the preparation method of the Prussian blue positive electrode material described in the second aspect.

[0056] The positive electrode plate provided in the third aspect of the present invention has both high discharge capacity and excellent rate performance and cycle performance.

[0057] The present invention has no special restrictions on other components and structures in the above-mentioned positive electrode plate. Any composition and structure that can be used for the positive electrode plate known to those skilled in the art can be adopted, and can also be adjusted according to the actual process. For example, it can be a method of coating the positive electrode material on the current collector, etc., wherein the conductive agent in the coating slurry can be, for example, any one of SP, acetylene black, Ketjen black, VGCF, CNTs or graphene, or a combination of at least two of them.

[0058] In a fourth aspect, the present invention provides a secondary battery, wherein the secondary battery comprises the positive electrode sheet described in the third aspect.

[0059] The secondary battery provided by the fourth aspect of the present invention has high capacity, good cycle performance and long service life.

[0060] The present invention has no special restrictions on other components and structures in the secondary battery. Any components and structures that can be used for secondary batteries and are known to those skilled in the art can be used. They can also be adjusted according to the actual process. For example, the negative electrode can be a sodium sheet, and the electrolyte can be a sodium hexafluorophosphate electrolyte.

[0061] In a fifth aspect, the present invention provides an electrical device, wherein the electrical device comprises the secondary battery described in the fourth aspect.

[0062] The present invention has no special restrictions on other components and structures in the above-mentioned electrical device. Any device requiring electricity known to those skilled in the art can be used, and can also be adjusted according to actual conditions, for example, the electrical device is an electronic watch, etc.

[0063] Compared with the prior art, the present invention has at least the following beneficial effects:

[0064] (1) The Prussian blue positive electrode material provided by the present invention can be used to replace the existing positive electrode materials of sodium ion batteries and has good application prospects;

[0065] (2) The Prussian blue positive electrode material provided by the present invention introduces iron ions and cobalt ions into the manganese-based Prussian blue material by regulating the composition, and synergizes with manganese ions to form a positive electrode material in which manganese, iron and cobalt coexist. The synergistic effect of MnC6, MnN6, FeN6, and CoN6 octahedra in the structure improves the stability of the crystal structure, and while achieving high capacity, improves the poor rate performance and cycle performance of the Prussian blue positive electrode material. Under preferred conditions, the battery made of the Prussian blue positive electrode material has an initial discharge capacity of more than 212.4 mAh / g at 0.1C, an initial discharge capacity of more than 182.7 mAh / g at 1C, and a cycle retention rate of more than 84.9% at 100 cycles.

[0066] (3) The preparation method of the Prussian blue positive electrode material provided by the present invention is simple and easy to industrialize and mass produce. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] Figure 1 This is the XRD diagram of the Prussian blue positive electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0068] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0069] Example 1

[0070] This embodiment provides a Prussian blue positive electrode material, wherein the molecular formula of the Prussian blue positive electrode material is Na 1.91 Ni 0.02 Co 0.08 Fe 0.15 Mn 0.75 [Mn(CN)6] 0.98 ·1.56H2O.

[0071] This embodiment also provides a method for preparing the Prussian blue positive electrode material, the preparation method comprising the following steps:

[0072] (1) dissolving sodium manganese cyanide in water to obtain solution A having a sodium manganese cyanide concentration of 0.3 mol / L; dissolving nickel sulfate, cobalt acetate, manganese acetate, iron acetate and sodium hexametaphosphate in water to obtain solution B; wherein the molar ratio of sodium hexametaphosphate to sodium manganese cyanide is 0.5:1; and the total concentration of metal salts in solution B is 0.35 mol / L;

[0073] (2) In an argon atmosphere (inert atmosphere), solution A and solution B are introduced into a reaction vessel at the same time, and a coprecipitation reaction is carried out at 50° C. until the particle size reaches 5 μm, thereby obtaining a coprecipitation reaction system;

[0074] (3) The coprecipitation reaction system was aged at 25° C. for 24 h, the aged system was filtered, and the obtained solid phase was washed and dried at 80° C. to obtain the Prussian blue positive electrode material (its XRD pattern is shown in FIG. Figure 1 shown).

[0075] Example 2

[0076] This embodiment provides a Prussian blue positive electrode material, wherein the molecular formula of the Prussian blue positive electrode material is Na 1.89 V 0.05 Co 0.15 Fe 0.4 Mn 0.4 [Mn(CN)6] 0.98 1.32H2O.

[0077] This embodiment also provides a method for preparing the Prussian blue positive electrode material, the preparation method comprising the following steps:

[0078] (1) dissolving sodium manganese cyanide in water to obtain solution A having a sodium manganese cyanide concentration of 5 mol / L; dissolving vanadium sulfate, cobalt nitrate, manganese acetate, ferric chloride trihydrate and sodium citrate in water to obtain solution B; wherein the molar ratio of sodium citrate to sodium manganese cyanide is 0.5:1; and the total concentration of metal salts in solution B is 1.1 mol / L;

[0079] (2) In a nitrogen atmosphere (inert atmosphere), solution A and solution B are introduced into a reaction vessel at the same time, and a coprecipitation reaction is carried out at 80° C. until the particle size reaches 10 μm, thereby obtaining a coprecipitation reaction system;

[0080] (3) The coprecipitation reaction system is aged at 30° C. for 32 h, the aged system is filtered, and the obtained solid phase is washed and dried at 250° C. to obtain the Prussian blue positive electrode material.

[0081] Example 3

[0082] This embodiment provides a Prussian blue positive electrode material, wherein the molecular formula of the Prussian blue positive electrode material is Na 1.93 Cu 0.01 Co 0.09 Fe 0.45 Mn 0.45 [Mn(CN)6] 0.98 1.48H2O.

[0083] This embodiment also provides a method for preparing the Prussian blue positive electrode material, the preparation method comprising the following steps:

[0084] (1) dissolving sodium manganese cyanide in water to obtain solution A having a sodium manganese cyanide concentration of 0.35 mol / L; dissolving cobalt nitrate, manganese acetate, copper sulfate, ferric chloride trihydrate and sodium citrate in water to obtain solution B; wherein the molar ratio of sodium citrate to sodium manganese cyanide is 3:1; and the total concentration of metal salts in solution B is 0.5 mol / L;

[0085] (2) In a nitrogen atmosphere (inert atmosphere), solution B is introduced into solution A, and a coprecipitation reaction is carried out at 15° C. until the particle size reaches 2 μm, thereby obtaining a coprecipitation reaction system;

[0086] (3) The coprecipitation reaction system is aged at 20° C. for 35 h, the aged system is filtered, and the obtained solid phase is washed and dried at 150° C. to obtain the Prussian blue positive electrode material.

[0087] Example 4

[0088] This embodiment provides a Prussian blue positive electrode material. The ratio of c to the sum of a+b is high, specifically 0.5:1. That is, the Prussian blue positive electrode material is Na 1.91 Ni 0.02 Co 0.3 Fe 0.1 Mn 0.5 [Mn(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0089] Example 5

[0090] This embodiment provides a Prussian blue positive electrode material. The ratio of c to the sum of a+b is relatively low, specifically 0.0045:1. That is, the Prussian blue positive electrode material is Na 1.91 Ni 0.02 Co 0.004 Fe 0.163 Mn 0.733 [Mn(CN)6]0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0091] Example 6

[0092] This embodiment provides a Prussian blue positive electrode material. The Prussian blue positive electrode material is composed of Na 1.91 Ni 0.02 Co 0.08 Fe 0.05 Mn 0.85 [Mn(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0093] Example 7

[0094] This embodiment provides a Prussian blue positive electrode material. The Prussian blue positive electrode material is composed of Na 1.91 Ni 0.02 Co 0.08 Fe 0.85 Mn 0.05 [Mn(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0095] Example 8

[0096] This embodiment provides a Prussian blue positive electrode material. The Prussian blue positive electrode material is the same as that of Embodiment 1 except that copper sulfate is not added, that is, the final product does not contain copper, and the details are not repeated here.

[0097] Comparative Example 1

[0098] This comparative example provides a Prussian blue positive electrode material, wherein the Prussian blue positive electrode material is replaced by sodium ferrocyanide except that sodium manganese cyanide is replaced by sodium ferrocyanide. 1.91 Ni 0.02 Co 0.08 Fe 0.15 Mn 0.75 [Fe(CN)6] 0.98 ·1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0099] Comparative Example 2

[0100] This comparative example provides a Prussian blue positive electrode material, wherein the Prussian blue positive electrode material is replaced by sodium cobalt cyanide except that sodium manganese cyanide is replaced by sodium cobalt cyanide, that is, the Prussian blue positive electrode material is Na 1.91 N i0.02 Co 0.08 Fe 0.15 Mn 0.75 [Co(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0101] Comparative Example 3

[0102] This comparative example provides a Prussian blue positive electrode material, wherein the Prussian blue positive electrode material does not contain cobalt acetate, that is, the final product does not contain cobalt, that is, the Prussian blue positive electrode material is Na 1.91 Ni 0.1 Fe 0.15 Mn 0.75 [Mn(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0103] Comparative Example 4

[0104] This comparative example provides a Prussian blue positive electrode material, wherein the Prussian blue positive electrode material does not contain manganese acetate, that is, the metal coordinated with N in the final product does not contain manganese, that is, the Prussian blue positive electrode material is Na 1.91 Ni 0.02 Co 0.08 Fe 0.9 [Mn(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0105] Comparative Example 5

[0106] This comparative example provides a Prussian blue positive electrode material, wherein the Prussian blue positive electrode material does not contain iron acetate, that is, the metal coordinated with N in the final product does not contain iron, that is, the Prussian blue positive electrode material is Na 1.91 Ni 0.02 Co 0.08 Mn 0.9 [Mn(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0107] Comparative Example 6

[0108] This comparative example provides a Prussian blue positive electrode material, wherein the Prussian blue positive electrode material is replaced with copper acetate in an equal amount except that manganese acetate is replaced with copper acetate, that is, the Prussian blue positive electrode material is Na 1.91 Ni0.02 Co 0.08 Fe 0.15 Cu 0.75 [Mn(CN)6] 0.98 Except for 1.56H2O, the rest are the same as those in Example 1 and will not be described again.

[0109] Preparation and testing of the battery: The positive electrode material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 8:1:1 and dissolved in N-methylpyrrolidone (NMP) and mixed evenly; then, the slurry was applied on aluminum foil with a coater and dried in a vacuum drying oven at 80°C for 8 hours. Finally, the aluminum foil was punched into 1.13 cm 2 The positive electrode sheet was obtained by forming a circular shape. The obtained electrode sheet was used as the positive electrode, the sodium metal sheet was used as the counter electrode, and a porous polypropylene membrane (Celgard2400, USA) was used as a separator to separate the positive electrode and the counter electrode. The button cell was assembled in an argon glove box. The cycle performance test was carried out using a battery test system at a rate of 0.1C and 0.5C at 2-4V and 25°C. The test results are shown in Table 1.

[0110] Table 1

[0111]

[0112]

[0113] From Table 1, we can see the following points:

[0114] (1) It can be seen from Examples 1 to 3 that the present invention adopts Mn coordinated with C (R position) and Mn, Fe and Co coordinated with N (P position), which not only has the advantage of high capacity of R-site Mn, but also improves structural stability and voltage platform by doping Fe and Co at P position, wherein the first discharge capacity at 0.1C is above 212.4 mAh / g, the first discharge capacity at 1C is above 182.7 mAh / g, and the cycle retention rate at 1C for 100 weeks is above 84.9%;

[0115] (2) Combining Example 1 and Examples 4 to 5, it can be seen that in Example 1, c / (a+b) is 0.089:1, compared with 0.5:1 and 0.0045:1 in Examples 4 to 5, respectively. In Example 1, the first discharge capacity at 0.1C is 230.7 mAh / g, the first discharge capacity at 1C is 200.7 mAh / g, and the cycle retention rate of 100 cycles @ 1C is 85.4%. In Example 4, the performance is not significantly improved compared with Example 1, and the high Co content leads to increased costs; in Example 5, the synergistic effect between Mn, Fe and Co is weakened, and the cycle performance is lower than that of Example 1, wherein the cycle retention rate of 100 cycles @ 1C in Example 5 is only 73.6%;

[0116] (3) Combining Example 1 and Examples 6 to 7, it can be seen that in Example 1, a:b=5:1, compared with 17:1 and 1:17 in Examples 6 to 7, respectively, the first discharge capacity at 0.1C in Example 1 is 230.7 mAh / g, the first discharge capacity at 1C is 200.7 mAh / g, and the 100-week cycle @1C retention rate is 85.4%, while the 100-week cycle @1C retention rates in Examples 6 to 7 are only 58.5% and 74.2%, respectively, and the first discharge capacity at 1C is only 133.7 mAh / g and 164.3 mAh / g, respectively. This shows that the present invention preferably has a:b in a specific range, which can better improve the cycle performance and ensure the discharge capacity at the same time;

[0117] (4) Based on Example 1 and Example 8, it can be seen that the present invention further preferably adds doping elements to the Prussian blue positive electrode material, which can better improve the cycle performance and gram capacity;

[0118] (5) Combining Example 1 and Comparative Examples 1 to 6, it can be seen that in Comparative Example 1, the element coordinated with C is replaced with Fe, resulting in a theoretical capacity reduction from 250 mAh / g to 170 mAh / g, and the final capacity is not as good as that in Example 1; in Comparative Example 2, sodium manganese cyanide is replaced with sodium cobalt cyanide, and the theoretical capacity is reduced from 250 mAh / g to 170 mAh / g, and the final capacity is not as good as that in Example 1; in Comparative Examples 3 to 6, the elements coordinated with N are reduced respectively, resulting in a decrease in the synergistic effect between the four elements and a significant decrease in the cycle performance. This shows that the present invention can simultaneously have excellent cycle performance and specific capacity by adopting Mn coordinated with C (R position) and Mn, Fe and Co coordinated with N (P position), and has broad application prospects.

[0119] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A Prussian blue positive electrode material, characterized in that: The molecular formula of the Prussian blue positive electrode material is A x M 1-a-b-c Co c Fe a Mn b [Mn(CN)6] y ·zH2O, wherein A is an alkali metal, 0<x≤2, 0<y≤1, 0<z≤2, 0<a<1, 0<b<1, 0<c<0.1, 0.9<a+b+c≤1.

2. The Prussian blue positive electrode material according to claim 1, characterized in that The ratio of a to b is a:b=1:99 to 99:1, preferably a:b=1:9 to 9:1; Preferably, the ratio of c to the sum of a+b is c:(a+b)=(0.005-0.3):

1.

3. The Prussian blue positive electrode material according to claim 1 or 2, characterized in that: Said A comprises Na and / or K; Preferably, the M includes any one of Ni, Cu, Zn, V or Cr, or a combination of at least two thereof.

4. A method for preparing the Prussian blue positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: The cobalt salt, manganese salt, iron salt, manganese cyanide alkali metal salt and complexing agent are subjected to coprecipitation reaction, and then aged, washed and dried to obtain the Prussian blue positive electrode material.

5. The preparation method according to claim 4, characterized in that: The manganous cyanide alkali metal salt includes sodium manganous cyanide and / or potassium manganous cyanide; Preferably, the iron salt is a divalent iron salt and / or a hydrate of a divalent iron salt; Preferably, the manganese salt comprises a divalent manganese salt and / or a hydrate of a divalent manganese salt; Preferably, the cobalt salt comprises a divalent cobalt salt and / or a hydrate of a divalent cobalt salt; Preferably, the complexing agent includes any one of sodium hexametaphosphate, triethanolamine, sodium citrate, ascorbic acid, tartaric acid, glucose or ethylenediaminetetraacetic acid, or a combination of at least two thereof.

6. The preparation method according to claim 4 or 5, characterized in that: A dopant is also added to the coprecipitation reaction; Preferably, the dopant includes any one of nickel salt, copper salt, zinc salt, vanadium salt or chromium salt, or a combination of at least two of them.

7. The preparation method according to claim 4, characterized in that: The temperature of the coprecipitation reaction is 0 to 100° C. Preferably, the coprecipitation reaction comprises: dissolving an alkali metal salt of manganese cyanide in water to obtain a solution A; dissolving a cobalt salt, a manganese salt, an iron salt, a dopant and a complexing agent in water to obtain a solution B; mixing solution A and solution B in an inert atmosphere to perform a coprecipitation reaction; Preferably, the concentration of the alkali metal manganocyanide salt in the solution A is 0.1 to 5 mol / L; Preferably, the inert atmosphere comprises any one of nitrogen, helium or argon, or a combination of at least two thereof; Preferably, the drying temperature is 80 to 250°C; Preferably, the molar ratio of the complexing agent to the alkali metal manganese cyanide salt is (0.1-10):1; Preferably, the molar ratio of the metal in the dopant to the sum of cobalt in the cobalt salt, manganese in the manganese salt and iron in the iron salt is (0.001-0.1):

1.

8. A positive electrode sheet, characterized in that: The positive electrode plate comprises the Prussian blue positive electrode material according to any one of claims 1 to 3, or the Prussian blue positive electrode material prepared by the method for preparing the Prussian blue positive electrode material according to any one of claims 4 to 7.

9. A secondary battery, characterized in that: The secondary battery comprises the positive electrode sheet according to claim 8.

10. An electrical device, characterized in that: The electric device comprises the secondary battery according to claim 9.

Citation Information

Cited By

  • Preparation method and application of high-manganese Prussian white material

    CN120398089A