Rechargeable water system magnesium ion battery with positive electrode and negative electrode made of organic materials

By using organic positive and negative electrode materials and high conductivity water/organic solvent mixed electrolyte in rechargeable water-based magnesium ion batteries, the capacity and stability of the existing batteries are solved, and a safe and economical energy storage effect is achieved.

CN118943520APending Publication Date: 2024-11-12SHAOXING INST OF NEW ENERGY & MOLECULAR ENG SHANGHAI JIAO TONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411031766.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing rechargeable magnesium ion batteries have lower specific capacity, poor circulation stability, and the organic electrolyte is highly toxic, which limits its further development.

Method used

Use a rechargeable water-based magnesium ion battery in which both positive and negative electrodes are organic materials, use an organic material with a carbonyl group or multiple active sites as the active substance of the positive and negative electrode, and use a mixed electrolyte with magnesium ions and an organic solvent as the electrolyte as the electrolyte The liquid combines conductive agent and binder to form a high conductivity electrolyte.

Benefits of technology

It realizes a low-cost and high-safe energy storage system, improves the specific capacity and cycle stability of the battery, and meets the needs of large-scale energy storage systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943520A_ABST
    Figure CN118943520A_ABST
Patent Text Reader

Abstract

The invention discloses a rechargeable aqueous magnesium ion battery with organic materials as a positive electrode and a negative electrode, and belongs to the technical field of magnesium ion batteries, the rechargeable aqueous magnesium ion battery comprises a positive electrode, a negative electrode and an electrolyte, and is characterized in that the positive electrode active material is an organic material containing a plurality of active sites or carbonyl; the negative active material is a carbonyl-containing organic material; the electrolyte is a water / organic solvent mixed electrolyte containing magnesium ions, and the concentration of the magnesium ions in the electrolyte is 0.01 mol L <-1 > to 2.0 mol L <-1 >; the selected organic positive and negative electrode materials can make up for the defect of slow dynamics of magnesium ions in a magnesium storage material due to high charge density caused by slightly small radius of the magnesium ions in a magnesium ion battery; the advantages of a magnesium ion battery and an aqueous battery are embodied; therefore, the system can be continuously developed into a large-scale energy storage system, and meets the requirements of a novel energy storage system at present.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rechargeable batteries, and in particular relates to a rechargeable aqueous magnesium ion battery in which both positive and negative electrodes are made of organic materials. Background Art

[0002] With the popularization of smart phones, computers, and electric vehicles, the public's requirements for energy storage devices are getting higher and higher. As a widely used lithium-ion battery, it is now facing the problems of uneven distribution of required metal resources such as lithium, cobalt, and nickel, scarce production, and high prices. Therefore, it is urgent to develop the next generation of energy storage systems. Magnesium metal is abundant in nature, cheaper than lithium metal, and has stable chemical properties. The pollution of metal and metal oxide-based electrode materials to the environment and the shortage of resources have restricted the development of the battery industry. Organic electrode materials have attracted widespread attention due to their safety, low cost, easy recycling, and sustainable development. The use of organic materials for both positive and negative electrodes can effectively reduce battery costs. Since organic electrolytes are highly toxic and have safety issues, and pure water electrolytes have a narrow electrochemical window, both hinder the further development of metal ion batteries. Here, we combine organic materials and aqueous electrolytes to form a rechargeable aqueous magnesium ion battery that takes advantage of both. Summary of the invention

[0003] The technical problem to be solved by the present invention is that the rechargeable magnesium ion battery in the prior art has a low specific capacity, poor cycle stability, and highly toxic organic electrolyte. The present invention provides a rechargeable aqueous magnesium ion battery based on organic positive and negative electrodes with low cost, wide source of raw materials, and high safety.

[0004] The present invention solves the above technical problems through the following technical means:

[0005] A rechargeable aqueous magnesium ion battery in which both positive and negative electrodes are organic materials, characterized in that: it comprises a positive electrode, a negative electrode, and an electrolyte, wherein the positive electrode active material is an organic material having a carbonyl group or multiple active sites; the negative electrode active material is an organic material having a carbonyl group; the electrolyte is a mixed electrolyte of water and an organic solvent containing magnesium ions, and the magnesium ion concentration in the electrolyte is 0.01 mol L -1 ~2.0mol L -1 .

[0006] Further settings are:

[0007] The positive electrode includes a conductive agent and a binder in addition to the positive electrode active material, and the negative electrode includes a conductive agent and a binder in addition to the negative electrode active material.

[0008] The conductive agent is any one of carbon black, acetylene black and Ketjen black.

[0009] The binder is any one of polyvinylidene fluoride, polytetrafluoroethylene and sodium carboxymethyl cellulose.

[0010] The organic positive electrode material having a carbonyl group is any one of 1,4,5,8-naphthalenetetracarboxylic anhydride (abbreviated as NTCDA) and 3,4,9,10-perylenetetracarboxylic dianhydride (abbreviated as PTCDA); the organic positive electrode material having multiple active sites is N1,N1'-(1,4-phenylene)bis(N1-(4-aminophenyl)benzene-1,4-diamine) (abbreviated as TP).

[0011] The organic negative electrode material having a carbonyl group is any one of 3,4,9,10-perylenetetracarboxylic diimide (PTCDI for short), 3,4,9,10-perylenetetracarboxylic dianhydride (PTCDA for short), 1,4,5,8-naphthalene diimide (NTCDI for short), 1,4,5,8-naphthalenetetracarboxylic anhydride (NTCDA for short), and anthraquinone (PAQ for short).

[0012] The magnesium salt of the electrolyte is one or more of magnesium chloride, magnesium fluoride, magnesium bromide, magnesium iodide, magnesium borohydride, magnesium perchlorate, magnesium nitrate, magnesium sulfate, magnesium chromate, magnesium acetate, magnesium hexafluoride, bis(hexamethyldisilazide)magnesium, bis(trifluoromethanesulfonyl)imide magnesium, bis(fluorosulfonyl)imide magnesium and magnesium trifluoromethanesulfonate.

[0013] The volume ratio of the organic solvent in the electrolyte is 0.1 to 99.0%, and the organic solvent is one or more of polyethylene glycol (PEG), polyethylene oxide (PEO), acetonitrile, ether, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dioxane, polyethylene glycol dimethyl ether, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dimethyl ether, diethyl ether, methyl formate, ethyl acetate, methyl propionate, ethyl propionate, butyl propionate, and ethyl butyrate.

[0014] The second aspect of the present invention aims to provide a method for preparing a rechargeable aqueous magnesium ion battery in which both the positive and negative electrodes are organic materials, comprising the following steps:

[0015] (1) Preparation of positive electrode

[0016] The positive electrode active material, the conductive agent and the binder are mixed in proportion, ball-milled to obtain a homogenous slurry, coated on the positive electrode collector, and dried to prepare a positive electrode sheet;

[0017] (2) Preparation of negative electrode

[0018] The negative electrode active material, the conductive agent and the binder are mixed in proportion, ball-milled to obtain a homogenous slurry, coated on the negative electrode current collector, and dried to prepare a negative electrode sheet;

[0019] (3) Assembly of rechargeable aqueous magnesium ion batteries

[0020] The positive electrode and negative electrode prepared above are assembled together with a separator and an electrolyte to form a rechargeable aqueous magnesium ion battery.

[0021] Preferably:

[0022] In step (1):

[0023] The positive electrode active material, the conductive agent and the binder are mixed in a mass ratio of 7:2:1.

[0024] In step (2):

[0025] The negative electrode active material, the conductive agent and the binder are mixed in a mass ratio of 6:3:1

[0026] In step (3):

[0027] The separator is disposed between the positive electrode and the negative electrode, and the separator is preferably a glass fiber separator.

[0028] The electrolyte is a mixed electrolyte of water and an organic solvent containing magnesium ions, and the concentration of magnesium ions in the electrolyte is 0.01 mol L -1 ~2.0mol L -1 .

[0029] The positive and negative current collectors are selected from any one of carbon paper, metal sheets, metal foils, and foamed metals. The metal is selected from chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, or stainless steel.

[0030] The working principle of the rechargeable aqueous magnesium ion battery based on organic positive and negative electrodes of the present invention is:

[0031] During charging, magnesium ions or anions in the electrolyte are stored in the redox-active C=O reaction of the positive electrode material or stored at the active site; at the same time, magnesium ions in the electrolyte react with the redox-active C=O in the negative electrode organic material for storage. During discharge, magnesium ions or anions and magnesium ions return to the electrolyte from the positive and negative electrodes respectively. The present invention combines the different storage mechanisms of magnesium ions and anions on organic positive and negative electrodes, and the electrolyte uses a magnesium salt solution of water / organic solvent with high conductivity, reflecting the advantages of both magnesium ion batteries and aqueous batteries.

[0032] The beneficial effects of the present invention are as follows:

[0033] The present invention proposes a novel and environmentally friendly rechargeable aqueous magnesium ion battery based on organic positive and negative electrodes, wherein the positive electrode active material is an organic material containing multiple active sites or carbonyl groups; the negative electrode active material is an organic material containing carbonyl groups; the electrolyte is a mixed electrolyte of water / organic solvent containing magnesium ions, and energy is stored by storing anions or cations in the electrolyte at the positive electrode and cations at the negative electrode; at the same time, the magnesium ions described in the present invention are divalent ions, and compared with monovalent ion batteries such as lithium ion, sodium ion, and potassium ion batteries, the charge stored in magnesium ion batteries is twice that of monovalent ion batteries. Selecting good organic positive and negative electrode materials can make up for the shortcomings of magnesium ion batteries due to their slightly smaller ion radius, resulting in higher charge density and slow kinetics of magnesium ions in magnesium storage materials. It can then continue to develop into a large-scale energy storage system to meet the current demand for new energy storage systems.

[0034] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a cycle performance diagram of the rechargeable aqueous magnesium ion battery prepared in Example 1 of the present invention.

[0036] Figure 2 1 is a charge and discharge curve diagram of the rechargeable aqueous magnesium ion battery prepared in Example 2 of the present invention.

[0037] Figure 3 Graph showing the cycle performance and coulombic efficiency of the rechargeable aqueous magnesium ion battery prepared in Example 2 of the present invention.

[0038] Figure 4 This is a rate performance diagram of the rechargeable aqueous magnesium ion battery prepared in Example 2 of the present invention.

[0039] Figure 5 This is a cycle performance diagram of the rechargeable aqueous magnesium ion battery prepared in Example 3 of the present invention.

[0040] Figure 6 This is a cycle performance diagram of the rechargeable aqueous magnesium ion battery prepared in Example 4 of the present invention.

[0041] Figure 7 This is a cycle performance diagram of the rechargeable aqueous magnesium ion battery prepared in Example 5 of the present invention.

[0042] Figure 8 This is a cycle performance diagram of the rechargeable aqueous magnesium ion battery prepared in Example 6 of the present invention. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] (1) The positive electrode uses the organic material N1,N1'-(1,4-phenylene)bis(N1-(4-aminophenyl)benzene-1,4-diamine) (abbreviated as TP). The electrode is prepared by mixing TP, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on the current collector carbon paper, drying it on an infrared drying coating machine at 80°C, and cutting it into electrode sheets with a diameter of 14 mm.

[0046] (2) The negative electrode uses 1,4,5,8-naphthalenediimide (NTCDI for short). The electrode is prepared by mixing NTCDI, acetylene black, and polyvinylidene fluoride in a mass ratio of 6:3:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0047] (3) TP and NTCDI were used as positive and negative electrodes, respectively, and assembled into a button cell with a glass fiber separator. The electrolyte was 1.0 mol L -1 Mg(TFSI)2.

[0048] (4) Carry out charge and discharge test in the working voltage range of 0.01-1.6V: The cycle performance diagram of the rechargeable aqueous magnesium ion battery prepared in Example 1 is as follows Figure 1 shown.

[0049] Example 2

[0050] (1) The positive electrode uses the organic material N1,N1'-(1,4-phenylene)bis(N1-(4-aminophenyl)benzene-1,4-diamine) (abbreviated as TP). The electrode is prepared by fully mixing TP, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0051] (2) The negative electrode uses the organic material 3,4,9,10-perylenetetracarboxylic diimide (PTCDI for short). The electrode is prepared by mixing PTCDI, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0052] (3) TP and PTCDI were used as positive and negative electrodes, respectively, and assembled into a button cell with a glass fiber separator. The electrolyte was 1.0 mol L -1 Mg(TFSI)2.

[0053] (4) Carry out charge and discharge test in the working voltage range of 0.01-2.4V: The charge and discharge curve of the rechargeable aqueous magnesium ion battery prepared in Example 2 is as follows: Figure 2 As shown, the cycle performance and Coulomb efficiency are shown in Figure 3 As shown in the figure, the rate performance diagram is as follows Figure 4 shown.

[0054] Example 3

[0055] (1) The positive electrode uses the organic material N1,N1'-(1,4-phenylene)bis(N1-(4-aminophenyl)benzene-1,4-diamine) (abbreviated as TP). The electrode is prepared by fully mixing TP, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, evenly coating the slurry on the current collector carbon paper, drying it on an infrared drying coater at 80°C, and cutting it into electrode sheets with a diameter of 14 mm.

[0056] (2) The negative electrode uses 1,4,5,8-naphthalenediimide (NTCDI for short). The electrode is prepared by mixing NTCDI, acetylene black, and polyvinylidene fluoride in a mass ratio of 6:3:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0057] (3) TP and NTCDI were used as positive and negative electrodes, respectively, and assembled into a button cell with a glass fiber separator. The electrolyte was 1.0 mol L -1 Mg(ClO4)2.

[0058] (4) The charge and discharge test was carried out in the working voltage range of 0.01-2.5 V: The cycle performance of the rechargeable aqueous magnesium ion battery prepared in Example 3 is as follows: Figure 5 shown.

[0059] Example 4

[0060] (1) The positive electrode uses the organic material N1,N1'-(1,4-phenylene)bis(N1-(4-aminophenyl)benzene-1,4-diamine) (abbreviated as TP). The electrode is prepared by fully mixing TP, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0061] (2) The negative electrode uses the organic material 3,4,9,10-perylenetetracarboxylic diimide (PTCDI for short). The electrode is prepared by mixing PTCDI, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0062] (3) TP and PTCDI were used as positive and negative electrodes, respectively, and assembled into a button cell with a glass fiber separator. The electrolyte was 1.0 mol L -1 Mg(CF3SO3)2.

[0063] (4) The charge and discharge test was carried out in the working voltage range of 0.01-2.5 V: The cycle performance of the rechargeable aqueous magnesium ion battery prepared in Example 4 is as follows: Figure 6 shown.

[0064] Example 5

[0065] (1) The positive electrode uses the organic material 1,4,5,8-naphthalenetetracarboxylic anhydride (NTCDA for short). The electrode is prepared by mixing NTCDA, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0066] (2) The negative electrode uses the organic material 3,4,9,10-perylenetetracarboxylic diimide (PTCDI for short). The electrode is prepared by mixing PTCDI, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0067] (3) NTCDA and PTCDI were used as positive and negative electrodes, respectively, and assembled into a button cell with a glass fiber separator. The electrolyte was 1.0 mol L-1 dissolved in acetonitrile / water (volume ratio of 99.0:1.0). -1 Mg(TFSI)2.

[0068] (4) Charge and discharge test was performed in the working voltage range of 0.01-2.5 V: The cycle performance of the rechargeable aqueous magnesium ion battery prepared in Example 5 is as follows: Figure 7 shown.

[0069] Example 6

[0070] (1) The positive electrode uses the organic material N1,N1'-(1,4-phenylene)bis(N1-(4-aminophenyl)benzene-1,4-diamine) (abbreviated as TP). The electrode is prepared by mixing TP, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0071] (2) The negative electrode uses anthraquinone (PAQ) as an organic material. The electrode is prepared by mixing PAQ, acetylene black, and polyvinylidene fluoride in a mass ratio of 7:2:1, ball milling to obtain a slurry, uniformly coating the slurry on a carbon paper current collector, drying it on an infrared drying coating machine at 80°C, and then cutting it into electrode sheets with a diameter of 14 mm.

[0072] (3) TP and PAQ were used as positive and negative electrodes, respectively, and assembled into a button cell with a separator. The electrolyte was 1.0 mol L -1 Mg(TFSI)2.

[0073] (4) The charge and discharge test was carried out in the working voltage range of 0.01-2.5 V: The cycle performance of the rechargeable aqueous magnesium ion battery prepared in Example 6 is as follows: Figure 8 shown.

[0074] analyze:

[0075] Figure 1-Figure 8 The cycle performance of the rechargeable aqueous magnesium ion batteries prepared in Examples 1-6 is shown:

[0076] (1) By comparing Example 1 with Example 2, it can be found that under the same conditions, the discharge capacity of Example 1 is higher, indicating that NTCDI is more suitable as the negative electrode material of magnesium ion batteries.

[0077] (2) Examples 3 and 4 use different electrolytes from Examples 1 and 2. Experimental comparison shows that the electrolyte using Mg(TFSI)2 has better effect.

[0078] In summary, the rechargeable aqueous magnesium ion battery based on organic positive and negative electrodes provided by the present invention overcomes the shortcomings of the previous organic system secondary batteries such as the harsh non-aqueous environment and the narrow electrochemical stability window of pure water electrolyte, and uses a mixed electrolyte, which makes the battery assembly process safer and more convenient; the present invention uses organic materials as positive and negative electrode materials to effectively reduce costs; the working voltage range of the rechargeable aqueous magnesium ion battery based on organic positive and negative electrodes of the present invention is 0.01-2.5V, and the charge and discharge current density can reach 5A g -1 , cycle stable, and is a storage device with broad application prospects.

Claims

1. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials, characterized in that: The invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode active material is an organic material having a carbonyl group or multiple active sites; the negative electrode active material is an organic material having a carbonyl group; the electrolyte is a mixed electrolyte of water and an organic solvent containing magnesium ions, and the magnesium ion concentration in the electrolyte is 0.01 mol L -1 ~2.0mol L -1 .

2. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 1, characterized in that: The positive electrode includes a conductive agent and a binder in addition to the positive electrode active material, and the negative electrode includes a conductive agent and a binder in addition to the negative electrode active material.

3. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 2, characterized in that: The conductive agent is any one of carbon black, acetylene black and Ketjen black.

4. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 2, characterized in that: The binder is any one of polyvinylidene fluoride, polytetrafluoroethylene and sodium carboxymethyl cellulose.

5. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 1, characterized in that: The positive electrode active material is selected from any one of 1,4,5,8-naphthalenetetracarboxylic anhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, and N1,N1'-(1,4-phenylene)bis(N1-(4-aminophenyl)benzene-1,4-diamine.

6. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 1, characterized in that: The negative electrode active material is selected from any one of 3,4,9,10-perylenetetracarboxylic diimide, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,4,5,8-naphthalenediimide, 1,4,5,8-naphthalenetetracarboxylic anhydride and anthraquinone.

7. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 1, characterized in that: The magnesium salt used in the electrolyte is selected from one or more of magnesium chloride, magnesium fluoride, magnesium bromide, magnesium iodide, magnesium borohydride, magnesium perchlorate, magnesium nitrate, magnesium sulfate, magnesium chromate, magnesium acetate, magnesium hexafluoride, bis(hexamethyldisilazide)magnesium, bis(trifluoromethanesulfonyl)imide magnesium, bis(fluorosulfonyl)imide magnesium and magnesium trifluoromethanesulfonate.

8. A rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 1, characterized in that: In the electrolyte, the volume ratio of the organic solvent is 0.1 to 99.0%, and the organic solvent is selected from one or more of polyethylene glycol, polyethylene oxide, acetonitrile, ether, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dioxane, polyethylene glycol dimethyl ether, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dimethyl ether, diethyl ether, methyl formate, ethyl acetate, methyl propionate, ethyl propionate, butyl propionate, and ethyl butyrate.

9. A method for preparing a rechargeable aqueous magnesium ion battery in which both the positive and negative electrodes are made of organic materials, characterized in that: The steps include: (1) Preparation of positive electrode The positive electrode active material, the conductive agent and the binder are mixed, ball-milled to obtain a homogenous slurry, coated on the positive electrode collector, and dried to prepare a positive electrode sheet; (2) Preparation of negative electrode The negative electrode active material, the conductive agent and the binder are mixed, ball-milled to obtain a homogenous slurry, coated on the negative electrode current collector, and dried to prepare a negative electrode sheet; (3) Assembly of rechargeable aqueous magnesium ion batteries The positive electrode and negative electrode prepared above are assembled together with a separator and an electrolyte to form a rechargeable aqueous magnesium ion battery.

10. The method for preparing a rechargeable aqueous magnesium ion battery with both positive and negative electrodes made of organic materials according to claim 9, characterized in that: In step (1), the positive electrode active material, the conductive agent and the binder are mixed in a mass ratio of 7:2:1; in step (2), the negative electrode active material, the conductive agent and the binder are mixed in a mass ratio of 6:3:1; in step (3), the separator is arranged between the positive electrode and the negative electrode, the separator is a glass fiber separator, the electrolyte is a mixed electrolyte of water and an organic solvent containing magnesium ions, and the magnesium ion concentration in the electrolyte is 0.01 mol L -1 ~2.0mol L -1 .