High-conductivity solid hydrogen ion electrolyte as well as preparation method and application thereof

CN118943522APending Publication Date: 2024-11-12UNIV OF MACAU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075957.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing solid hydrogen ion electrolyte has low hydrogen ion conductivity in room temperature and anhydrous environment, which cannot meet the needs of batteries. The narrow electrochemical window of the aqueous electrolyte results in serious gas extraction problems in hydrogen ion batteries.

Method used

The metal organic frame material and metallic acid salt are used to react in situ to form a hydrogen bond network to improve the conductivity of hydrogen ions, including mixing and grinding of metallic organic frame material with acid to generate metallic acid salt loaded in metallic organic frame material to form Hydrogen bond network to achieve rapid transmission of hydrogen ions.

Benefits of technology

Achieve high conductivity (greater than 1×10-3S·cm-1) in room temperature and anhydrous environment, and exhibit excellent rate and cycling performance in all-solid-state batteries, with an electrochemical window width (approximately 3.9V ) can maintain high capacity and long cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004982252580000011
    Figure HDA0004982252580000011
  • Figure HDA0004982252580000012
    Figure HDA0004982252580000012
  • Figure HDA0004982252580000021
    Figure HDA0004982252580000021
Patent Text Reader

Abstract

The invention discloses a high-conductivity solid hydrogen ion electrolyte as well as a preparation method and application thereof. The solid hydrogen ion electrolyte comprises a metal organic framework material and metal acid salt, the metal acid salt is loaded in the metal organic framework material; the metal acid salt is obtained by carrying out in-situ reaction on metal and acid in the metal organic framework material. The solid hydrogen ion electrolyte disclosed by the invention has a relatively wide electrochemical window, the conductivity is greater than 1 * 10 <-3 > S.cm <-1 > at room temperature and in an anhydrous environment, and meanwhile, the solid hydrogen ion electrolyte shows excellent rate capability and cycle performance in an all-solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of batteries, and in particular relates to a high-conductivity solid hydrogen ion electrolyte and a preparation method and application thereof. Background Art

[0002] Hydrogen ion batteries are based on aqueous electrolytes (such as sulfuric acid, phosphoric acid, and hydrochloric acid), which have ultra-high hydrogen ion conductivity, thereby achieving rapid hydrogen transport in electrochemical conductive devices. However, these liquid electrolytes also have some problems, including leakage, potential safety issues, electrode dissolution, and corrosion. In addition, due to the narrow redox potential window of water, aqueous electrolytes limit the operating voltage and cause serious gassing problems in hydrogen ion batteries. In contrast, solid-state hydrogen ion electrolytes without leakage problems exhibit a wider voltage window and inhibit electrode dissolution and current collector corrosion.

[0003] Currently, perfluorosulfonic acid polymer hydrogen ion electrolytes have been commercially produced, but their high hydrogen ion conductivity can only be achieved under high humidity conditions. Other solid hydrogen ion electrolytes include polybenzimidazole, open framework sulfides, metal organic frameworks and covalent organic frameworks. The hydrogen ion conductivity of these materials has been significantly enhanced by the introduction of acidic guest molecules or functional groups. However, under ambient temperature and non-humid conditions, these materials show low hydrogen ion conductivity levels (<10 -3 S cm -1 ), which cannot meet the battery usage requirements. Summary of the invention

[0004] In order to overcome the problems existing in the prior art, one of the objectives of the present invention is to provide a solid hydrogen ion electrolyte.

[0005] A second object of the present invention is to provide a method for preparing a solid hydrogen ion electrolyte.

[0006] A third object of the present invention is to provide a hydrogen ion battery.

[0007] A fourth object of the present invention is to provide application of the above-mentioned solid hydrogen ion electrolyte in a battery.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] The first aspect of the present invention provides a solid hydrogen ion electrolyte, comprising a metal organic framework material and a metal acid salt; the metal acid salt is loaded in the metal organic framework material; the metal acid salt is obtained by an in-situ reaction between a metal and an acid in the metal organic framework material.

[0010] Preferably, the metal organic framework material is a material synthesized using raw materials including benzene carboxylic acid compounds.

[0011] Preferably, the benzene carboxylic acid compound is selected from at least one of pyromellitic acid, terephthalic acid and trimesic acid.

[0012] Preferably, the pKa value of the acid is less than 3.

[0013] Preferably, the metal organic framework material is selected from at least one of MIL-121, MIL-88B and MIL-100.

[0014] Preferably, the acid is selected from at least one of phosphoric acid, sulfuric acid, trifluoromethanesulfonic acid, bistrifluoromethanesulfonimide and trifluoroacetic acid.

[0015] Preferably, the particle size of the solid hydrogen ion electrolyte is 3 to 20 μm.

[0016] Preferably, the solid hydrogen ion electrolyte has a thickness of 0.9 to 2 mm.

[0017] Preferably, the metal acid salt is selected from at least one of Al(H2PO4)3, Al(CF3SO3)3, Al(N(CF3SO2)2)3, Al(CF3COO)3, Al(HSO4)3, Fe(H2PO4)3, Fe(HSO4)3, Fe(CF3SO3)3, Fe(N(CF3SO2)2)3, and Fe(CF3COO)3.

[0018] Preferably, the metal salt and the metal organic framework material form a hydrogen bond network. The metal salt and the metal organic framework material form a hydrogen bond network to achieve rapid transfer of hydrogen ions, thereby solving the problem of severe gas production in hydrogen ion batteries caused by the narrow electrochemical window of aqueous electrolytes, and solving the problem of hydrogen ion conduction level (significantly lower than 10 -3 S cm -1 ) Lower problem

[0019] The second aspect of the present invention provides a method for preparing the solid hydrogen ion electrolyte according to the first aspect of the present invention, comprising the following steps:

[0020] The metal organic framework material and the acid are mixed, ground and then pressed into tablets to obtain the product.

[0021] In the present invention, metal acid salts are generated during the mixed grinding process of the metal organic framework material and the acid. The metal acid salts are in-situ loaded in the metal organic framework material and cooperate with the metal organic framework material to form a hydrogen bond network, thereby achieving rapid transfer of hydrogen ions and improving the conductivity of the prepared solid hydrogen ion electrolyte.

[0022] Preferably, the mass ratio of the metal organic framework material to the acid is 1:(0.25-8), for example, it can be: 1:0.25, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8.

[0023] Preferably, the grinding step is ball milling at a rate of 300 to 1000 r / min.

[0024] Preferably, the grinding step is performed by manual grinding or automatic grinding equipment.

[0025] The third aspect of the present invention provides a hydrogen ion battery, comprising the solid hydrogen ion electrolyte described in the first aspect of the present invention.

[0026] The fourth aspect of the present invention provides the use of the solid hydrogen ion electrolyte described in the first aspect of the present invention in a battery.

[0027] The beneficial effects of the present invention are as follows: the solid hydrogen ion electrolyte of the present invention has a wide electrochemical window (about 3.9V), and the conductivity is greater than 1×10 -3 S cm -1 At the same time, it exhibits excellent rate performance (at a current density of 1000mA / g, it can maintain a discharge capacity of more than 15mAh / g) and cycle performance (200 cycles at a current density of 100mA / g, with a capacity retention rate of more than 96%) in all-solid-state batteries.

[0028] The preparation method of the present invention is simple to operate. Only through physical grinding, the acid and the metal organic framework material react to form a metal acid salt. The metal acid salt is in situ loaded in the metal organic framework material and synergistically forms a hydrogen bond network with the metal organic framework material to achieve rapid transfer of hydrogen ions, thereby improving the conductivity and battery performance of the prepared solid hydrogen ion electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a process flow chart for preparing the solid hydrogen ion electrolyte in Example 1.

[0030] Figure 2 This is a scanning electron microscope image of the solid hydrogen ion electrolyte in Example 1.

[0031] Figure 3 This is the X-ray diffraction pattern of the solid hydrogen ion electrolyte in Example 1.

[0032] Figure 4This is the electrochemical impedance spectrum of the solid hydrogen ion electrolyte in Example 1.

[0033] Figure 5 This is the electrochemical impedance spectrum of the solid hydrogen ion electrolyte in Comparative Example 1.

[0034] Figure 6 This is the linear sweep voltammetry curve of the solid hydrogen ion electrolyte in Example 1.

[0035] Figure 7 This is a rate performance diagram of a battery assembled using the solid hydrogen ion electrolyte in Example 1.

[0036] Figure 8 The charge and discharge cycle curve of the battery assembled using the solid hydrogen ion electrolyte in Example 1. DETAILED DESCRIPTION

[0037] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.

[0038] Example 1

[0039] Reference Figure 1 The preparation process flow chart in this example provides a method for preparing a solid hydrogen ion electrolyte with high electrical conductivity, and the preparation steps include:

[0040] 1) Weigh 100 mg of MIL-121 metal organic framework and 50 mg of phosphoric acid into a ball mill, and mix them thoroughly at a speed of 500 r / min for 60 min to obtain the electrolyte material MIL-121-H3PO4;

[0041] 2) Weigh 100 mg of MIL-121-H3PO4 powder and put it into a tableting mold, and press it to obtain a solid hydrogen ion electrolyte sheet with a diameter of 10 mm and a thickness of 1 mm.

[0042] The solid hydrogen ion electrolyte in this example is ball-milled with MIL-121 solid and phosphoric acid solid. During the ball-milling process, a chemical reaction occurs between the MIL-121 solid and the phosphoric acid solid to generate Al(H2PO4)3. When the solid hydrogen ion electrolyte in this example is assembled into a battery, both MIL-121 and Al(H2PO4)3 participate in the transmission of hydrogen ions, and therefore has higher electrical conductivity and better battery performance.

[0043] Example 2

[0044] The preparation method of the high-conductivity solid hydrogen ion electrolyte in this example is different from that in Example 1 only in that the acid in step 1) of this example is 100 mg of phosphoric acid, specifically as follows:

[0045] The method for preparing the high conductivity solid hydrogen ion electrolyte in this example comprises the following steps:

[0046] 1) Weigh 100 mg of MIL-121 and 100 mg of phosphoric acid into a ball mill, and mix them thoroughly at a speed of 500 r / min for 60 min to obtain the electrolyte material MIL-121-H3PO4;

[0047] 2) Weigh 100 mg of MIL-121-H3PO4 powder and put it into a tableting mold, and press it to obtain a solid hydrogen ion electrolyte sheet with a diameter of 10 mm and a thickness of 1 mm.

[0048] Example 3

[0049] The preparation method of the high-conductivity solid hydrogen ion electrolyte in this example is different from that in Example 1 only in that the acid in step 1) of this example is 50 mg of sulfuric acid, as follows:

[0050] The method for preparing the high conductivity solid hydrogen ion electrolyte in this example comprises the following steps:

[0051] 1) Weigh 100 mg of MIL-121 and 50 mg of sulfuric acid into a ball mill, mix them thoroughly at a speed of 500 r / min for 60 min to obtain the electrolyte material MIL-121-H2SO4;

[0052] 2) Weigh 100 mg of MIL-121-H2SO4 powder and put it into a tableting mold, and press it to obtain a solid hydrogen ion electrolyte sheet with a diameter of 10 mm and a thickness of 1 mm.

[0053] The solid hydrogen ion electrolyte in this example is ball-milled with MIL-121 solid and sulfuric acid. During the ball-milling process, a chemical reaction occurs between the MIL-121 solid and the sulfuric acid to generate Al(HSO4)3. When the solid hydrogen ion electrolyte in this example is assembled into a battery, both MIL-121 and Al(HSO4)3 participate in the transmission of hydrogen ions, and therefore has higher electrical conductivity and better battery performance.

[0054] Example 4

[0055] The preparation method of the high-conductivity solid hydrogen ion electrolyte in this example is different from that in Example 1 only in that the MOF used in step 1) is MIL-101, as follows:

[0056] The method for preparing the high conductivity solid hydrogen ion electrolyte in this example comprises the following steps:

[0057] 1) Weigh 100 mg of MIL-101 and 50 mg of phosphoric acid into a ball mill and mix them thoroughly at a speed of 500 r / min for 60 min to obtain the electrolyte material MIL-101-H3PO4;

[0058] 2) Weigh 100 mg of MIL-101-H3PO4 powder and put it into a tableting mold, and press it to obtain a solid hydrogen ion electrolyte sheet with a diameter of 10 mm and a thickness of 1 mm.

[0059] Example 5

[0060] The preparation method of the high-conductivity solid hydrogen ion electrolyte in this example is different from that in Example 1 only in that the mixing is carried out by grinding in step 1), as follows:

[0061] The method for preparing the high conductivity solid hydrogen ion electrolyte in this example comprises the following steps:

[0062] 1) Weigh 100 mg of MIL-121 and 50 mg of phosphoric acid into a mortar and grind for 20 min to obtain the electrolyte material MIL-121-H3PO4;

[0063] 2) Weigh 100 mg of MIL-121-H3PO4 powder and put it into a tableting mold, and press it to obtain a solid hydrogen ion electrolyte sheet with a diameter of 10 mm and a thickness of 1 mm.

[0064] Example 6

[0065] The preparation method of the high-conductivity solid hydrogen ion electrolyte in this example is different from that in Example 1 only in that: 200 mg of MIL-121-H3PO4 is weighed in step 2), as follows:

[0066] The method for preparing the high conductivity solid hydrogen ion electrolyte in this example comprises the following steps:

[0067] 1) Weigh 100 mg of MIL-121 and 50 mg of phosphoric acid into a mortar and grind for 20 min to obtain the electrolyte material MIL-121-H3PO4;

[0068] 2) Weigh 200 mg of MIL-121-H3PO4 powder and put it into a tableting mold, and press it to obtain a solid hydrogen ion electrolyte sheet with a diameter of 10 mm and a thickness of 2 mm.

[0069] Comparative Example 1

[0070] This example provides a method for preparing a solid hydrogen ion electrolyte, and the preparation steps include:

[0071] 100 mg of MIL-121 powder was weighed and put into a tablet pressing mold, and pressed to obtain a MIL-121 sheet with a diameter of 10 mm and a thickness of 1 mm, which is the solid hydrogen ion electrolyte in this example.

[0072] Performance Testing:

[0073] The surface morphology of the electrolyte material MIL-121-H3PO4 in Example 1 was tested by scanning electron microscopy. Figure 2 As shown by Figure 2 It can be seen that the particle size of the electrolyte material MIL-121-H3PO4 is 3 to 20 μm. Then, the X-ray diffraction pattern (XRD) of the electrolyte material MIL-121-H3PO4 in Example 1 was tested using an X-ray diffractometer. Figure 3 As shown in the figure, it can be seen from the XRD pattern that MIL-121 reacts with phosphoric acid and generates a new product, Al(H2PO4)3.

[0074] A button-type symmetrical cell was prepared using a stainless steel sheet as an electrode and the solid hydrogen ion electrolyte in Example 1 as an electrolyte to measure the electrochemical impedance spectrum of the electrolyte. The electrochemical impedance spectrum is shown in FIG. Figure 4 As shown by Figure 4 It can be seen that the conductivity of the solid hydrogen ion electrolyte in Example 1 at room temperature is 1.94×10 -3 S cm -1 , which is greater than 1.0×10 -3 S cm -1 .

[0075] A button-type symmetrical cell was prepared using a stainless steel sheet as an electrode and the solid hydrogen ion electrolyte in Comparative Example 1 as an electrolyte to measure the electrochemical impedance spectrum of the electrolyte. The electrochemical impedance spectrum of the MIL-121 sheet is shown in FIG. Figure 5 As shown. Figure 5 It can be seen that the conductivity of the solid hydrogen ion electrolyte in Comparative Example 1 is only 5.6×10 -9 S cm -1 , while the conductivity of pure Al(H2PO4)3 at 100-200℃ is 10 -6 ~10 -7 S cm -1 Therefore, pure MIL-121 flakes and Al(H2PO4)3 do not have good conductivity in anhydrous environment at room temperature. The solid hydrogen ion electrolyte in the present invention has excellent conductivity at room temperature, which is attributed to the formation of a stable hydrogen bond network between the MOF material and the product Al(H2PO4)3, so that the solid hydrogen ion electrolyte in the present invention can quickly transfer protons between electrodes.

[0076] A button cell was prepared with the titanium sheet as the working electrode, the foil as the counter electrode and the reference electrode, and the solid hydrogen ion electrolyte in Example 1 as the electrolyte, and was used to measure the electrochemical window of the electrolyte. The measured linear sweep voltammetric curve is as follows: Figure 6 As shown. Figure 6 It can be seen that the electrochemical window of the solid hydrogen ion electrolyte in Example 1 is about 3.9 V, which has a wider electrochemical window, and is conducive to obtaining better battery performance.

[0077] Molybdenum trioxide (MoO3) was used as the negative electrode, and protonated Prussian blue analog (H-TBA, i.e. H x Cu[Fe(CN)6] 2 / 3 ·4H2O, synthesis method see AHigh-Rate Aqueous Proton Battery Delivering Power Below-78℃ via an Unfrozen Phosphoric Acid, H. Jiang, W. Shin, J. J. Hong, Dr. Z. Wei, Y. Liu, Dr. X. Wu, Y. Xu, Q. Guo, Prof. MA Subramanian, Prof. X. Ji, Adv. Energy Mater. 2020, 2000968) as the positive electrode, the solid hydrogen ion electrolyte in Example 1 as the electrolyte, prepared into a button battery for testing the rate performance and cycle performance of the electrolyte, the rate performance test results are shown in Figure 7 The cycle performance test results are shown in Figure 8 As shown. Figure 7 It can be seen that the button cell containing the solid hydrogen ion electrolyte in Example 1 can maintain a discharge capacity of 48 mAh / g, 42 mAh / g, 28 mAh / g and 19 mAh / g at current densities of 50 mA / g, 100 mA / g, 500 mA / g and 1000 mA / g, respectively. Figure 8 It can be seen that the button battery containing the solid hydrogen ion electrolyte in Example 1 has a capacity retention rate of more than 96% after 200 cycles at a current density of 100 mAh / g, and still maintains a charge-discharge specific capacity of 25 mAh / g after 800 cycles, and has excellent electrochemical performance.

[0078] In summary, the preparation method of the solid hydrogen ion electrolyte in the present invention has the characteristics of simple operation and low cost. After mechanical mixing of MOF and acid, MOF and the newly generated product synergistically form a hydrogen bond network, which promotes the high-speed transmission of hydrogen ions and realizes high hydrogen ion conduction at room temperature and in anhydrous environment. Specifically, it has a wide electrochemical window (~3.9V) and a conductivity of 1.94×10 -3 S cm-1 At the same time, it exhibits excellent rate performance (at a current density of 1000mA / g, it can maintain a discharge capacity of more than 15mAh / g) and cycle performance (200 cycles at a current density of 100mA / g, with a capacity retention rate of more than 96%) in all-solid-state batteries.

[0079] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A solid hydrogen ion electrolyte, characterized in that: The invention comprises a metal organic framework material and a metal acid salt; the metal acid salt is loaded in the metal organic framework material; the metal acid salt is obtained by in-situ reaction of the metal in the metal organic framework material and the acid.

2. The solid hydrogen ion electrolyte according to claim 1, characterized in that: The metal organic framework material is a material synthesized using raw materials including benzene carboxylic acid compounds; And / or, the pKa value of the acid is less than 3.

3. The solid hydrogen ion electrolyte according to claim 1, characterized in that: The metal organic framework material is selected from at least one of MIL-121, MIL-88B, and MIL-100; And / or, the acid is selected from at least one of phosphoric acid, sulfuric acid, trifluoromethanesulfonic acid, bistrifluoromethanesulfonimide, and trifluoroacetic acid.

4. The solid hydrogen ion electrolyte according to claim 1, characterized in that: The particle size of the solid hydrogen ion electrolyte is 3 to 20 μm.

5. The solid hydrogen ion electrolyte according to claim 1, characterized in that: The metal acid salt is selected from at least one of Al(H2PO4)3, Al(CF3SO3)3, Al(N(CF3SO2)2)3, Al(CF3COO)3, Al(HSO4)3, Fe(H2PO4)3, Fe(HSO4)3, Fe(CF3SO3)3, Fe(N(CF3SO2)2)3, and Fe(CF3COO)3.

6. The solid hydrogen ion electrolyte according to any one of claims 1 to 5, characterized in that: The metal salt and the metal organic framework material form a hydrogen bonding network.

7. The method for preparing the solid hydrogen ion electrolyte according to any one of claims 1 to 6, characterized in that: The following steps are involved: The metal organic framework material and the acid are mixed, ground and then pressed into tablets to obtain the product.

8. The method for preparing a solid hydrogen ion electrolyte according to claim 7, characterized in that: The grinding step is ball milling at a speed of 300 to 1000 r / min.

9. A hydrogen ion battery, characterized in that: The invention comprises the solid hydrogen ion electrolyte according to any one of claims 1 to 6.

10. Use of the solid hydrogen ion electrolyte according to any one of claims 1 to 6 in a battery.