Simulation type memristor based on high-entropy oxide and metal oxide lamination and preparation method and application thereof

By using a stacked structure of high-entropy oxide and metal oxide in the resistive change memory, the oxygen vacancies conductive channel is controlled, and the problem of sudden change in resistance performance in the prior art is solved, and high-performance simulated resistance characteristics and low-power are achieved Consumable, suitable for neural network computing and in-memory computing.

CN118946246APending Publication Date: 2024-11-12SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410992292.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing binary and ternary oxide-based resistive change memory exhibits mutation characteristics in resistive change performance, which limits its application in fields such as neural network computing, especially analog memristor devices that achieve stable slow-change performance have not yet been available. Report.

Method used

Using a simulated memristor preparation method based on high entropy oxide and metal oxide stacking, a conductive film is deposited on an insulating substrate and a physical vapor deposition method is used to deposit metal oxide and high entropy oxide layer to form a stacking layer The structure acts as a resistive layer to regulate the formation and breakage of conductive channels of oxygen vacancy, and achieves simulated resistive characteristics.

Benefits of technology

It realizes high-performance analog resistance change characteristics, has high conductivity regulation linearity, good stability and low power consumption. It is suitable for in-memory computing and brain-like neuromorphic computing, significantly reducing system energy consumption, improving computing efficiency and Storage efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946246A_ABST
    Figure CN118946246A_ABST
Patent Text Reader

Abstract

The invention discloses an analog memristor based on high-entropy oxide and metal oxide lamination and a preparation method and application of the analog memristor, and belongs to the technical field of nonvolatile resistive random access memories and neural network computation.A conductive film is deposited on an insulating substrate to serve as a lower electrode; a physical vapor deposition mode is adopted, a metal oxide layer is deposited on the lower electrode firstly, then a high-entropy oxide layer is deposited, and an obtained laminated layer serves as a resistive layer; and continuously depositing a conductive film as an upper electrode to obtain the analog memristor based on the high-entropy oxide and metal oxide lamination. The preparation process is simple, compatible with the CMOS process, low in energy consumption, environment-friendly and excellent in performance, migration of oxygen vacancies under electric excitation regulation has continuity, so that formation and fracture of a constructed conductive channel have gradual change, the resistance change simulation characteristic is further achieved, the resistance change simulation performance of high electrical conductivity, wide regulation and control range and good symmetry is achieved, and the application prospect is wide. The method has application prospects in the fields of information storage and neural network calculation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of non-volatile resistive random access memory and neural network computing, and specifically relates to an analog memristor based on a high entropy oxide and a metal oxide stack, and a preparation method and application thereof. Background Art

[0002] In recent years, high entropy oxide materials, which are composed of five or more multi-metal oxides mixed in nearly equal molar ratios, have attracted the attention of researchers due to their unique structural characteristics and excellent material properties (such as high ionic conductivity, excellent long-term cycle stability, and huge dielectric constant). At present, high entropy oxides mainly show their advantages in the fields of catalysis and energy storage. However, due to their high stability, huge dielectric constant and adjustable composition, they can theoretically realize high-performance resistive memory as resistive memory materials. The current mainstream resistive memory is based on binary oxide and ternary oxide resistive layers, and there is little research on five-element and above high entropy oxide-based resistive memristors.

[0003] Memristors can be divided into digital and analog resistive switching devices according to the change of their conductance with applied excitation voltage. Analog memristors, inspired by the structure of human brain synapses, have the characteristics of simple structure, low power consumption, and continuously adjustable high and low resistance states. They are an important basis for realizing in-memory computing and brain-like neuromorphic computing. However, at present, resistive switching memristors with two-terminal structures usually show the characteristics of digital memristors with sudden changes in high and low resistance states. Therefore, it is of great significance to select a suitable resistive switching layer to construct an analog memristor with stable and slow-changing characteristics.

[0004] The current mainstream binary and ternary oxide-based resistive memory exhibits abrupt changes in resistive switching performance, which limits its application in fields such as neural network computing that require continuously adjustable resistance states. There are few constructions based on high-entropy oxide memristors, especially the realization of analog memristor devices with stable slow-changing performance has not yet been reported. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an analog memristor based on a high entropy oxide and a metal oxide stack, and a preparation method and application thereof, so as to solve the technical problem that the existing binary and ternary oxide-based resistive memory has a sudden change in resistive performance, which limits its application in fields such as neural network computing.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention discloses a method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides, comprising the following steps:

[0008] 1) Depositing a conductive film on an insulating substrate as the lower electrode of an analog memristor;

[0009] 2) on the lower electrode prepared in step 1), a metal oxide layer is first deposited by physical vapor deposition, and then a high entropy oxide layer is deposited, and the obtained stacked layer is used as a resistive switching layer of the analog memristor;

[0010] 3) On the stack grown in step 2), a conductive film is further deposited as the upper electrode of the analog memristor; thus, an analog memristor based on a stack of high entropy oxide and metal oxide is obtained.

[0011] Preferably, in step 1), the insulating substrate is highly flat transparent glass, a polyethylene terephthalate substrate or polished silicon oxide / silicon.

[0012] Preferably, in step 1), the lower electrode is a metal with high stability, such as gold, platinum, tungsten, fluorine-doped tin dioxide or indium tin oxide; the thickness of the lower electrode is 50-200 nm;

[0013] In step 3), the upper electrode is a metal with high stability, such as gold, platinum, tungsten, fluorine-doped tin dioxide or indium tin oxide; the thickness of the upper electrode is 50-200nm.

[0014] Preferably, in step 2), the physical vapor deposition method is magnetron sputtering or pulsed laser; the metal oxide layer is titanium oxide, tungsten oxide, hafnium oxide, tantalum oxide, manganese oxide, yttrium oxide, niobium oxide or vanadium oxide; the high entropy oxide layer is a five-element metal oxide prepared by mixing five metals of iron, cobalt, nickel, cadmium and manganese in an equiatomic ratio; and the deposition method of the high entropy oxide layer is radio frequency magnetron sputtering.

[0015] Preferably, in step 2), the thickness of the metal oxide layer is 10-100 nm; the thickness of the high entropy oxide layer is 5-50 nm.

[0016] Preferably, in step 2), the heating temperature of the metal oxide layer is 30-300°C; the working gas pressure is 0.1-5Pa; argon and oxygen are introduced simultaneously during the deposition process, the argon flow rate is 5-25sccm, and the oxygen flow rate is 5-30sccm; the film growth time is 3-30min; and the sputtering power is 50-350W.

[0017] Preferably, in step 2), the heating temperature of the high entropy oxide is 100-400°C; the working gas pressure is 1-10Pa; argon and oxygen are introduced simultaneously during the deposition process, the argon flow rate is 2-20sccm, and the oxygen flow rate is 10-60sccm; the growth time of the film is 0.5-5min; and the sputtering power is 20-200W.

[0018] The present invention also discloses an analog memristor based on a high entropy oxide and a metal oxide stack obtained by the above preparation method, which comprises, from bottom to top, an insulating substrate, a lower conductive electrode, a metal oxide, a high entropy oxide and an upper conductive electrode.

[0019] The present invention also discloses the application of the analog memristor based on high entropy oxide and metal oxide stack prepared by the above preparation method in information storage.

[0020] The present invention also discloses the application of the analog memristor based on high entropy oxide and metal oxide stack prepared by the above preparation method in neural network calculation.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention discloses a method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide, which has the advantages of simple preparation process, compatibility with CMOS process, low energy consumption, environmental protection and excellent performance. High entropy oxide has the advantages of high stability, huge dielectric constant and adjustable composition. As a resistive memory material, it can realize high-performance resistive memory. However, the current mainstream resistive memory uses binary oxide and ternary oxide as the resistive layer, and most of the constructed devices show resistive performance with mutation characteristics, which restricts the application in the fields of neural network calculation. The present invention adopts an alloy target material composed of five or more multi-metals mixed in a nearly equal molar ratio, uses radio frequency magnetron sputtering to deposit high entropy oxide as the core resistive layer, and superimposes an oxide layer to regulate the stability of the device. Under the condition of electrical excitation, the migration of oxygen vacancies is continuous, so the formation and fracture of the constructed conductive channel are gradual, thereby realizing the analog resistive property, which is of great significance for realizing the application in the fields of in-memory computing and brain-like neuromorphic computing.

[0023] Furthermore, a highly flat insulating substrate is selected. High flatness is a prerequisite for obtaining a high-stability analog memristor, and the insulating property can reduce the influence of the substrate's conductivity on the device current; transparent glass helps to realize the construction of transparent devices and helps to realize light-controlled coupled analog resistive performance; polyethylene terephthalate substrate is a flexible substrate, which helps to build flexible devices and realize applications in the wearable field; polished silicon oxide / silicon substrate helps to achieve compatibility with CMOS technology and realize mass production.

[0024] Furthermore, the selection of metals with high stability such as gold, platinum, and tungsten for the lower and upper electrodes helps prevent electrode atoms from entering the resistive switching layer and affecting the resistive switching performance of the device. Moreover, the stable metal can prevent the reaction with water molecules and oxygen in the air, thereby obtaining a higher contact between the electrodes. Fluorine-doped tin dioxide and indium tin oxide electrodes combined with transparent substrates can construct transparent devices, and use light-controlled coupling to regulate the analog resistive switching characteristics. The use of metals with high stability such as gold, platinum, and tungsten, or fluorine-doped tin dioxide and indium tin oxide metal oxides as the upper and lower electrodes of the analog memristor provides a guarantee for the realization of high-stability analog resistive switching devices and transparent resistive switching devices. The physical vapor deposition method is used to grow high entropy oxide and metal oxide layers respectively. The grown stacked layers are used as the resistive switching layer of the device, which can effectively regulate the slow formation and breakage of the conductive channel of the oxygen vacancy structure, and is the core of realizing the analog resistive switching performance.

[0025] Furthermore, the thickness of the lower electrode and the upper electrode is 50-200 nm. If the thickness is lower than this, the reliability of the manufactured device deteriorates. If the thickness is higher than this, it has little effect on improving the performance of the device and wastes energy.

[0026] Furthermore, physical vapor deposition methods such as magnetron sputtering or pulsed laser are selected to deposit oxide and high entropy oxide layers. The magnetron sputtering preparation method has the advantages of simple preparation process, high reliability and repeatability, low cost, and the ability to effectively control the oxygen vacancy concentration in the film, thereby achieving the regulation of the analog resistive switching performance of the device; the pulsed laser method has the advantages of low cost and fast growth rate, and the resistive switching performance of the device can also be regulated by controlling conditions such as the concentration of the growth atmosphere.

[0027] Furthermore, the metal oxide layer is one of titanium oxide, tungsten oxide, hafnium oxide, tantalum oxide, manganese oxide, yttrium oxide, niobium oxide and vanadium oxide. The memristor constructed with the above metal oxide as the single resistive switching layer exhibits excellent resistive switching performance and is a good memristor storage material.

[0028] Furthermore, the high entropy oxide layer is a five-element metal oxide prepared by mixing five metals of iron, cobalt, nickel, cadmium and manganese in an equiatomic ratio; a high entropy oxide layer is formed by mixing five metal elements (iron, cobalt, nickel, cadmium, and manganese) in an equiatomic ratio. This diversified design not only increases the complexity of the material, but also may bring unique physical and chemical properties, such as high hardness, high strength, and high corrosion resistance. Due to the uniform mixing of multiple elements, the phase separation or segregation phenomenon that may be caused by a single element is reduced, thereby improving the overall stability and reliability of the material. The deposition method of the high entropy oxide layer is radio frequency magnetron sputtering, which can accurately control the thickness, composition, and uniformity of the film, thereby ensuring that the high entropy oxide layer has excellent performance. With a high deposition rate and yield, a large-area, uniform high entropy oxide layer can be prepared in a short time. This helps to improve production efficiency and reduce manufacturing costs.

[0029] Furthermore, the thickness of the metal oxide layer in the resistive layer of the constructed analog memristor is 10-100nm, and the high entropy oxide is 5-50nm. For memristors with a thickness below this, the voltage resistance is not high due to the thinner resistive layer, the device is easily broken down, and the stability of the device is reduced; for resistive layers with a thickness above this range, a larger transition voltage is required to perform resistive switching control, and the power consumption of the device increases.

[0030] Furthermore, the heating temperature of the metal oxide layer is 30-300°C, and the heating temperature of the high entropy oxide is 100-400°C. The surface roughness of the film prepared below this temperature range is high, and the performance and stability of the constructed device are poor. The oxygen vacancies of the film prepared above this temperature range are difficult to control, and the simulated resistive switching performance of the device is poor; the working gas pressure of the metal oxide layer is 0.1-5Pa, and the working gas pressure of the high entropy oxide is 1-10Pa. The growth rate of the film prepared below this pressure range is too slow, and the manufacturing cost of the device is increased. The quality of the film above this pressure range is poor, resulting in poor performance and stability of the device; during the growth of the metal oxide layer, the flow rates of argon and oxygen are 5-25sccm and 5-30sccm, and during the growth of the high entropy oxide, the flow rates of argon and oxygen are 2-20sccm and 10-60sccm. In this pressure range, the film growth rate is too slow, which increases the device preparation cost. The film prepared above this pressure range is poor, which reduces the performance of the device. The growth time of the metal oxide layer film is 3-30min, and the growth time of the high entropy oxide film is 0.5-5min. Too long deposition time leads to a large film thickness, requiring a higher excitation voltage to achieve resistive switching performance, resulting in increased power consumption of the device. The thickness of the resistive layer prepared with too low growth time is low. Although the constructed analog memristor has low power consumption, it is easily broken down, resulting in poor stability of the device. The sputtering power of metal oxide is 50-350W, and the sputtering power of high entropy oxide is 20-200W. The resistive layer prepared below this power range requires a longer time to complete the device construction, which is inefficient. The roughness of the film grown above this power range increases, and the simulated resistive switching performance of the constructed device deteriorates.

[0031] The present invention also discloses an analog memristor based on a high entropy oxide and a metal oxide stack obtained by the above-mentioned preparation method. By introducing a high-entropy oxide with high stability, a huge dielectric constant and adjustable composition, the high entropy oxide is used as the core resistive switching layer of the resistive switching device, and a single metal oxide is superimposed to construct a double-layer structure, so as to construct an analog memristor with high stability, realize an analog resistive switching characteristic with high and stable linearity of conductivity regulation, provide hardware support for the application in the field of in-memory computing and brain-like neuromorphic computing, and have great application prospects in non-volatile resistive memory, especially in the field of neural network computing.

[0032] The present invention also discloses the application of the analog memristor based on high entropy oxide and metal oxide stack prepared by the above preparation method in information storage. By adopting the method of physical vapor deposition, high entropy oxide and metal oxide layers are grown, and the grown stack is used as the resistive switching layer of the device, which can effectively regulate the slow formation and fracture of the conductive channel constructed by oxygen vacancies. Compared with binary oxide and ternary oxide based memristors, it has a resistive switching performance with mutation characteristics, a higher storage window, better cycle durability and longer data retention time. It has the characteristics of low power consumption and non-volatility, and is suitable for the development of the next generation of non-volatile memory, improving storage efficiency and reducing energy consumption. The design of the stacked structure helps to achieve a higher density storage array to meet the demand for storage capacity in the era of big data and cloud computing.

[0033] The present invention also discloses the application of the analog memristor based on high entropy oxide and metal oxide stacks prepared by the above-mentioned preparation method in neural network computing. The continuously adjustable resistance state characteristics of the high entropy oxide and metal oxide stack analog memristor enable it to simulate the plasticity of biological synapses, providing an ideal basic element for building brain-like neuromorphic computing systems. In a pulse neural network, the memristor can adjust weights in real time, accelerate the training process of the neural network, and improve computing efficiency and accuracy. Combined with its low power consumption characteristics, the memristor can significantly reduce system energy consumption and improve overall performance in neural network computing, and is suitable for resource-constrained scenarios such as edge computing and mobile devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A schematic diagram of the structure of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Embodiment 1 of the present invention;

[0035] Figure 2 A logarithmic current-voltage curve diagram of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Embodiment 1 of the present invention;

[0036] Figure 3 A retention characteristic curve diagram of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Embodiment 1 of the present invention;

[0037] Figure 4 Cyclic characteristic diagram of an analog memristor based on a high entropy oxide and metal oxide stack constructed in Embodiment 1 of the present invention;

[0038] Figure 5 A graph showing the change in current of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Embodiment 1 of the present invention under continuous same forward electrical excitation;

[0039] Figure 6A graph showing the change in current of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Embodiment 1 of the present invention under continuous negative electrical excitation;

[0040] Figure 7 LTD and LTP curves of an analog memristor based on a high entropy oxide and metal oxide stack constructed in embodiment 1 of the present invention. DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0042] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0043] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0044] The present invention discloses a method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides, comprising the following steps:

[0045] 1) Depositing a conductive film of a certain thickness on an insulating substrate as the lower electrode of the analog memristor;

[0046] 2) depositing a metal oxide layer of a specific thickness on the lower electrode obtained in step 1) by physical vapor deposition; then continuing to deposit a high entropy oxide layer of a specific thickness, and the obtained stacked layer serves as a resistive switching layer of an analog memristor;

[0047] 3) On the stack grown in step 2), a conductive film of a certain thickness is continuously deposited as the upper electrode of the analog memristor; thus, an analog memristor based on a stack of high entropy oxide and metal oxide is obtained.

[0048] Wherein, in step 1), the highly flat insulating substrate is selected from transparent glass, polyethylene terephthalate substrate or polished silicon oxide / silicon.

[0049] The lower electrode is made of metal with high stability such as gold, platinum, tungsten, fluorine-doped tin dioxide or indium tin oxide.

[0050] The thickness of the lower electrode is 50-200nm.

[0051] In step 2), the physical vapor deposition method is magnetron sputtering or pulsed laser deposition.

[0052] The thickness of the metal oxide layer is 10-100 nm, and the thickness of the high entropy oxide layer is 5-50 nm.

[0053] The metal oxide layer is titanium oxide, tungsten oxide, hafnium oxide, tantalum oxide, manganese oxide, yttrium oxide, niobium oxide or vanadium oxide.

[0054] The high entropy oxide layer is an oxide of five elements (iron, cobalt, nickel, cadmium and manganese) in equal atomic proportions, that is, a five-element metal oxide prepared by mixing the five metals iron, cobalt, nickel, cadmium and manganese in equal atomic proportions; the deposition method of the high entropy oxide layer is radio frequency magnetron sputtering.

[0055] The heating temperature of the metal oxide layer is 30-300°C, the working gas pressure is 0.1-5Pa, argon and oxygen are introduced simultaneously during the deposition process, the flow rates of argon and oxygen are 5-25sccm and 5-30sccm, the film growth time is 3-30min, and the sputtering power is 50-350W.

[0056] The heating temperature of the high entropy oxide is 100-400°C, the working gas pressure is 1-10Pa, argon and oxygen are introduced simultaneously during the deposition process, the flow rates of argon and oxygen are 2-20sccm and 10-60sccm, the film growth time is 0.5-5min, and the sputtering power is 20-200W.

[0057] In step 3), the upper electrode is a metal with high stability such as gold, platinum, tungsten, fluorine-doped tin dioxide or indium tin oxide. The thickness of the upper electrode is 50-200 nm.

[0058] The present invention also discloses an analog memristor based on a high entropy oxide and a metal oxide stack obtained by the above-mentioned preparation method. From bottom to top, it is an insulating substrate, a lower electrode, a metal oxide, a high entropy oxide, and an upper electrode, which belongs to the field of non-volatile resistive memory and neural network computing. The preparation method of the present invention has a sudden resistive switching characteristic compared to the memristor device constructed by binary oxides and ternary oxides. The device of the present invention realizes excellent analog resistive switching characteristics and has great application prospects in the fields of information storage and neural network computing.

[0059] The present invention also discloses that the analog memristor based on high entropy oxide and metal oxide stack prepared by the above preparation method has great applications in the fields of information storage, non-volatile resistive random access memory and neural network calculation.

[0060] At present, there are few constructions based on high entropy oxide memristors, especially there are no reports on realizing analog resistive switching devices with stable slow-switching performance. In view of this, the present invention realizes analog resistive switching performance by constructing a device of high entropy oxide and metal oxide stacks.

[0061] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0062] S1, depositing a conductive film of a certain thickness on an insulating substrate as the lower electrode of the analog memristor;

[0063] Preferably, the highly flat insulating substrate is polished silicon oxide / silicon.

[0064] Preferably, the lower electrode is metal platinum with high stability.

[0065] Preferably, the thickness of the lower conductive electrode is 100 nm.

[0066] S2. On the lower electrode, a metal oxide layer of a specific thickness is deposited by physical vapor deposition, and then a high entropy oxide layer of a specific thickness is deposited, and the obtained stacked layer is used as a resistive switching layer of an analog memristor;

[0067] Preferably, the physical vapor deposition method is magnetron sputtering.

[0068] Preferably, the metal oxide layer is titanium oxide.

[0069] Preferably, the thickness of the metal oxide layer is 50 nm.

[0070] Preferably, the high entropy oxide is an oxide of five elements (iron, cobalt, nickel, cadmium and manganese) in equal atomic proportions.

[0071] Preferably, the high entropy oxide is 20 nm.

[0072] Preferably, the heating temperature of titanium oxide is 250° C., the working gas pressure is 0.5 Pa, the flow rates of argon and oxygen are 15 sccm and 10 sccm, the deposition time is 20 min, and the sputtering power is 150W.

[0073] Preferably, the heating temperature of the high entropy oxide is 250° C., the working gas pressure is 2 Pa, the flow rates of argon and oxygen are 5 sccm and 30 sccm, the deposition time is 1 min, and the sputtering power is 70W.

[0074] S3. On top of the grown stack, a conductive film of a certain thickness is continuously deposited as the upper electrode of the device; thus, an analog memristor based on a stack of high entropy oxides and metal oxides is obtained.

[0075] Preferably, the upper electrode is metal platinum with high stability.

[0076] Preferably, the thickness of the upper conductive electrode is 100 nm.

[0077] Example 1

[0078] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0079] S1, depositing a 100 nm thick platinum conductive film on a polished silicon oxide / silicon insulating substrate as the lower electrode of the analog memristor;

[0080] S2. On the lower electrode, a 50nm thick titanium oxide layer is deposited by magnetron sputtering physical vapor deposition. The heating temperature of the titanium oxide is 250°C, the working pressure is 0.5Pa, the argon and oxygen flow rates are 15sccm and 10sccm, the deposition time is 20min, and the sputtering power is 150W. Then continue to deposit a high-entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions in a specific thickness of 20nm. The heating temperature of the high-entropy oxide layer is 250°C, the working pressure is 2Pa, the argon and oxygen flow rates are 5sccm and 30sccm, the deposition time is 1min, and the sputtering power is 70W. The obtained stack is used as the resistive switching layer of the analog memristor;

[0081] S3, on the grown stack, continue to deposit a 100 nm thick platinum conductive film as the upper electrode of the device, and obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0082] See also Figure 1 , which is a structural schematic diagram of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Example 1 of the present invention. The constructed analog memristor comprises an insulating substrate, a lower conductive electrode, a metal oxide, a high entropy oxide and an upper conductive electrode from bottom to top.

[0083] See also Figure 2 , which is a logarithmic current-voltage curve of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Example 1 of the present invention. From the figure, it can be seen that the memristor has excellent slow-change resistive characteristics during the startup process under positive electrical excitation and the recovery process under negative voltage excitation.

[0084] See also Figure 3, which is a retention characteristic curve of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Example 1 of the present invention. It can be seen from the figure that during the retention characteristic test process lasting up to 10,000 seconds, both the high resistance state and the low resistance state show good stability.

[0085] See also Figure 4 , which is a cycle characteristic curve of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Example 1 of the present invention. It can be seen from the figure that it maintains relatively good stability during a cycle process of up to 300 times.

[0086] See also Figure 5 , which is a current variation curve of an analog memristor based on a high entropy oxide and metal oxide stack constructed in Example 1 of the present invention under continuous same positive electrical excitation. It can be seen from the figure that the current shows a trend of gradually increasing, indicating that the conductivity of the device has a cumulative effect.

[0087] See also Figure 6 , is a current variation curve of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Example 1 of the present invention under continuous negative electrical excitation. It can be seen from the figure that the current shows a gradually decreasing trend.

[0088] See also Figure 7 , which are LTD and LTP curves of an analog memristor based on a high entropy oxide and a metal oxide stack constructed in Example 1 of the present invention. It can be seen that LTD and LTP basically present a linear relationship and have good symmetry, indicating that the constructed analog memristor has good application prospects in the field of neural network computing.

[0089] Example 2

[0090] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0091] S1, depositing a 50 nm thick indium tin oxide conductive film on a transparent glass substrate as the lower electrode of the analog memristor;

[0092] S2. On the lower electrode, a 10nm thick tungsten oxide layer is deposited by pulsed laser physical vapor deposition. The heating temperature of tungsten oxide is 250℃, the working pressure is 0.5Pa, the flow rates of argon and oxygen are 15sccm and 10sccm, the deposition time is 20min, and the sputtering power is 150W. Then continue to deposit a 20nm thick high entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions. The heating temperature of the high entropy oxide is 250℃, the working pressure is 2Pa, the flow rates of argon and oxygen are 5sccm and 30sccm, the deposition time is 1min, and the sputtering power is 70W. The obtained stack is used as the resistive switching layer of the analog memristor;

[0093] S3, on the grown stack, continue to deposit a 50nm thick indium tin oxide conductive film as the upper electrode of the device, to obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0094] In Example 2, transparent glass is selected as the high-flat insulating substrate, the thickness of the upper electrode and the lower electrode are both 50nm, and the electrode material is indium tin oxide; the metal oxide of the resistive layer is tungsten oxide, the thickness is 10nm, and it is deposited by pulsed laser physical vapor deposition. Compared with Example 1, the analog memristor constructed by transparent glass and indium tin oxide can realize photoelectric coupling control, the oxide layer is tungsten oxide and has a low thickness, and the stability of the analog resistive device is poor.

[0095] Example 3

[0096] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0097] S1, depositing a 200 nm thick fluorine-doped tin dioxide conductive film on a polyethylene terephthalate insulating substrate as a lower electrode of an analog memristor;

[0098] S2. On the lower electrode, a 100nm thick hafnium oxide layer is deposited by magnetron sputtering physical vapor deposition. The heating temperature of hafnium oxide is 250°C, the working pressure is 0.5Pa, the flow rates of argon and oxygen are 15sccm and 10sccm, the deposition time is 20min, and the sputtering power is 150W. Then continue to deposit a high entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions in a specific thickness of 20nm. The heating temperature of the high entropy oxide is 250°C, the working pressure is 2Pa, the flow rates of argon and oxygen are 5sccm and 30sccm, the deposition time is 1min, and the sputtering power is 70W. The obtained stack is used as the resistive switching layer of the analog memristor;

[0099] S3, on the grown stack, continue to deposit a 200 nm thick fluorine-doped tin dioxide conductive film as the upper electrode of the device, to obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0100] In Example 3, a polyethylene terephthalate substrate is selected as the high-flat insulating substrate, the thickness of the upper electrode and the lower electrode are both 200nm, and the electrode materials are both fluorine-doped tin dioxide; the metal oxide of the resistive layer is hafnium oxide, and the thickness is 100nm. Compared with Example 1, the analog memristor constructed using a polyethylene terephthalate edge substrate can be used on a flexible substrate, the oxide layer is hafnium oxide and has a thick thickness, and the obtained analog resistive device has a large power consumption.

[0101] Example 4

[0102] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0103] S1, depositing a 100 nm thick gold conductive film on a polished silicon oxide / silicon insulator substrate as the lower electrode of the analog memristor;

[0104] S2. On the lower electrode, a 50nm thick tantalum oxide layer is deposited by magnetron sputtering physical vapor deposition. The heating temperature of the tantalum oxide is 30°C, the working pressure is 0.1Pa, the argon and oxygen flow rates are 5sccm and 5sccm, the deposition time is 3min, and the sputtering power is 50W. Then continue to deposit a specific 5nm thick high entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions. The heating temperature of the high entropy oxide is 250°C, the working pressure is 2Pa, the argon and oxygen flow rates are 5sccm and 30sccm, the deposition time is 1min, and the sputtering power is 70W. The obtained stack is used as the resistive switching layer of the analog memristor;

[0105] S3, on the grown stack, continue to deposit a 100 nm thick gold conductive film as the upper electrode of the device, and obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0106] In Example 4, the lower electrode and the upper electrode are metal gold with high stability, the high entropy oxide is 5nm, the metal oxide is tantalum oxide, the heating temperature of the metal oxide layer is 30°C, the working pressure is 0.1Pa, the argon and oxygen flow rates are 5sccm and 5sccm, the film growth time is 3min, and the sputtering power is 50W. Compared with Example 1, the thickness of the high entropy oxide is reduced, and under the growth conditions of this oxide, the stability of the constructed analog memristor is poor.

[0107] Example 5

[0108] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0109] S1, depositing a 100 nm thick tungsten conductive film on a polished silicon oxide / silicon insulating substrate as the lower electrode of the analog memristor;

[0110] S2. On the lower electrode, a 50nm thick manganese oxide layer is deposited by magnetron sputtering physical vapor deposition. The heating temperature of the manganese oxide is 300℃, the working pressure is 5Pa, the argon and oxygen flow rates are 25sccm and 30sccm, the deposition time is 30min, and the sputtering power is 350W. Then continue to deposit a specific 50nm thick high entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions. The heating temperature of the high entropy oxide is 250℃, the working pressure is 2Pa, the argon and oxygen flow rates are 5sccm and 30sccm, the deposition time is 1min, and the sputtering power is 70W. The obtained stack is used as the resistive switching layer of the analog memristor;

[0111] S3, on the grown stack, continue to deposit a 100 nm thick tungsten conductive film as the upper electrode of the device, and obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0112] In Example 5, the lower electrode and the upper electrode are metal tungsten with high stability, the high entropy oxide is 50nm, the metal oxide is manganese oxide, the heating temperature of the metal oxide layer is 300°C, the working pressure is 5Pa, the argon and oxygen flow rates are 25sccm and 30sccm, the film growth time is 30min, and the sputtering power is 350W. Compared with Example 1, the thickness of the high entropy oxide is increased, and under the growth conditions of this oxide, the power consumption of the constructed analog memristor is relatively large.

[0113] Example 6

[0114] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0115] S1, depositing a 100 nm thick platinum conductive film on a polished silicon oxide / silicon insulating substrate as the lower electrode of the analog memristor;

[0116] S2. On the lower electrode, a 50nm thick yttrium oxide layer is deposited by magnetron sputtering physical vapor deposition. The heating temperature of yttrium oxide is 250℃, the working pressure is 0.5Pa, the flow rates of argon and oxygen are 15sccm and 10sccm, the deposition time is 20min, and the sputtering power is 150W. Then continue to deposit a specific 20nm thick high entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions. The heating temperature of the high entropy oxide is 100℃, the working pressure is 1Pa, the flow rates of argon and oxygen are 2sccm and 10sccm, the deposition time is 0.5min, and the sputtering power is 20W. The obtained stack is used as the analog memristor resistive switching layer;

[0117] S3, on the grown stack, continue to deposit a 100 nm thick platinum conductive film as the upper electrode of the device, and obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0118] In Example 6, the metal oxide is yttrium oxide, the heating temperature of the high entropy oxide is 100°C, the working pressure is 1 Pa, the flow rates of argon and oxygen are 2 sccm and 10 sccm, the film growth time is 0.5 min, and the sputtering power is 20 W. Compared with Example 1, the constructed analog memristor has the same high performance, but poor stability.

[0119] Example 7

[0120] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0121] S1, depositing a 100 nm thick platinum conductive film on a polished silicon oxide / silicon insulating substrate as the lower electrode of the analog memristor;

[0122] S2. On the lower electrode, a 50nm thick niobium oxide layer is deposited by magnetron sputtering physical vapor deposition. The heating temperature of the niobium oxide is 250°C, the working pressure is 0.5Pa, the flow rates of argon and oxygen are 15sccm and 10sccm, the deposition time is 20min, and the sputtering power is 150W. Then continue to deposit a specific 20nm thick high entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions. The heating temperature of the high entropy oxide is 400°C, the working pressure is 10Pa, the flow rates of argon and oxygen are 20sccm and 60sccm, the deposition time is 5min, and the sputtering power is 200W. The obtained stack is used as the resistive switching layer of the analog memristor;

[0123] S3, on the grown stack, continue to deposit a 100 nm thick platinum conductive film as the upper electrode of the device, and obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0124] In Example 7, the metal oxide is niobium oxide, the heating temperature of the high entropy oxide is 400°C, the working pressure is 10 Pa, the flow rates of argon and oxygen are 20 sccm and 60 sccm, the film growth time is 5 min, and the sputtering power is 200 W. Compared with Example 1, the constructed analog memristor has the same high performance, but the power consumption is higher.

[0125] Example 8

[0126] A method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides comprises the following steps:

[0127] S1, depositing a 100 nm thick platinum conductive film on a polished silicon oxide / silicon insulating substrate as the lower electrode of the analog memristor;

[0128] S2. On the lower electrode, a 50nm thick vanadium oxide layer is deposited by magnetron sputtering physical vapor deposition. The heating temperature of the vanadium oxide is 250°C, the working pressure is 0.5Pa, the argon and oxygen flow rates are 15sccm and 10sccm, the deposition time is 20min, and the sputtering power is 150W. Then continue to deposit a high-entropy oxide layer made of five elements (iron, cobalt, nickel, cadmium and manganese) with equal atomic proportions in a specific thickness of 20nm. The heating temperature of the high-entropy oxide is 250°C, the working pressure is 2Pa, the argon and oxygen flow rates are 5sccm and 30sccm, the deposition time is 1min, and the sputtering power is 70W. The obtained stack is used as the resistive switching layer of the analog memristor;

[0129] S3, on the grown stack, continue to deposit a 100 nm thick platinum conductive film as the upper electrode of the device, and obtain an analog memristor based on the high entropy oxide and metal oxide stack;

[0130] In Example 8, the metal oxide is vanadium oxide. Compared with Example 1, the stability of the constructed analog memristor is poor.

[0131] In summary, a method for preparing an analog memristor based on a stack of high entropy oxides and metal oxides has the following characteristics:

[0132] 1) The present invention proposes a preparation method of a high entropy oxide and metal oxide stacked analog memristor. Compared with the mutation characteristics of a two-terminal resistive memristor from a high resistance state to a low resistance state, the analog memristor has good analog resistive switching performance.

[0133] 2) The present invention proposes an analog memristor based on a high entropy oxide and metal oxide stack, which has the advantages of simple preparation process, compatibility with CMOS process, low energy consumption, environmental protection and excellent performance. In particular, it has analog resistive switching performance with high electrical conductivity, wide adjustable range and good symmetry under electrical excitation control, and has great application prospects in the fields of information storage and neural network computing.

[0134] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide, characterized in that: The steps include: 1) Depositing a conductive film on an insulating substrate as the lower electrode of an analog memristor; 2) on the lower electrode prepared in step 1), a metal oxide layer is first deposited by physical vapor deposition, and then a high entropy oxide layer is deposited, and the obtained stacked layer is used as a resistive switching layer of the analog memristor; 3) On the stack grown in step 2), a conductive film is further deposited as the upper electrode of the analog memristor; thus, an analog memristor based on a stack of high entropy oxide and metal oxide is obtained.

2. The method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide according to claim 1, characterized in that: In step 1), the insulating substrate is a highly flat transparent glass, a polyethylene terephthalate substrate or a polished silicon oxide / silicon.

3. The method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide according to claim 1, characterized in that: In step 1), the lower electrode is a metal with high stability such as gold, platinum, tungsten, fluorine-doped tin dioxide or indium tin oxide; the thickness of the lower electrode is 50-200 nm; In step 3), the upper electrode is a metal with high stability, such as gold, platinum, tungsten, fluorine-doped tin dioxide or indium tin oxide; the thickness of the upper electrode is 50-200 nm.

4. The method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide according to claim 1, characterized in that: In step 2), the physical vapor deposition method is magnetron sputtering or pulsed laser; the metal oxide layer is titanium oxide, tungsten oxide, hafnium oxide, tantalum oxide, manganese oxide, yttrium oxide, niobium oxide or vanadium oxide; the high entropy oxide layer is a five-element metal oxide prepared by mixing five metals of iron, cobalt, nickel, cadmium and manganese in an equiatomic ratio; the deposition method of the high entropy oxide layer is radio frequency magnetron sputtering.

5. The method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide according to claim 1, characterized in that: In step 2), the thickness of the metal oxide layer is 10-100 nm; the thickness of the high entropy oxide layer is 5-50 nm.

6. The method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide according to claim 1, characterized in that: In step 2), the heating temperature of the metal oxide layer is 30-300°C; the working gas pressure is 0.1-5Pa; argon and oxygen are introduced simultaneously during the deposition process, the argon flow rate is 5-25sccm, and the oxygen flow rate is 5-30sccm; the film growth time is 3-30min; and the sputtering power is 50-350W.

7. The method for preparing an analog memristor based on a stack of high entropy oxide and metal oxide according to claim 1, characterized in that: In step 2), the heating temperature of the high entropy oxide is 100-400°C; the working gas pressure is 1-10Pa; argon and oxygen are introduced simultaneously during the deposition process, the argon flow rate is 2-20sccm, and the oxygen flow rate is 10-60sccm; the film growth time is 0.5-5min; and the sputtering power is 20-200W.

8. An analog memristor based on a high entropy oxide and a metal oxide stack, characterized in that: The method is prepared by any one of claims 1 to 7, and comprises, from bottom to top, an insulating substrate, a lower conductive electrode, a metal oxide, a high entropy oxide and an upper conductive electrode.

9. Application of the analog memristor based on high entropy oxide and metal oxide stack prepared by the preparation method according to any one of claims 1 to 7 in information storage.

10. Application of the analog memristor based on high entropy oxide and metal oxide stack prepared by the preparation method according to any one of claims 1 to 7 in neural network computing.