Metal foil with carrier

By setting a metal layer on the side of the metal foil with the carrier and controlling the concave and convex area of ​​the interface expansion area ratio, the metal layer peeling problem caused by chemical solution is solved, ensuring the correct formation of the circuit pattern and the smooth progress of the multi-layer wiring process.

CN118946454APending Publication Date: 2024-11-12MITSUI MINING & SMELTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380030853.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the process of forming a wiring layer and a resin layer using a metal foil with a carrier, chemical solution damage causes the metal layer to be undesirably peeled off, affecting the formation of the circuit pattern and the progress of subsequent processes.

Method used

By providing a metal layer on the side surface of the carrier, it extends from one side surface to the side surface, and setting an interface expansion area ratio Sdr to control the concave and convex areas within a specified range in the side surface to suppress metal caused by chemical solutions Layer peeling.

Benefits of technology

It effectively suppresses the peeling of metal layer caused by chemical solutions, ensures the formation of circuit patterns and the smooth progress of multi-layer wiring processes, and improves the reliability and yield of the processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946454A_ABST
    Figure CN118946454A_ABST
Patent Text Reader

Abstract

Provided is a metal foil with a carrier capable of suppressing undesired peeling of a metal layer due to immersion of a chemical solution from an end portion. This copper foil with a carrier is provided with: a carrier having a first surface and a second surface facing each other, and a side surface section connected to the first surface and the second surface; the stripping layer is arranged on the first surface of the carrier; and a metal layer provided on the release layer and having a thickness of 0.01 [mu] m or more and 4.0 [mu] m or less. The metal layer extends from the first surface of the carrier to the side surface portion such that at least a portion of the side surface portion is covered by the metal layer. The carrier has, on the side surface portion, or on the side surface portion and the first surface, a concavo-convex region having an interface expansion area ratio Sdr of 3% or more and 39% or less as measured in accordance with ISO 25178, and the concavo-convex region includes a region in which the side surface portion is covered with the metal layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metal foil with a carrier. Background Art

[0002] With the miniaturization and high functionality of electronic devices such as portable electronic devices in recent years, the wiring patterns of printed wiring boards are required to be further miniaturized (fine pitch). In order to meet the above needs, it is expected that the metal foil used in the manufacture of printed wiring boards is thinner than before and has a lower surface roughness. For example, Patent Document 1 (Japanese Patent Publication No. 2005-76091) discloses a method for manufacturing an ultra-thin copper foil with a carrier, which includes the operation of sequentially stacking a peeling layer and an ultra-thin copper foil on a smooth surface of a carrier copper foil whose average surface roughness Rz is reduced to 0.01 μm or more and 2.0 μm or less; It also discloses that a multilayer printed wiring board is obtained by implementing high-density ultra-fine wiring (fine pattern) through the ultra-thin copper foil with a carrier.

[0003] In addition, in order to further reduce the thickness and surface roughness of the metal layer in the metal foil with a carrier, the following scheme has been proposed recently: using a glass substrate, a polished metal substrate, etc. as an ultra-smooth carrier to replace the resin carrier that has been typically used, and forming a metal layer on the ultra-smooth surface by a vapor phase method such as sputtering. For example, Patent Document 2 (International Publication No. 2017 / 150283) discloses a copper foil with a carrier having a carrier (such as a glass carrier), a peeling layer, an anti-reflection layer, and an ultra-thin copper layer in sequence, and records the formation of the peeling layer, the anti-reflection layer, and the ultra-thin copper layer by sputtering. In addition, Patent Document 3 (International Publication No. 2017 / 150284) discloses a copper foil with a carrier having a carrier (such as a glass carrier), an intermediate layer (such as a close-fitting metal layer and a peeling auxiliary layer), a peeling layer, and an ultra-thin copper layer, and records the formation of the intermediate layer, the peeling layer, and the ultra-thin copper layer by sputtering. In both Patent Documents 2 and 3, each layer is formed by sputtering on a support such as glass having excellent surface flatness, thereby achieving an extremely low arithmetic mean roughness Ra of 1.0 nm to 100 nm for the outer surface of the ultra-thin copper layer.

[0004] However, when the metal foil with a carrier is transported, the laminated part of the carrier and the metal layer contacts other components, so sometimes the metal layer is unexpectedly peeled off, and several metal foils with carriers that can cope with the above-mentioned problems are proposed. For example, Patent Document 4 (Japanese Patent Publication No. 2016-137727) discloses a laminated body in which a part or the entire periphery of a metal carrier and a metal foil is covered with resin, and it is believed that by setting the above-mentioned structure to prevent contact with other components, the peeling of the metal foil during processing can be reduced. Patent Document 5 (International Publication No. 2014 / 054812) discloses a metal foil with a carrier, wherein the interface between the resin carrier and the metal foil is firmly bonded by an adhesive layer at at least four corners of the peripheral area, thereby preventing unexpected peeling of the corner part; it is also disclosed that the metal foil with a carrier is cut at a part closer to the inner side than the adhesive layer after the transportation is completed. Patent document 6 (Japanese Patent Publication No. 2000-331537) discloses a copper foil with a carrier, in which the surface roughness of the left and right edges of the copper foil carrier is greater than that of the central portion. It is believed that by doing so, when the copper foil with a carrier is operated or when a copper-clad laminate is produced, undesirable situations such as the copper layer peeling off from the carrier will not occur.

[0005] In addition, when IC chips and the like are mounted on a substrate, cutting of a metal foil with a carrier is performed for the purpose of miniaturization to a size that can be handled by the mounting equipment. During this cutting, since the peeling strength of the peeling layer exposed at the cutting interface is low, the metal layer is sometimes peeled off from the carrier due to the load during cutting, and a metal foil with a carrier that can cope with the above-mentioned problem is also proposed. For example, Patent Document 7 (International Publication No. 2019 / 163605) discloses a concave-convex area with a maximum height Rz of 1.0 μm or more and 30.0 μm or less is linearly set as a cutting margin on the surface of a flat glass carrier, and by doing so, it is possible to prevent the undesired peeling of the copper layer during and after the cutting of the copper foil of the glass carrier. Patent document 8 (Japanese Patent Publication No. 2019-102779) discloses a carrier substrate, which includes a core layer, a first metal layer arranged on the core layer, a release layer arranged on the first metal layer, and a second metal layer arranged on the release layer, wherein at least one of the first metal layer, the release layer, and the second metal layer constitutes a plurality of unit pattern portions having an area smaller than that of the core layer. According to the above configuration, since the state of preventing separation is designed by the unit pattern portion, it is believed that the release layer can be prevented from being separated during cutting into quadrilateral or strip-shaped units.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-76091

[0009] Patent Document 2: International Publication No. 2017 / 150283

[0010] Patent Document 3: International Publication No. 2017 / 150284

[0011] Patent Document 4: Japanese Patent Application Publication No. 2016-137727

[0012] Patent Document 5: International Publication No. 2014 / 054812

[0013] Patent Document 6: Japanese Patent Application Publication No. 2000-331537

[0014] Patent Document 7: International Publication No. 2019 / 163605

[0015] Patent Document 8: Japanese Patent Application Publication No. 2019-102779 Summary of the invention

[0016] However, in the process of forming a redistribution layer including a wiring layer and a resin layer using a metal foil with a carrier, various chemical solutions such as a developer of a liquid resist, a stripping solution, a copper sulfate plating solution, and an etching solution for a metal layer can be used. By using such a chemical solution, the chemical solution damage is accumulated at the end of the metal foil with a carrier. Then, the chemical solution penetrates into the stripping layer from the end of the metal foil with a carrier, and the metal layer may be undesirably stripped from the carrier. As a result, the problem of not being able to form a desired circuit pattern and not being able to proceed to the subsequent process may occur.

[0017] The inventors of the present invention have obtained the following insight: in a metal foil with a carrier, a metal layer is extended from one surface of the carrier to a side portion, and a concave-convex area with an interface extension area ratio Sdr controlled within a specified range is provided on the side portion of the carrier in a manner that includes an area covered by the metal layer, thereby being able to suppress undesired peeling of the metal layer caused by infiltration of a chemical solution from the end.

[0018] Therefore, an object of the present invention is to provide a metal foil with a carrier that can suppress unintended peeling of a metal layer due to penetration of a chemical solution from an end portion.

[0019] According to the present invention, the following aspects are provided.

[0020] [Method 1]

[0021] A metal foil with a carrier, comprising:

[0022] A carrier having a first surface and a second surface opposite to each other, and a side surface connected to the first surface and the second surface;

[0023] a peeling layer disposed on the first surface of the carrier; and

[0024] The metal layer is provided on the release layer and has a thickness of 0.01 μm or more and 4.0 μm or less.

[0025] The metal layer extends from the first surface of the carrier to the side surface in a manner that at least a portion of the side surface is covered by the metal layer.

[0026] The carrier has a concavo-convex region having an interface extension area ratio Sdr of 3% or more and 39% or less measured in accordance with ISO25178 on the side surface, or on the side surface and the first surface, and the concavo-convex region includes a region of the side surface covered by the metal layer.

[0027] [Method 2]

[0028] The metal foil with a carrier according to aspect 1, wherein the concavo-convex region is provided over the entire circumference of the side surface portion.

[0029] [Method 3]

[0030] The metal foil with a carrier according to embodiment 1 or 2, wherein the carrier has, on the first surface, a flat region having an interface expansion area ratio Sdr of less than 5% as measured in accordance with ISO 25178, and the concavo-convex region surrounding the flat region,

[0031] The concavo-convex region is provided continuously from the side surface portion of the carrier to the first surface.

[0032] [Method 4]

[0033] The metal foil with a carrier according to Embodiment 3, wherein a ratio of an area of ​​the concavo-convex region to a total area of ​​the flat region and the concavo-convex region on the first surface of the carrier is 0.01 or more and 0.5 or less.

[0034] [Method 5]

[0035] The metal foil with a carrier according to aspect 3 or 4, wherein the concavo-convex region is provided on the first surface in a pattern that divides the flat region into two or more regions.

[0036] [Method 6]

[0037] A metal foil with a carrier according to any one of methods 1 to 5, wherein the metal foil with a carrier has a height difference portion on the concave-convex area whose height is lower than the flat surface of the metal layer in the flat area, and the height difference between the height difference portion and the flat surface is greater than 0.05 μm and is less than 100 μm.

[0038] [Method 7]

[0039] The metal foil with a carrier according to any one of aspects 1 to 6, wherein the carrier has a micro Vickers hardness of 500 HV or more and 3000 HV or less.

[0040] [Method 8]

[0041] The metal foil with a carrier according to any one of aspects 1 to 7, wherein the metal layer is composed of at least one metal selected from the group consisting of Cu, Au, and Pt.

[0042] [Method 9]

[0043] A metal foil with a carrier according to any one of methods 1 to 8, wherein an intermediate layer comprising at least one metal selected from the group consisting of Cu, Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, In, Sn, Zn, Ga and Mo is provided between the carrier and the peeling layer.

[0044] [Method 10]

[0045] A metal foil with a carrier according to any one of methods 1 to 9, further comprising a functional layer composed of at least one metal selected from the group consisting of Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni and Mo between the peeling layer and the metal layer.

[0046] [Method 11]

[0047] The metal foil with a carrier according to any one of aspects 1 to 10, wherein the carrier is a glass substrate or a silicon substrate containing SiO 2 .

[0048] [Method 12]

[0049] The metal foil with a carrier according to Embodiment 11, wherein the carrier is the glass substrate, and the glass substrate is composed of at least one selected from the group consisting of quartz glass, borosilicate glass, alkali-free glass, soda-lime glass, and aluminosilicate glass.

[0050] [Method 13]

[0051] The metal foil with a carrier according to any one of aspects 1 to 12, wherein the peel strength of the carrier in the concavo-convex region is 20 gf / cm or more and 3000 gf / cm or less.

[0052] [Method 14]

[0053] The metal foil with a carrier according to any one of aspects 1 to 13, wherein the metal foil with a carrier has a redistribution layer on the metal layer.

[0054] When the metal foil with a carrier is viewed in plan, at least a portion of the redistribution layer reaches an end portion of the carrier.

[0055] [Method 15]

[0056] The metal foil with a carrier according to embodiment 14, wherein at least a portion of an end portion of the redistribution layer is located on the concave-convex region.

[0057] [Method 16]

[0058] The metal foil with a carrier according to any one of aspects 1 to 15, wherein a line width of the pattern of the concavo-convex region R provided on the first surface is 0.1 mm or more and 50 mm or less.

[0059] [Method 17]

[0060] The metal foil with a carrier according to any one of aspects 1 to 16, wherein the metal foil with a carrier further comprises:

[0061] a second peeling layer disposed on the second surface of the carrier; and

[0062] a second metal layer provided on the second release layer and having a thickness of 0.01 μm or more and 4.0 μm or less,

[0063] The second metal layer extends from the second surface of the carrier to the side surface in a manner that at least a portion of the side surface is covered by the second metal layer.

[0064] The carrier further has the uneven region on the second surface, and the uneven region includes a region of the side surface portion covered by the second metal layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is a schematic cross-sectional view showing an example of the metal foil with a carrier of the present invention.

[0066] Figure 2 is a schematic cross-sectional view of a carrier, showing a first side, a second side and a side portion.

[0067] Figure 3A This is a top view of the wafer-shaped carrier viewed from the first surface side, showing the concave and convex regions surrounding the flat region.

[0068] Figure 3B It is a top view of the panel-shaped carrier viewed from the first surface side, showing the concave and convex regions surrounding the flat region.

[0069] Figure 4 This is a process flow chart showing an example of a conventional process for forming wiring using a metal foil with a carrier.

[0070] Figure 5 This is a process flow chart showing an example of a wiring formation process using another metal foil with a carrier.

[0071] Figure 6 This is a process flow chart showing an example of a wiring formation process based on one embodiment of the metal foil with a carrier of the present invention.

[0072] Fig. 7A This is a process flow chart for explaining the change of the surface profile of the carrier accompanying the progress of the sandblasting process, and shows the first half of the process.

[0073] Figure 7B is a process flow chart for explaining the change of the surface profile of the carrier accompanying the progress of the sandblasting process, showing the following Fig. 7A The second half of the process.

[0074] Fig. 8A This is a schematic cross-sectional view for explaining the method of measuring the breaking load.

[0075] Figure 8B It is shown Fig. 8A A schematic top view of the positional relationship between the carrier and the supporting member S is shown. DETAILED DESCRIPTION

[0076] definition

[0077] In this specification, "interface expansion area ratio Sdr" or "Sdr" refers to a parameter indicating how much the expansion area (surface area) of a defined area measured in accordance with ISO25178 increases relative to the area of ​​the defined area. In this specification, the interface expansion area ratio Sdr is expressed as the increase in surface area (%). The smaller the value, the closer the surface shape is to being flat, and the Sdr of a completely flat surface is 0%. On the other hand, the larger the value, the more concave and convex the surface shape is. For example, when the Sdr of a surface is 30%, it means that the surface area of ​​the surface is 30% larger than that of a completely flat surface. Sdr can be calculated by measuring the surface profile of a specified measurement area (e.g., a two-dimensional area of ​​258.346μm×258.348μm) of the target surface using a commercially available laser microscope (e.g., using a 50x objective lens). In this specification, the numerical value of Sdr is a value measured under the conditions where the cutoff wavelength based on the S filter is set to 0.8μm and no cutoff based on the L filter is performed.

[0078] Metal foil with carrier

[0079] Figure 1 An example of the metal foil with a carrier of the present invention is schematically shown. Figure 1 As shown, the metal foil with a carrier 10 of the present invention sequentially comprises a carrier 12, a peeling layer 16, and a metal layer 18. As desired, the metal foil with a carrier 10 may further comprise an intermediate layer 14 between the carrier 12 and the peeling layer 16, and may further comprise a functional layer 17 between the peeling layer 16 and the metal layer 18. In addition, the metal foil with a carrier 10 may further comprise a redistribution layer 20 on the metal layer 18. Figure 2 As shown, the carrier 12 has a first surface 12a and a second surface 12b opposite to each other, and a side surface 12c connected to the first surface 12a and the second surface 12b. The peeling layer 16 is a layer provided on the carrier 12. The metal layer 18 is a layer provided on the peeling layer 16 and having a thickness of 0.01 μm or more and 4.0 μm or less. The metal layer 18 extends from the first surface 12a of the carrier to the side surface 12c, so that at least a portion of the side surface 12c of the carrier 12 is covered by the metal layer 18. The carrier 12 has a concave-convex region R having an interface extension area ratio Sdr of 3% or more and 39% or less on the side surface 12c, or on the side surface 12c and the first surface 12a. The concave-convex region R includes an area where the side surface 12c is covered by the metal layer 18. In this way, in the metal foil 10 with a carrier, the metal layer 18 extends from the first surface 12a of the carrier to the side surface 12c, and on the side surface 12c of the carrier, a concave-convex area R with an interface expansion area ratio Sdr controlled within a specified range is set in a manner that includes an area covered by the metal layer 18, thereby suppressing undesirable peeling of the metal layer 18 caused by the infiltration of a chemical solution from the end.

[0080] As described above, in the process of forming the redistribution layer using the metal foil with a carrier, various chemical solutions such as the developer of the dry film resist, the stripping solution, the copper sulfate plating solution, and the etching solution of the metal layer are used. By using the above-mentioned chemical solutions, chemical solution damage will accumulate at the end of the metal foil with a carrier. Then, the chemical solution penetrates into the stripping layer from the end of the metal foil with a carrier, etc., and the metal layer may be undesirably stripped from the carrier. As a result, the desired circuit pattern cannot be formed, and the problem of not being able to proceed to the next process may occur.

[0081] The problem can be solved appropriately by the metal foil 10 with a carrier of the present invention. First, by covering at least a portion of the side portion 12c of the carrier with the metal layer 18, the infiltration of the chemical solution can be suppressed and the end of the stripping layer 16 will not be exposed. On the other hand, even if the above-mentioned structure is used, the end of the metal layer 18, etc. will dissolve and the chemical solution will penetrate into the stripping layer 16. In this regard, by setting the concave-convex area R in a manner that includes the area covered by the metal layer 18 of the side portion 12c, the various layers extending to the side portion 12c of the metal layer 18, etc., also become a shape rich in concave-convex. Therefore, even in the case where the chemical solution penetrates from the end of the metal foil 10 with a carrier, the further infiltration of the chemical solution can be suppressed by the concave-convex shape, and the chemical solution can be prevented from reaching the stripping layer 16 present on the first surface 12a of the carrier. As a result, the undesired peeling of the metal layer 18 can be extremely effectively suppressed, and the formation process of the multi-layer wiring can be fully tolerated.

[0082] The concavo-convex region R is preferably provided on the entire circumference of the side surface portion 12c of the carrier. By doing so, it is possible to prevent the chemical solution from penetrating into the peeling layer 16 around the metal foil 10 with the carrier, and it is possible to further effectively suppress the undesired peeling of the metal layer 18. It should be noted that when the carrier 12 is viewed in section, the side surface portion 12c of the carrier may have a curved surface shape (see Figure 2 ), may have a planar shape vertically connecting the first surface 12a and the second surface 12b, and preferably has a curved surface shape from the viewpoint of preventing the carrier 12 from breaking.

[0083] The interface extension area ratio Sdr of the concave-convex region R of the carrier 12 is 3% or more and 39% or less, preferably 3.5% or more and 35% or less, more preferably 4.0% or more and 30% or less, further preferably 4.5% or more and 25% or less, and particularly preferably 5% or more and 15% or less. If it is within such a range, the easy peelability of the concave-convex region R with the peeling layer 16 is reduced (the adhesion is improved), and the undesirable peeling of the metal layer can be effectively suppressed. In addition, the strength reduction of the carrier 12 can be effectively suppressed. Furthermore, in the case where the concave-convex region R is also provided on the first surface 12a, when the metal foil 10 with a carrier is cut according to the pattern of the concave-convex region R as described later, good peeling strength at the cut surface can be ensured, and undesirable peeling of the metal layer 18 accompanying the cutting can be effectively suppressed. On this basis, it is not easy to produce sharp parts and broken parts on the surface of the carrier 12, so the number of granular fragments of the carrier generated when the metal foil 10 with a carrier is cut can be reduced. The peel strength of the carrier 12 in the concavo-convex region R is preferably 20 gf / cm or more and 3000 gf / cm or less, more preferably 25 gf / cm or more and 2000 gf / cm or less, further preferably 30 gf / cm or more and 1000 gf / cm or less, particularly preferably 35 gf / cm or more and 500 gf / cm or less, and most preferably 50 gf / cm or more and 300 gf / cm or less. Within this range, undesired peeling of the metal layer 18 can be effectively suppressed when the metal foil 10 with a carrier is cut, and the concavo-convex region R can be formed with good productivity. The peel strength is a value measured in accordance with JIS Z 0237-2009 as described in the examples described later.

[0084] like Figure 3A and 3B As shown, the carrier 12 preferably has a flat region F and a concave-convex region R surrounding the flat region F on the first surface 12a. The interface extension area ratio Sdr of the flat region F of the carrier 12 is less than 5%, preferably not less than 0.01% and not more than 4.0%, more preferably not less than 0.03% and not more than 3.0%, further preferably not less than 0.05% and not more than 1.0%, particularly preferably not less than 0.07% and not more than 0.50%, and most preferably not less than 0.08% and not more than 0.50%. By making the carrier 12 have a flat region F with a small Sdr, the surface on the flat region F of the metal layer 18 stacked on the first surface 12a of the carrier via the release layer 16 also becomes a flat shape, and the flat surface of the metal layer 18 can be suitably formed with the formation of a fine pattern. It should be noted that the shape of the carrier 12 when viewed from above can be Figure 3A The circular shape (wafer shape) shown can also be Figure 3BIn the case where the carrier 12 is a single crystal silicon carrier, it is typically provided with a reference point at the outer periphery to indicate the crystal orientation. Figure 3A The notch N shown, or the orientation flat (Orientation Flat). Generally, when the diameter of the single crystal silicon is less than 200 mm, an orientation flat is formed, and when it is more than 200 mm, a notch N is formed.

[0085] The first surface 12a of the carrier has a concave-convex region R, such as Figure 1 As shown, the concavo-convex region R is preferably provided continuously from the side surface portion 12c of the carrier to the first surface 12a. By doing so, even after the unnecessary part of the metal layer 18 (and the functional layer 17 if present) is etched away, the infiltration of the chemical solution into the peeling layer 16 can be effectively suppressed. The following is an explanation of this effect by comparison with a conventional metal foil with a carrier.

[0086] first, Figure 4 An example of a wiring formation process based on a conventional metal foil 110 with a carrier is shown. The metal foil 110 with a carrier has a first intermediate layer 114a, a second intermediate layer 114b, a peeling layer 116, a functional layer 117, a metal layer 118 and a redistribution layer 120 on a carrier 112 in this order, and the end of the peeling layer 116 is exposed ( Figure 4 (i)). In order to form wiring on the metal foil 110 with a carrier, a photoresist layer is formed, a copper electroplating layer is formed, the photoresist layer is stripped, and copper flash etching is performed as desired according to a known method. For example, as described below. First, a photoresist layer is formed on the surface of the metal layer 118 in a prescribed pattern. The photoresist is preferably a photosensitive film, such as a photosensitive dry film. The photoresist layer is given a prescribed wiring pattern by exposure and development. If necessary, a copper electroplating layer is formed on the exposed surface of the metal layer 118 (i.e., the portion not masked by the photoresist layer). The copper electroplating can be performed using a known method without particular limitation. Next, the photoresist layer is stripped. In this way, after removing the unnecessary portions of the metal layer 118 and the functional layer 117 ( Figure 4 (ii)), when the metal foil 110 with a carrier is immersed in a chemical solution ( Figure 4 In (iii)), the chemical solution infiltrates from the exposed end of the release layer 116 , whereby undesired release may occur between the carrier 112 and the metal layer 118 .

[0087] in addition, Figure 5An example of a wiring formation process based on another metal foil 210 with a carrier is shown. The metal foil 210 with a carrier has a first intermediate layer 214a, a second intermediate layer 214b, a peeling layer 216, a functional layer 217, a metal layer 218 and a redistribution layer 220 on a carrier 212 in this order, and the side surface of the carrier 212 is covered by the metal layer 218 ( Figure 5 (i)). The metal foil 210 with the carrier is etched in the same manner as the above wiring formation process to remove unnecessary portions of the metal layer 218 and the functional layer 217 ( Figure 5 (ii)), when the metal foil 210 with a carrier is immersed in a chemical solution ( Figure 5 In (iii)), the chemical solution infiltrates from the exposed end of the release layer 216 , whereby undesired release may occur between the carrier 212 and the metal layer 218 .

[0088] on the other hand, Figure 6 An example of a wiring formation process based on one embodiment of the metal foil with carrier 10 of the present invention is shown. Figure 6 As shown in (i), the metal foil with a carrier 10 has a first intermediate layer 14a, a second intermediate layer 14b, a peeling layer 16, a functional layer 17, a metal layer 18 and a redistribution layer 20 on the carrier 12 in this order. Next, the side surface 12c of the carrier is covered with the metal layer 18, and the concave-convex region R is continuously provided from the side surface 12c of the carrier to the first surface 12a. The metal foil with a carrier 10 is etched in the same manner as the above-mentioned wiring formation process, and after removing unnecessary parts of the metal layer 18 and the functional layer 17 ( Figure 6 (ii)), when the metal foil 10 with a carrier is immersed in a chemical solution ( Figure 6 (iii)), the chemical solution contacts the end of the exposed peeling layer 16. However, since the concavo-convex region R exists on the first surface 12a of the carrier, the various layers such as the peeling layer 16 on the first surface 12a also have a shape rich in concavo-convexity. Therefore, even if the chemical solution infiltrates from the end of the exposed peeling layer 16, the further infiltration of the chemical solution can be suppressed by the concavo-convex shape, and the time required for the chemical solution to reach the inside of the peeling layer 16 (for example, the flat region F) can be delayed (thus preventing it from reaching).

[0089] The concave-convex region R may also be provided over the entire area in the height direction (vertical direction relative to the first surface 12a and the second surface 12b) of the side surface 12c of the carrier. By doing so, the strength of the carrier 12 is made uniform, which also helps prevent cracking. That is, when the height of the first surface 12a is set to 0% and the height of the second surface 12b is set to 100% in a cross-sectional view of the carrier 12, it is preferred that the concave-convex region R is provided continuously from the side surface 12c to a height exceeding 0% and below 100%. The upper limit of the height is not particularly limited, and from the viewpoint of the formatibility of the concave-convex region R, it is typically below 95%, more typically below 90%, and further typically below 85%. On the other hand, from the viewpoint of providing the concave-convex region R continuously from the side surface 12c of the carrier to the first surface 12a, the lower limit of the above-mentioned height is preferably 0%.

[0090] For the first surface 12a of the carrier, from the viewpoint of sufficiently ensuring an area (i.e., flat area F) that can provide the metal layer 18 with the flatness required for forming a fine pattern, the ratio of the area of ​​the concave-convex area R to the total area of ​​the flat area F and the concave-convex area R is preferably 0.01 or more and 0.5 or less. The ratio of the area of ​​the concave-convex area R is more preferably 0.02 or more and 0.45 or less, further preferably 0.05 or more and 0.40 or less, and particularly preferably 0.1 or more and 0.35 or less.

[0091] The concavoconvex region R may also be provided on the first surface 12a in a pattern that divides the flat region F into two or more regions. In the case of the above-mentioned configuration, by cutting the metal foil 10 with a carrier according to the pattern of the concavoconvex region R, a plurality of metal foils with a carrier 10 having each flat region F and miniaturized to a size that can be handled by the circuit mounting equipment can be obtained. The cut surface of the metal foil 10 with a carrier after miniaturization exists in the concavoconvex region R, so the peeling strength of the peeling layer 16 at the cut surface is high, so that not only the metal layer 18 is prevented from being undesirably peeled off from the cut surface during cutting, but also the metal layer 18 can be extremely effectively prevented from being undesirably peeled off from the cut surface after cutting (for example, during the transportation and processing of the metal foil with a carrier in the installation process). From the aspect of easily dividing a plurality of flat regions F into equal shapes and sizes suitable for the circuit mounting substrate, it is preferred that the pattern of the concavoconvex region R is set in a lattice, a fence or a cross shape. Among them, it is particularly preferred to set the pattern of the concavoconvex region R in a lattice or a fence shape. By doing so, since the entire or most of the periphery of each flat region F can be surrounded by the concavo-convex region R, it is difficult for an unintended starting point of peeling to occur at the end of each of the metal foils with carriers 10 divided after dicing.

[0092] The line width of the pattern of the concavo-convex region R provided on the first surface 12a is preferably 0.1 mm to 50 mm, more preferably 0.2 mm to 45 mm, further preferably 0.3 mm to 40 mm, and particularly preferably 0.3 mm to 35 mm. By setting it within such a range, it is easy to position a cutting unit such as a cutter in the concavo-convex region R and it also becomes easy to cut, while ensuring a large amount of flat area F and expecting to achieve various advantages based on the concavo-convex region R.

[0093] The method for forming the concavo-convex region R is not particularly limited. For example, a preferred concavo-convex region R can be formed by processing a specified area on the surface of the flat carrier 12 using a physical method such as sandblasting. Therefore, the metal foil 10 with a carrier typically has a height difference portion on the concavo-convex region R whose height is lower than the flat surface of the metal layer 18 in the flat region F. The height difference between the height difference portion and the flat surface is preferably greater than 0.05 μm and less than 100 μm, more preferably greater than 0.1 μm and less than 80 μm, further preferably greater than 0.5 μm and less than 50 μm, and particularly preferably greater than 1 μm and less than 30 μm. If it is within this range, the chemical solution is further effectively inhibited from penetrating into the interior of the peeling layer 16 (for example, in the flat region F), and the strength of the carrier 12 can be prevented from being reduced as described later. The height difference of the height difference portion can be calculated by measuring and analyzing the surface profile on the first surface 12a using a commercially available laser microscope. The preferred measurement conditions and analysis conditions for the height difference of the height difference portion using a laser microscope are shown in the embodiments described later.

[0094] Here, the change in the surface profile of the carrier 12 accompanying the progress of the sandblasting treatment is referred to Fig. 7A and 7B First, if the medium M is projected onto the surface of the prepared carrier 12 by sandblasting, fragments ( Fig. 7A Then, if the projection of the medium M continues, the fragments gradually intensify and the surface profile of the carrier 12 changes ( Fig. 7A (iii)), after which the fragments reach the entire processing area of ​​the carrier 12 and the surface profile is saturated ( Figure 7B (iv)). If the projection of the medium M is further continued in this state, the carrier 12 is cut while maintaining the saturated surface profile, thereby the thickness of the carrier 12 becomes thinner and the strength decreases. In this regard, by controlling the height difference of the height difference portion within the above range, the desired function as the concave-convex region R can be exerted, and the carrier 12 can be prevented from becoming too thin and causing a decrease in strength.

[0095] As long as the carrier 12 has Sdr within the above-mentioned specified range (or Sdr can be controlled by processing), its material is not particularly limited, and it is preferably composed of glass, silicon or metal, and more preferably a glass substrate or a silicon substrate containing SiO2. As a silicon substrate, any substrate can be used as long as it contains Si as an element, and SiO2 substrates, SiN substrates, Si single crystal substrates, Si polycrystalline substrates, etc. can be applied, but Si single crystal substrates or Si polycrystalline substrates are preferred. Preferred examples of metals constituting the carrier 12 include copper, titanium, nickel, stainless steel, aluminum, etc. The form of the carrier 12 can be any of a sheet, a film, and a plate. In addition, the carrier 12 can be a stack of these sheets, films, plates, etc. For example, the carrier 12 is preferably a SiO2 substrate, a Si single crystal substrate, a glass plate, etc., which can function as a rigid support. From the viewpoint of preventing the warping of the metal foil 10 with a carrier in the process accompanied by heating, it is more preferable to use a Si single crystal substrate or a glass plate with a thermal expansion coefficient (CTE) lower than 25ppm / K (typically 1.0ppm / K or more and 23ppm / K or less). In addition, from the viewpoint of ensuring the handling property and the flatness during chip mounting, the micro-Vickers hardness of the carrier 12 is preferably 500HV or more and 3000HV or less, and more preferably 600HV or more and 2000HV or less. In the case where glass is used as a carrier, it has the advantages of being able to make the surface of the metal layer 18 extremely smooth due to its light weight, low thermal expansion coefficient, high insulation, high rigidity and flat surface. In addition, when the carrier is glass, after forming the wiring layer, it has advantages in terms of excellent visibility during image detection, surface flatness (coplanarity) that is beneficial when mounting electronic components, decontamination in the printed wiring board manufacturing process, chemical resistance in various plating processes, and the ability to use a chemical separation method when peeling the carrier 12 from the metal foil 10 with a carrier. The carrier 12 is preferably a glass substrate containing SiO2, more preferably a glass containing 50% by weight or more of SiO2, and further preferably a glass containing 60% by weight or more of SiO2. Preferred examples of glass constituting the carrier 12 include quartz glass, borosilicate glass, alkali-free glass, soda-lime glass, aluminosilicate glass, and combinations thereof, more preferably borosilicate glass, alkali-free glass, soda-lime glass, and combinations thereof, particularly preferably alkali-free glass, soda-lime glass, and combinations thereof, and most preferably alkali-free glass. When the carrier 12 is composed of borosilicate glass, alkali-free glass, or soda-lime glass, it is preferred because the broken pieces of the carrier 12 can be reduced when the metal foil 10 with the carrier is cut. Alkali-free glass refers to glass having silicon dioxide, aluminum oxide, boron oxide, and alkaline earth metal oxides such as calcium oxide and barium oxide as main components, further containing boric acid, and substantially no alkali metal.The alkali-free glass has a low thermal expansion coefficient of 3 ppm / K or more and 5 ppm / K or less in a wide temperature range from 0°C to 350°C and is stable, so it has the advantage of being able to minimize the warping of the glass in the process accompanied by heating. When a substrate containing silicon is used as the carrier 12, it is lightweight, has a low thermal expansion coefficient, has high insulation, is rigid and has a flat surface, just like glass, so it has the advantages of being able to make the surface of the metal layer 18 extremely smooth. In addition, when the carrier 12 is a substrate containing silicon, it has advantages in that it has surface flatness (coplanarity) that is conducive to the formation of fine circuits, has chemical resistance in the decontamination process in the wiring manufacturing process, and in various plating processes, and that a chemical separation method can be used when the carrier 12 is peeled off from the metal foil 10 with the carrier. The thickness of the carrier 12 is preferably 100 μm or more and 2000 μm or less, more preferably 300 μm or more and 1800 μm or less, and further preferably 400 μm or more and 1100 μm or less. When the thickness of the carrier 12 is within such a range, it is possible to achieve a reduction in the thickness of the printed wiring board while ensuring appropriate strength that does not cause problems in handling, and to reduce warping that occurs when electronic components are mounted.

[0096] The intermediate layer 14, which is provided as desired, is a layer which is interposed between the carrier 12 and the peeling layer 16 and helps to ensure the adhesion between the carrier 12 and the peeling layer 16. Examples of metals constituting the intermediate layer 14 include Cu, Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, In, Sn, Zn, Ga, Mo, and combinations thereof (hereinafter referred to as metal M), preferably Cu, Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, Mo, and combinations thereof, more preferably Cu, Ti, Zr, Al, Cr, W, Ni, Mo, and combinations thereof, further preferably Cu, Ti, Al, Cr, Ni, Mo, and combinations thereof, and particularly preferably Cu, Ti, Al, Ni, and combinations thereof. The intermediate layer 14 may be a pure metal or an alloy. The metal constituting the intermediate layer 14 may also contain unavoidable impurities arising from raw material components, film forming processes, and the like. In addition, there is no particular restriction, and in the case where the intermediate layer 14 is exposed to the atmosphere after film formation, the presence of oxygen mixed therein is acceptable. The upper limit of the above-mentioned metal content is not particularly limited, and can be 100 atomic %. The intermediate layer 14 is preferably a layer formed by physical vapor deposition (PVD) method, and more preferably a layer formed by sputtering. From the viewpoint of uniformity of film thickness distribution, it is particularly preferred that the intermediate layer 14 is a layer formed by magnetron sputtering using a metal target. The thickness of the intermediate layer 14 is preferably more than 10nm and less than 1000nm, more preferably more than 30nm and less than 800nm, further preferably more than 60nm and less than 600nm, and particularly preferably more than 100nm and less than 400nm. By setting such a thickness, an intermediate layer having the same roughness as the carrier can be formed. The thickness is a value measured by analyzing the layer cross section using an energy dispersive X-ray spectrometer (TEM-EDX) of a transmission electron microscope.

[0097] The intermediate layer 14 may be composed of a single layer or may be composed of two or more layers. When the intermediate layer 14 is composed of a single layer, the intermediate layer 14 preferably includes a layer containing a metal composed of Cu, Al, Ti, Ni, or a combination thereof (e.g., an alloy, an intermetallic compound), more preferably Al, Ti, or a combination thereof (e.g., an alloy, an intermetallic compound), and further preferably a layer mainly containing Al or a layer mainly containing Ti. On the other hand, when the intermediate layer 14 is made of a metal or alloy whose adhesion to the carrier 12 is not sufficiently high, such as Figure 1As shown, it is preferred that the intermediate layer 14 is formed into a two-layer structure having a first intermediate layer 14a and a second intermediate layer 14b in order from the carrier 12. That is, by providing a layer composed of a metal (such as Ti) or an alloy having excellent adhesion to the carrier 12 as the first intermediate layer 14a adjacent to the carrier 12, and providing a layer composed of a metal (such as Cu) or an alloy having poor adhesion to the carrier 12 as the second intermediate layer 14b adjacent to the peeling layer 16, the adhesion to the carrier 12 can be improved. Therefore, as an example of a preferred two-layer structure of the intermediate layer 14, a stacked structure including a Ti-containing layer adjacent to the carrier 12 and a Cu-containing layer adjacent to the peeling layer 16 can be cited. In addition, if the balance of the constituent elements and thickness of each layer of the two-layer structure is changed, the peel strength also changes, so it is preferred to appropriately adjust the constituent elements and thickness of each layer. It should be noted that the scope of the "metal M-containing layer" in this specification also includes alloys containing elements other than metal M within the range that does not impair the peelability of the carrier. Therefore, the intermediate layer 14 can also be referred to as a layer mainly containing the metal M. From the above-mentioned aspect, the content of the metal M in the intermediate layer 14 is preferably 50 atomic % or more and 100 atomic % or less, more preferably 60 atomic % or more and 100 atomic % or less, further preferably 70 atomic % or more and 100 atomic % or less, particularly preferably 80 atomic % or more and 100 atomic % or less, and most preferably 90 atomic % or more and 100 atomic % or less.

[0098] In the case where the intermediate layer 14 is composed of an alloy, a Ni alloy can be cited as an example of a preferred alloy. The Ni content of the Ni alloy is preferably 45% by weight or more and 98% by weight or less, more preferably 55% by weight or more and 90% by weight or less, and further preferably 65% ​​by weight or more and 85% by weight or less. The preferred Ni alloy is an alloy of Ni and at least one selected from the group consisting of Cr, W, Ta, Co, Cu, Ti, Zr, Si, C, Nd, Nb and La, and more preferably an alloy of Ni and at least one selected from the group consisting of Cr, W, Cu and Si. In the case where the intermediate layer 14 is made into a Ni alloy layer, from the viewpoint of uniformity of film thickness distribution, it is particularly preferred to use a layer formed by a magnetron sputtering method using a Ni alloy target.

[0099] The peeling layer 16 is a layer that can peel off or easily peel off the carrier 12 and the intermediate layer 14 when present. The peeling layer 16 can be any of an organic peeling layer and an inorganic peeling layer, and can be a layer that can be peeled off by a laser peeling method (laser peeling, LLO). In the case where the peeling layer 16 is composed of a material that can be peeled off by laser peeling, the peeling layer 16 can be composed of a resin whose interface bonding strength is reduced by laser beam irradiation after curing, or it can also be a layer of silicon, silicon carbide, etc. modified by laser beam irradiation. As examples of organic components used in the case where the peeling layer 16 is an organic peeling layer, nitrogen-containing organic compounds, sulfur-containing organic compounds, carboxylic acids, etc. can be listed. As examples of nitrogen-containing organic compounds, triazole compounds, imidazole compounds, etc. can be listed. On the other hand, as examples of inorganic components used in inorganic peeling layers, metal oxides or metal nitrides containing at least one or more of Ni, Mo, Co, Cr, Fe, Ti, W, P, Zn, Cu, Al, Nb, Zr, Ta, Ag, In, Sn, and Ga, or carbon layers can be listed. Among these, in particular, from the perspective of ease of stripping and film formation, the stripping layer 16 is preferably a carbon-containing layer, that is, preferably a layer mainly containing carbon, more preferably a layer mainly containing carbon or hydrocarbons, and further preferably a layer formed of amorphous carbon as a hard carbon film. In this case, the carbon concentration of the stripping layer 16 (i.e., the carbon-containing layer) measured by XPS is preferably 60 atomic % or more, more preferably 70 atomic % or more, further preferably 80 atomic % or more, and particularly preferably 85 atomic % or more. The upper limit of the carbon concentration is not particularly limited, and can be 100 atomic %, and it is realistic to be 98 atomic % or less. The stripping layer 16 may contain unavoidable impurities (for example, oxygen, hydrogen, etc. from the surrounding environment such as the atmosphere). In addition, the stripping layer 16 may be mixed with metal atoms of a type other than the metal contained in the stripping layer 16 due to the film forming method of the functional layer 17 or the metal layer 18. When a carbon-containing layer is used as the peeling layer 16, the mutual diffusion and reactivity with the carrier are small, and even if it is subjected to pressing processing at a temperature exceeding 300°C, the formation of a metal bond caused by high-temperature heating between the metal layer and the bonding interface can be prevented, thereby maintaining a state in which the carrier is easily peeled and removed. From the aspects of suppressing excessive impurities in the peeling layer 16 and the continuous productivity of the film formation of the intermediate layer 14 set as desired, it is preferred that the peeling layer 16 is also a layer formed by a gas phase method such as sputtering. When a carbon-containing layer is used as the peeling layer 16, the thickness is preferably greater than 1 nm and less than 20 nm, and more preferably greater than 1 nm and less than 10 nm. By setting such a thickness, a peeling layer having the same roughness as the carrier can be formed. The thickness is a value measured by analyzing the layer cross section using an energy dispersive X-ray spectrometer (TEM-EDX) of a transmission electron microscope.

[0100] The peeling layer 16 includes a metal oxide layer and a carbon-containing layer, or may be a layer containing both metal oxide and carbon. In particular, when the metal foil 10 with a carrier includes an intermediate layer 14, the carbon-containing layer contributes to the stable peeling of the carrier 12, and the metal oxide layer can suppress the diffusion of the metal elements from the intermediate layer 14 and the metal layer 18 accompanied by heating, and as a result, even after heating at a high temperature of, for example, 350° C. or more, stable peeling properties can be maintained. The metal oxide layer is preferably a layer of an oxide of a metal composed of Cu, Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, In, Sn, Zn, Ga, Mo or a combination thereof. From the aspect that the film thickness can be easily controlled by adjusting the film forming time, it is particularly preferred that the metal oxide layer is a layer formed by a reactive sputtering method using a metal target and sputtering in an oxidizing atmosphere. The thickness of the metal oxide layer is preferably 0.1 nm or more and 100 nm or less. The upper limit of the thickness of the metal oxide layer is more preferably 60 nm or less, further preferably 30 nm or less, and particularly preferably 10 nm or less. The thickness is a value measured by analyzing the layer cross section using an energy dispersive X-ray spectrometer (TEM-EDX) of a transmission electron microscope. At this time, the order in which the metal oxide layer and the carbon layer are stacked as the peeling layer 16 is not particularly limited. In addition, the peeling layer 16 may exist in a mixed phase (i.e., a layer containing both metal oxide and carbon) in which the boundary between the metal oxide layer and the carbon-containing layer is not clearly defined.

[0101] Similarly, from the viewpoint of maintaining stable peeling properties even after heat treatment at high temperature, the peeling layer 16 may be a metal-containing layer whose surface adjacent to the metal layer 18 is a fluorinated surface and / or a nitrided surface. In the metal-containing layer, preferably, there is a region (hereinafter referred to as "(F+N) region") in which the sum of the fluorine content and the nitrogen content is 1.0 atomic % or more within a thickness of 10 nm or more, and the (F+N) region is preferably present on the metal layer 18 side of the metal-containing layer. The thickness (SiO2 conversion) of the (F+N) region is a value determined by performing elemental analysis in the depth direction of the metal foil 10 with a carrier using XPS. The fluorinated surface or the nitrided surface can preferably be formed by reactive ion etching (RIE: Reactive ion etching) or reactive sputtering. On the other hand, the metal element contained in the metal-containing layer preferably has a negative standard electrode potential. As preferred examples of metal elements contained in the metal-containing layer, Cu, Ag, Sn, Zn, Ti, Al, Nb, Zr, W, Ta, Mo and combinations thereof (e.g., alloys, intermetallic compounds) can be cited. The content of metal elements in the metal-containing layer is preferably 50 atomic % or more and 100 atomic % or less. The metal-containing layer can be a single layer consisting of one layer, or a multilayer consisting of two or more layers. The overall thickness of the metal-containing layer is preferably 10 nm or more and 1000 nm or less, more preferably 30 nm or more and 500 nm or less, further preferably 50 nm or more and 400 nm or less, and particularly preferably 100 nm or more and 300 nm or less. The thickness of the metal-containing layer itself is a value measured by analyzing the cross section of the layer using an energy dispersive X-ray spectrometer (TEM-EDX) of a transmission electron microscope.

[0102] Alternatively, the peeling layer 16 may also be a layer containing metal nitride instead of the carbon layer. The surface of the layer containing metal nitride on the opposite side of the carrier 12 (i.e., the metal layer 18 side) preferably contains at least one metal nitride selected from the group consisting of TaON, NiON, TiON, NiWON and MoON. In addition, from the perspective of ensuring the adhesion between the carrier 12 and the metal layer 18, the surface of the layer containing metal nitride on the carrier 12 side preferably contains at least one selected from the group consisting of Cu, Ti, Ta, Cr, Ni, Al, Mo, Zn, W, TiN and TaN. By doing so, the number of foreign particles on the surface of the metal layer 18 can be suppressed to improve the circuit formation, and even after long-term heating at high temperature, stable peeling strength can be maintained. The thickness of the layer containing metal nitride is preferably 5 nm or more and 500 nm or less, more preferably 10 nm or more and 400 nm or less, further preferably 20 nm or more and 200 nm or less, and particularly preferably 30 nm or more and 100 nm or less. This thickness is a value measured by analyzing a layer cross section using an energy dispersive X-ray spectrometer (TEM-EDX) of a transmission electron microscope.

[0103] A functional layer 17 may also be provided between the release layer 16 and the metal layer 18 as desired. The functional layer 17 is not particularly limited as long as it imparts the desired functions such as an etching stop function and an anti-reflection function to the metal foil 10 with a carrier. Preferred examples of metals constituting the functional layer 17 include Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, Mo, and combinations thereof, more preferably Ti, Zr, Al, Cr, W, Ni, Mo, and combinations thereof, further preferably Ti, Al, Cr, Ni, Mo, and combinations thereof, and particularly preferably Ti, Mo, and combinations thereof. These elements have the property of being insoluble in a flash etching solution (e.g., a copper flash etching solution), and as a result, they can exhibit excellent chemical resistance to the flash etching solution. Therefore, the functional layer 17 is a layer that is difficult to be etched by the flash etching solution compared to the metal layer 18, and therefore can function as an etching stop layer. In addition, the above-mentioned metal constituting the functional layer 17 also has the function of preventing the reflection of light, so the functional layer 17 can also function as an anti-reflection layer for improving the visibility in image detection (such as automatic image detection (AOI)). The functional layer 17 can be a pure metal or an alloy. The metal constituting the functional layer 17 may also contain inevitable impurities caused by raw material components, film forming processes, etc. In addition, the upper limit of the content of the above-mentioned metal is not particularly limited and can be 100 atomic%. The functional layer 17 is preferably a layer formed by physical vapor deposition (PVD) method, and more preferably a layer formed by sputtering. The thickness of the functional layer 17 is preferably 1 nm or more and 500 nm or less, more preferably 10 nm or more and 400 nm or less, further preferably 30 nm or more and 300 nm or less, and particularly preferably 50 nm or more and 200 nm or less.

[0104] The metal layer 18 is a layer composed of metal. Preferred examples of metals constituting the metal layer include Cu, Au, Pt and combinations thereof (e.g., alloys, intermetallic compounds), preferably Cu alloys or Cu. The metal constituting the metal layer 18 may also contain inevitable impurities caused by raw material components, film forming processes, etc. The metal layer 18 may be manufactured by any method, for example, it may also be a metal layer formed by wet film forming methods such as chemical metal plating and electrolytic metal plating, physical vapor deposition (PVD) methods such as sputtering and vacuum evaporation, chemical vapor film forming, or a combination thereof. From the perspective of being easy to cope with fine pitch based on ultra-thinning, it is particularly preferred to form a metal layer by physical vapor deposition (PVD) methods such as sputtering and vacuum evaporation, and it is most preferred to form a metal layer by sputtering. In addition, the metal layer 18 is preferably a metal layer without roughening, as long as it does not hinder the formation of wiring patterns during the manufacture of printed wiring boards, and it may also be a secondary roughening by pre-roughening, soft etching, cleaning, and oxidation-reduction treatment. From the perspective of coping with the above-mentioned fine pitch, the thickness of the metal layer 18 is 0.01 μm or more and 4.0 μm or less, preferably 0.02 μm or more and 3.0 μm or less, more preferably 0.05 μm or more and 2.5 μm or less, further preferably 0.10 μm or more and 2.0 μm or less, particularly preferably 0.20 μm or more and 1.5 μm or less, and most preferably 0.30 μm or more and 1.2 μm or less. The thickness is a value measured by analyzing the layer cross section using an energy dispersive X-ray spectrometer (TEM-EDX) of a transmission electron microscope. From the perspective of maintaining the in-plane uniformity of the film thickness and improving the productivity of the sheet and roll, the metal layer 18 with a thickness within this range is preferably manufactured using a sputtering method.

[0105] The outermost surface on the first surface 12a of the metal layer 18 preferably has a flat shape corresponding to the surface shape of the flat region F of the carrier 12, and a concave-convex shape corresponding to the surface shape of the concave-convex region R of the carrier 12. Figure 1As shown, a metal layer 18 is formed on a carrier 12 having a flat region F and a concave-convex region R via an intermediate layer 14 (if present), a peeling layer 16, and a functional layer 17 (if present), so that the surface profiles of the flat region F and the concave-convex region R of the carrier 12 are transferred to the surfaces of each layer. In this way, it is preferred that the outermost surface of the metal layer 18 is given a desired surface profile corresponding to the shape of each region of the carrier 12 while transferring the concave-convex shape to a part of the peeling layer 16. By doing so, it is possible to further prevent the metal layer 18 from peeling off when the metal foil 10 with the carrier is cut, and it is possible to further cope with fine pitch. Typically, the interface expansion area ratio Sdr of the surface (i.e., the flat surface) having a flat shape corresponding to the flat region F of the carrier 12 on the outermost surface of the metal layer 18 is less than 5%, preferably 0.01% or more and 4.0% or less, more preferably 0.03% or more and 3.0% or less, further preferably 0.05% or more and 1.0% or less, and particularly preferably 0.08% or more and 0.50% or less. In addition, the interface extension area ratio Sdr of the outermost surface of the metal layer 18, which has a concave-convex shape corresponding to the concave-convex region R of the carrier 12 (i.e., the concave-convex surface), is typically greater than 3% and less than 39%, preferably greater than 3.5% and less than 35%, more preferably greater than 4.0% and less than 30%, further preferably greater than 4.5% and less than 25%, and particularly preferably greater than 5% and less than 15%.

[0106] The metal layer 18 extends from the first surface 12a of the carrier to the side surface 12c in a manner covering at least a portion of the side surface 12c of the carrier. The side surface 12c of the carrier is preferably covered by the metal layer 18 in its entire area. In short, as described above, the concave-convex area R includes the area of ​​the side surface 12c covered by the metal layer 18. As desired, the functional layer 17, the peeling layer 16 and / or the intermediate layer 14 may also extend from the first surface 12a of the carrier to the side surface 12c. In the case where the peeling layer 16 extends to the side surface 12c, from the viewpoint of effectively preventing the chemical solution from penetrating from the end of the peeling layer 16, the metal layer 18 (and the functional layer 17 as desired) preferably extends to the side surface 12c in a manner covering the peeling layer 16. It should be noted that the thickness of each layer of the above-mentioned intermediate layer 14, peeling layer 16, functional layer 17 and metal layer 18 refers to the thickness of each layer provided on the first surface 12a. That is, the thickness of each layer provided on the side surface 12c may also be out of the above-mentioned thickness range. For example, the thickness of the metal layer 18 provided on the side surface portion 12c is allowed to deviate from the range of 0.01 μm to 4.0 μm. The thickness of the metal layer 18 on the side surface portion 12c is not particularly limited, but is typically 0.02 μm to 3 μm, more typically 0.04 μm to 2 μm, and further typically 0.05 μm to 0.8 μm.

[0107] The intermediate layer 14 (if present), the peeling layer 16, the functional layer 17 (if present) and the metal layer 18 are preferably physical vapor deposition (PVD) films, i.e. films formed using the physical vapor deposition (PVD) method, and more preferably sputtered films, i.e. films formed using the sputtering method.

[0108] The overall thickness of the metal foil 10 with a carrier is not particularly limited, and is preferably 500 μm or more and 3000 μm or less, more preferably 700 μm or more and 2500 μm or less, further preferably 900 μm or more and 2000 μm or less, and particularly preferably 1000 μm or more and 1700 μm or less. The size of the metal foil 10 with a carrier is not particularly limited, and is preferably 10 cm square or more, more preferably 20 cm square or more, and further preferably 25 cm square or more. The upper limit of the size of the metal foil 10 with a carrier is not particularly limited, and one standard with 1000 cm square as the upper limit can be cited. In addition, the metal foil 10 with a carrier is in a form that can be handled separately before and after the wiring is formed.

[0109] As desired, the metal foil 10 with a carrier may further include a redistribution layer 20 on the metal layer 18. In this specification, the redistribution layer refers to a layer including an insulating layer and a wiring layer formed inside and / or on the surface of the insulating layer. In a top view of the metal foil 10 with a carrier, it is preferred that at least a portion of the redistribution layer 20 reaches the end of the carrier 12 (the boundary between the first surface 12a and the side surface 12c), and it is further preferred that the entire peripheral area of ​​the redistribution layer 20 reaches the end of the carrier 12. In addition, as Figure 1 As shown, it is preferred that at least a portion of the end portion (typically the insulating layer) of the redistribution layer 20 is located on the concave-convex region R, and it is further preferred that the entire peripheral portion of the redistribution layer 20 is located on the concave-convex region R. By doing so, the adhesion between the metal layer 18 and the redistribution layer 20 can be improved. As a result, in the process of using a chemical solution during and after the formation of the redistribution layer 20, it is possible to suppress the infiltration of the chemical solution between the metal layer 18 and the redistribution layer 20, and it is also possible to effectively prevent the unwanted peeling between the two layers. Figure 1 As shown, in the case of a cross-section of the metal foil 10 with a carrier, the length of overlap between the peripheral portion of the redistribution layer 20 and the concave-convex area R (the width of the redistribution layer 20 located on the concave-convex area R) is preferably greater than 0.1 mm and less than 50 mm, more preferably greater than 0.2 mm and less than 45 mm, further preferably greater than 0.3 mm and less than 40 mm, still more preferably greater than 1.0 mm and less than 40 mm, particularly preferably greater than 1.5 mm and less than 40 mm, particularly preferably greater than 2.0 mm and less than 40 mm, and most preferably greater than 2.5 mm and less than 35 mm.

[0110] The metal foil 10 with a carrier may be a structure in which the above-mentioned various layers are sequentially provided on both sides of the carrier 12 in a vertically symmetrical manner. That is, the metal foil 10 with a carrier may further include: a second peeling layer provided on the second surface 12b of the carrier, and a second metal layer having a thickness of 0.01 μm or more and 4.0 μm or less provided on the second peeling layer. In this case, it is preferred that the second metal layer extends from the second surface 12b of the carrier to the side surface 12c in a manner such that at least a portion of the side surface 12c of the carrier is covered by the second metal layer. In addition, the carrier 12 preferably further has the above-mentioned concave-convex region R on the second surface 12b, and the concave-convex region R includes the area of ​​the side surface 12c covered by the second metal layer. In addition, the metal foil 10 with a carrier may further have an additional intermediate layer between the second surface 12b of the carrier and the second peeling layer, and may further have a second functional layer between the second peeling layer and the second metal layer. The metal foil 10 with a carrier may further have a second redistribution layer on the second metal layer. The preferred method for the first surface 12a, intermediate layer 14, peeling layer 16, functional layer 17, metal layer 18 and redistribution layer 20 of the carrier described above is also directly applicable to the second surface 12b, additional intermediate layer, second peeling layer, second functional layer, second metal layer and each layer of the second redistribution layer of the carrier. The formation of various layers arranged on the second surface 12b of the carrier can be carried out by continuous film formation from the first surface 12a to the second surface 12b of the carrier. That is, the intermediate layer 14 and the additional intermediate layer, the peeling layer 16 and the second peeling layer, the functional layer 17 and the second functional layer, and / or the metal layer 18 and the second metal layer can also be connected to each other through the side surface 12c of the carrier.

[0111] Method for producing metal foil with carrier

[0112] The metal foil 10 with a carrier of the present invention can be manufactured by: (1) preparing a carrier, (2) roughening at least the side surface of the carrier, (3) forming various layers such as a peeling layer and a metal layer on the carrier, and (4) forming a redistribution layer on the metal layer as desired, thereby enabling manufacturing.

[0113] (1) Preparation of vector

[0114] First, prepare a carrier 12. The carrier 12 preferably has a flat surface with an Sdr of less than 5% on at least one surface. The Sdr is preferably 0.01% or more and 4.0% or less, more preferably 0.03% or more and 3.0% or less, further preferably 0.05% or more and 1.0% or less, particularly preferably 0.07% or more and 0.50% or less, and most preferably 0.08% or more and 0.50% or less. Generally, substrates of SiO2, SiN, Si single crystal, Si polycrystalline, and plate-shaped glass products have excellent flatness, so commercially available SiO2 substrates, SiN substrates, Si single crystal substrates, Si polycrystalline substrates, glass sheets, glass films, and glass plates having a flat surface that satisfies the above-mentioned range of Sdr can also be used as carriers 12. Alternatively, by grinding the surface of the carrier 12 that does not satisfy the above-mentioned Sdr using a known method, the Sdr within the above-mentioned range can also be imparted. The preferred materials and characteristics of the carrier 12 are as described above.

[0115] (2) Roughening of the carrier surface

[0116] Next, at least the side portion 12c of the carrier is roughened to form a concave-convex region R with an Sdr of 3% to 39%. The Sdr is preferably 3.5% to 35%, more preferably 4.0% to 30%, further preferably 4.5% to 25%, and particularly preferably 5% to 15%. In addition, in addition to the roughening of the side portion 12c, it is preferred that a specified area of ​​the first surface 12a of the carrier be roughened in such a manner that the concave-convex region R surrounds the flat surface on the first surface 12a of the carrier. The roughening treatment can be carried out according to a known method, and there is no particular limitation as long as the Sdr within the above range can be achieved and the concave-convex region R can be formed in a desired pattern (with masking as needed). From the perspective of being able to efficiently form the concave-convex region R of the desired Sdr, the preferred method of roughening treatment is sandblasting or etching, and sandblasting is more preferred.

[0117] The roughening treatment based on sandblasting can be performed by projecting a granular medium M (projection material) from a nozzle to a specified area (i.e., an area where a concave-convex area R should be formed) of the side portion 12c and / or the first surface 12a of the carrier. For the preferred size of the nozzle, when the ejection port is rectangular, the width is 0.1 mm or more and 20 mm or less and the length is 100 mm or more and 1000 mm or less, more preferably the width is 3 mm or more and 15 mm or less and the length is 200 mm or more and 800 mm or less. On the other hand, when the ejection port is circular, the preferred size of the nozzle is 0.2 mm or more and 50 mm or less in diameter, more preferably 3 mm or more and 20 mm or less in diameter. The particle size of the medium is preferably 7 μm or more and 50 μm or less in diameter, more preferably 8 μm or more and 35 μm or less. As preferred examples of the material of the medium, aluminum oxide, zirconium oxide, silicon carbide, iron, aluminum, zinc, glass, steel and boron carbide can be cited. The Mohs hardness of the medium is preferably 4 or more, more preferably 5.5 or more, and further preferably 6.0 or more. In particular, by using such a medium, it is possible to form a desired concave-convex region R in which the Sdr is controlled within the above range on the surface of the carrier 12. The preferred medium ejection pressure is 0.01 MPa to 0.80 MPa, more preferably 0.1 MPa to 0.50 MPa, and even more preferably 0.15 MPa to 0.25 MPa. In addition, the sandblasting time per unit area of ​​the carrier 12 is preferably 0.03 sec / cm 2 Above and 10 seconds / cm 2 Below, more preferably 0.1 sec / cm 2 Above and 5 seconds / cm 2 In particular, from the perspective of easily forming the concavo-convex region R in which the Sdr is controlled within the above range on the surface of the carrier 12, it is preferred to mix the medium with water to form a slurry and spray the slurry from a nozzle by pressurized air for sandblasting. In addition, by performing the roughening treatment (sandblasting treatment) under the above conditions, it is possible to more effectively suppress the reduction in strength of the carrier after the roughening treatment.

[0118] On the other hand, preferred examples of roughening treatment by etching include a wet process using a solution containing hydrofluoric acid and a dry process based on reactive ion etching (RIE) using a process gas containing fluorine (eg, CF4, SF6, etc.).

[0119] In order to selectively roughen the desired area (especially sandblasting or etching), it is preferred to use masking. Specifically, it is preferred that a masking layer is formed on the side surface portion 12c and / or the first surface 12a of the carrier other than the specified area (i.e., the area where the concavo-convex area R is to be formed) before the roughening treatment. In this case, in order to make the formation of various layers as a post-process proceed more smoothly, it is desirable to remove the masking layer after the roughening treatment.

[0120] (3) Formation of various layers on the carrier

[0121] On the first surface 12a of the carrier subjected to the roughening treatment, a desired intermediate layer 14, a peeling layer 16, a desired functional layer 17, and a metal layer 18 having a thickness of 0.01 μm or more and 4.0 μm or less are formed. From the perspective of being easy to cope with the fine pitch based on ultra-thinning, the formation of each layer of the intermediate layer 14 (if present), the peeling layer 16, the functional layer 17 (if present), and the metal layer 18 is preferably performed by a physical vapor deposition (PVD) method. As examples of the physical vapor deposition (PVD) method, sputtering, vacuum evaporation, and ion plating can be cited. From the perspective of being able to control the film thickness in a wide range of 0.05 nm or more and 5000 nm or less, and being able to ensure the uniformity of the film thickness in a wide range or area, the sputtering method is most preferred. In particular, by forming all the layers of the intermediate layer 14 (if present), the peeling layer 16, the functional layer 17 (if present), and the metal layer 18 by sputtering, the manufacturing efficiency is significantly improved. The film formation based on the physical vapor deposition (PVD) method uses a known gas phase film forming device and is carried out according to known conditions without any particular limitation. For example, it can be carried out by directly adopting the film forming conditions of various layers based on the physical vapor deposition (PVD) method disclosed in patent document 7 (International Publication No. 2019 / 163605), or by making appropriate changes. In the case of sputtering, the sputtering method can be various known methods such as magnetron sputtering, dipole sputtering, and target sputtering, but magnetron sputtering is preferred from the perspective of fast film forming speed and high productivity. Sputtering can be carried out with any power supply of DC (direct current) and RF (high frequency). In addition, the target shape can also use a well-known plate target, but from the perspective of target use efficiency, it is desirable to use a cylindrical target.

[0122] (4) Formation of redistribution layer (optional process)

[0123] A redistribution layer 20 may be formed on the metal layer 18 of the metal foil 10 with a carrier as desired. The redistribution layer 20 may be formed by a known method without particular limitation. For example, the redistribution layer 20 may be preferably formed by alternately stacking insulating layers and wiring layers using a coreless deposition method to form a multilayer.

[0124] After forming the redistribution layer 20, the metal foil 10 with a carrier can also be mounted based on a chip and sealed with a molding resin. Chip mounting and resin sealing can be performed using a known method without particular limitation. In addition, the carrier 12 (and the intermediate layer 14 if present) can be peeled off after resin sealing, and the exposed metal layer 18 (and the functional layer 17 if present) can also be removed by etching after peeling. The peeling of the carrier 12 can also be performed in the following manner. First, an incision is made in the thickness direction from the surface opposite to the carrier 12 of the metal foil 10 with a carrier (typically the molding resin side), and various layers other than the carrier 12 are divided into a central portion (the portion containing the chip) and a peripheral portion. Thereafter, while the central portion is fixed, a pressing member is used to press down the peripheral portion, and the central portion containing the metal layer 18 and the redistribution layer 20 is peeled off from the carrier 12. By doing so, the carrier 12 can be easily peeled off.

[0125] Example

[0126] The present invention is further specifically described through the following examples.

[0127] Example A1~A11

[0128] like Figure 1 As shown, a glass or single crystal silicon carrier is prepared as the carrier 12. After forming the concavo-convex region R on the carrier, the first intermediate layer 14a, the second intermediate layer 14b, the peeling layer 16, the functional layer 17, and the metal layer 18 are sequentially formed to produce the metal foil with carrier 10. The specific steps are as follows.

[0129] It should be noted that the Sdr mentioned in the following examples is a value measured by a laser microscope (OLYMPUS CORPORATION, LEXT OLS5000) in accordance with ISO25178. Specifically, the surface profile of the 258.346μm×258.348μm area of ​​the surface of the measured object is measured on the above-mentioned laser microscope using a 50x objective lens. For the obtained surface profile, Sdr is calculated by surface property analysis using an analytical software (OLYMPUS CORPORATION, LEXT OLS5100 analytical application). At this time, the cutoff wavelength based on the S filter is set to 0.8μm, and no cutoff based on the L filter is performed.

[0130] (1) Preparation of vector

[0131] A disc-shaped carrier 12 having a first surface 12a and a second surface 12b facing each other and a curved side surface 12c connecting them, and having a diameter of 300 mm and a thickness of 1.1 mm was prepared. The type of the carrier 12 was a glass carrier (soda-lime glass, manufactured by Central Glass Co., Ltd., Sdr in the first surface 12a: 0.10%) for Examples A1 to A4 and A9 to A11, and a single crystal silicon carrier (manufactured by Trinity Inc., Sdr in the first surface 12a: 0.10%) for Examples A5 to A8.

[0132] (2) Roughening of the carrier

[0133] A masking layer is formed on the first surface 12a of the carrier in a manner that covers the portion other than the periphery (width 1 mm) of the first surface 12a. The masking layer is formed by cutting a cutting sheet (PVC100M M11K manufactured by LINTEC Corporation) into a diameter of 298 mm using a cutting plotter, and stacking the cut cutting sheet on the first surface 12a of the carrier in a manner that the center of the cutting sheet and the carrier overlap. Next, a sandblasting device (manufactured by Fuji Seisakusho Co., Ltd., model: SCM-4RBT-05-401) is used to project a medium (manufactured by Fuji Seisakusho Co., Ltd., white molten alumina) having an average particle size D50 shown in Table 1 under a spray pressure of 0.4 MPa for each of Examples A1 to A10, thereby roughening the carrier 12. At this time, the sandblasting time per unit area of ​​the carrier 12 is 0.33 seconds / cm 2 . In addition, the roughening treatment of the side surface portion 12c is performed in the range of 0.6 mm in the thickness direction from the first surface 12a to the second surface 12b and on the entire circumference of the side surface portion 12c. In this way, the concave-convex region R is continuously formed from the side surface portion 12c of the carrier to the periphery of the first surface 12a. Thereafter, the masking layer is removed to expose the flat region F. The Sdr of the concave-convex region R in the carrier 12 after the roughening treatment is shown in Table 1. It should be noted that for Example A11, the roughening treatment of the carrier 12 was not performed.

[0134] (3) Formation of the first intermediate layer

[0135] On the first surface 12 a and the side surface portion 12 c of the carrier, a Ti layer having a thickness of 100 nm was formed as the first intermediate layer 14 a by sputtering using the following apparatus and conditions.

[0136] - Equipment: Single-wafer magnetron sputtering equipment (manufactured by Canon Tokki Corporation, MLS464)

[0137] - Target: 8-inch (203.2 mm) diameter Ti target (99.999% purity)

[0138] -Ultimate vacuum degree: less than 1×10 -4 Pa

[0139] -Carrier gas: Ar (flow rate: 100 sccm)

[0140] -Sputtering pressure: 0.35Pa

[0141] -Sputtering power: 1000W (3.1W / cm 2 )

[0142] -Film forming temperature: 40℃

[0143] (4) Formation of the second intermediate layer

[0144] On the first intermediate layer 14a, a Cu layer having a thickness of 100 nm was formed as the second intermediate layer 14b by sputtering under the following apparatus and conditions.

[0145] - Equipment: Single wafer DC sputtering equipment (manufactured by Canon Tokki Corporation, MLS464)

[0146] - Target: 8-inch (203.2 mm) diameter Cu target (99.98% purity)

[0147] -Ultimate vacuum degree: less than 1×10 -4 Pa

[0148] -Carrier gas: Ar (flow rate: 100 sccm)

[0149] -Sputtering pressure: 0.35Pa

[0150] -Sputtering power: 1000W (6.2W / cm 2 )

[0151] -Film forming temperature: 40℃

[0152] (5) Formation of peeling layer

[0153] On the second intermediate layer 14 b , an amorphous carbon layer having a thickness of 6 nm was formed as the peeling layer 16 by sputtering under the following apparatus and conditions.

[0154] - Equipment: Single wafer DC sputtering equipment (manufactured by Canon Tokki Corporation, MLS464)

[0155] - Target: 8-inch (203.2 mm) diameter carbon target (99.999% purity)

[0156] -Ultimate vacuum degree: less than 1×10 -4 Pa

[0157] -Carrier gas: Ar (flow rate: 100 sccm)

[0158] -Sputtering pressure: 0.35Pa

[0159] -Sputtering power: 250W (0.7W / cm 2 )

[0160] -Film forming temperature: 40℃

[0161] (6) Formation of functional layer

[0162] On the surface of the release layer 16 , a Ti layer having a thickness of 100 nm was formed as the functional layer 17 by sputtering in the following apparatus and conditions.

[0163] - Equipment: Single wafer DC sputtering equipment (manufactured by Canon Tokki Corporation, MLS464)

[0164] - Target: 8-inch (203.2 mm) diameter Ti target (99.999% purity)

[0165] -Carrier gas: Ar (flow rate: 100 sccm)

[0166] -Ultimate vacuum degree: less than 1×10 -4 Pa

[0167] -Sputtering pressure: 0.35Pa

[0168] -Sputtering power: 1000W (3.1W / cm 2 )

[0169] (7) Formation of Metal Layer

[0170] On the functional layer 17, a Cu layer having a thickness of 300 nm was formed as the metal layer 18 by sputtering under the following apparatus and conditions to obtain the metal foil with carrier 10. At this time, the metal layer 18 was formed so as to cover the side surface portion 12c of the carrier and the release layer 16.

[0171] - Equipment: Single wafer DC sputtering equipment (manufactured by Canon Tokki Corporation, MLS464)

[0172] - Target: 8-inch (203.2 mm) diameter Cu target (99.98% purity)

[0173] -Ultimate vacuum degree: less than 1×10 -4 Pa

[0174] -Carrier gas: Ar (flow rate: 100 sccm)

[0175] -Sputtering pressure: 0.35Pa

[0176] -Sputtering power: 1000W (3.1W / cm 2 )

[0177] -Film forming temperature: 40℃

[0178] (8) Determination of peel strength of concave-convex area

[0179] A metal foil with a carrier in which the entire area of ​​the first surface 12a is a concave-convex area is produced in the same manner as in the above (1) to (7), except that a masking layer is not formed and the side portion 12c is not roughened. A measurement sample is obtained by laminating 18 μm of Cu on the metal layer side of the metal foil with a carrier by electrolytic plating. For the measurement sample, the peel strength (gf / cm) when peeling off the electrolytically plated Cu layer is measured under the conditions of a measurement width of 10 mm, a measurement length of 17 mm, and a peeling speed of 50 mm / min in accordance with JISZ 0237-2009. The peel strength of the concave-convex area measured in this way is shown in Table 1.

[0180] Various evaluations

[0181] The metal foils 10 with a carrier obtained in Examples A1 to A11 were subjected to various evaluations described below.

[0182] <Difference in height of the height difference section>

[0183] Using a laser microscope (OLYMPUS CORPORATION, LEXT OLS5100), the area of ​​258.346 μm in length and 258.348 μm in width on the first surface 12a of the metal foil 10 with a carrier is measured in a manner that the boundary of the concave-convex area R and the flat area F is parallel to the longitudinal direction and consistent with the center of the transverse direction. At this time, the magnification of the objective lens is 50 times. In this way, the cross-sectional profile near the boundary of the concave-convex area R and the flat area F is obtained. The cross-sectional profile is analyzed by using analysis software (OLYMPUS CORPORATION, LEXT OLS5100 analysis application) to calculate the lateral height profile (the height of 0 μm to 258.346 μm in length is averaged). In this lateral height profile, the difference between the average value of the height of the concave-convex area R part and the average value of the height of the flat area F part is measured as the height difference of the height difference part. The results are shown in Table 1.

[0184] <Stripping during the redistribution layer formation process>

[0185] The presence or absence of peeling and the immersion width of the chemical solution in the redistribution layer formation process were confirmed. Specifically, first, an insulating resin material (photosensitive insulating material) was laminated on the surface of the metal layer 18 side of the metal foil 10 with a carrier, and a heat curing treatment was performed at 230°C for 60 minutes, thereby forming an insulating layer with a thickness of 10μm. Next, a Ti layer and a Cu layer were sputtered in sequence on the surface of the insulating layer side of the metal foil 10 with a carrier. A photosensitive liquid resist was applied to the surface of the Cu layer, exposed and developed, and a photoresist layer of a predetermined pattern was formed. At this time, TMAH (tetramethylammonium hydroxide, manufactured by Tokyo Ohka Industry Co., Ltd., NMD-3 2.38%) was used as a developer and applied to the surface of the metal foil 10 with a carrier by a spin coater. Thereafter, the exposed surface of the Cu layer (i.e., the portion not masked by the photoresist layer) was subjected to pattern electrolytic copper plating, and after the electrolytic copper plating layer was formed, the photoresist layer was peeled off. At this time, ST-120 (manufactured by Tokyo Ohka Industry Co., Ltd.) is used as a stripping solution to immerse the metal foil 10 with a carrier and strip the resist. Afterwards, the exposed copper layer and the unnecessary parts of the Ti layer are removed using a sulfuric acid-hydrogen peroxide etching solution and a hydrogen peroxide alkaline etching solution (Meltex Inc., Melstrip TI-3991), respectively, to form a wiring layer with a circuit thickness of 5 μm on the Cu layer. Afterwards, the insulating resin material is laminated and heat-cured at 230°C for 60 minutes to form an insulating layer with a thickness of 10 μm. Next, the Ti layer and the Cu layer are sputtered in sequence on the surface of the insulating layer side of the metal foil 10 with a carrier. In this way, a redistribution layer 20 is formed. In the formation process of the redistribution layer 20, it is confirmed whether natural peeling occurs between the carrier 12 and the metal layer 18. In addition, the cross-section of the redistribution layer 20 is observed with an optical microscope, thereby measuring the immersion width of the chemical solution used in the process, and evaluating according to the following criteria. The results are shown in Table 1.

[0186] (Evaluation criteria for chemical solution immersion width)

[0187] -Evaluation A: Chemical solution immersion width less than 0.1mm (best)

[0188] -Evaluation B: Chemical solution immersion width is 0.1 mm or more and less than 0.5 mm (good)

[0189] -Evaluation C: Chemical solution immersion width is 0.5 mm or more (not good)

[0190] -Evaluation F: Unable to measure due to peeling during the process

[0191] [Table 1]

[0192] Table 1

[0193]

[0194] *Indicates comparative example.

[0195] Examples B1 to B6

[0196] This example is an experimental example for verifying the relationship between the interface expansion area ratio Sdr and the mechanical strength when the carrier 12 is made of glass.

[0197] (1) Preparation of vector

[0198] A glass sheet (material: soda-lime glass, manufactured by Nippon Sheet Glass Co., Ltd.) having a size of 300 mm square and a thickness of 1.1 mm and having a flat surface with an interface expansion area ratio Sdr of 0.10% was prepared.

[0199] (2) Roughening of the carrier

[0200] A masking layer is formed on the surface of the carrier 12 in a manner that covers the portion other than the periphery (width 11 mm) of the carrier 12. The masking layer is formed by cutting a cutting sheet (PVC100MM11K manufactured by LINTEC Corporation) into 278 mm squares using a cutting plotter, and stacking the cut cutting sheet on the surface of the carrier 12 in a manner that the cutting sheet overlaps the center of the carrier. Next, a sandblasting device (manufactured by Fuji Seisakusho Co., Ltd., model: SCM-4RBT-05-401) is used to roughen the exposed portion of the carrier 12 by projecting a medium (manufactured by Fuji Seisakusho Co., Ltd., white molten alumina) with an average particle size D50 shown in Table 2 at a spray pressure shown in Table 2 in each of Examples B1 to B6. In this way, a concave-convex region R is formed around the carrier 12 (width 11 mm). Thereafter, the masking layer is removed to expose the flat region F. In this way, a concave-convex region R is formed on the surface of the carrier 12. Thereafter, the masking layer is removed to expose the flat region F. Table 2 shows the Sdr of the concave-convex region R in the carrier 12 after the roughening process.

[0201] Example B7 (Compare)

[0202] When the glass carrier was not subjected to the roughening treatment, the same glass sheet as that prepared in Examples B1 to B6 was used as the carrier 12 as it was.

[0203] evaluate

[0204] For the carriers 12 of Examples B1 to B7, the breaking load was measured using a universal material tester (manufactured by Instron, model: 5985). Fig. 8A and 8BAs shown in FIG. 1 , the carrier 12 is placed on a support member S (made of carbon steel S45C for mechanical structure, quenching hardness: 50HRC, curvature radius of the contact portion: 5mm) at 8 points arranged at equal intervals on an imaginary circle of 280mm in diameter. Then, a pressing member P (made of high carbon chromium bearing steel SUJ2, quenching hardness: 67HRC, curvature radius of the contact portion: 15mm) is moved along the Fig. 8A Move in the direction of the arrow in the figure, press the center part of the carrier 12, and thus destroy the carrier 12. For each example, the measurement is performed on 10 carriers 12. Based on the obtained measurement data, a Wyble diagram is prepared (X-axis: breaking load (N), Y-axis: cumulative breaking probability (%)), and the average breaking load, 10% breaking load (B10) and shape parameters are calculated. The results are shown in Table 2. It should be noted that Table 2 also shows the percentage of the breaking load of the roughened glass carrier (Example B1 to B6) relative to the breaking load of the untreated glass carrier (Example B7).

[0205] [Table 2]

[0206]

Claims

1. A metal foil with a carrier, comprising: A carrier having a first surface and a second surface opposite to each other, and a side surface portion connected to the first surface and the second surface; a peeling layer disposed on the first surface of the carrier; as well as a metal layer disposed on the release layer and having a thickness of 0.01 μm or more and 4.0 μm or less, The metal layer extends from the first surface of the carrier to the side surface in a manner that at least a portion of the side surface is covered by the metal layer. The carrier has a concavo-convex region having an interface extension area ratio Sdr of 3% or more and 39% or less measured in accordance with ISO 25178 on the side surface or on the side surface and the first surface, and the concavo-convex region includes a region of the side surface covered by the metal layer.

2. The metal foil with a carrier according to claim 1, wherein The concavo-convex area is provided on the entire circumference of the side surface portion.

3. The metal foil with a carrier according to claim 1 or 2, wherein The carrier has, on the first surface, a flat region having an interface extension area ratio Sdr of less than 5% as measured in accordance with ISO 25178, and the concavo-convex region surrounding the flat region. The concavo-convex region is provided continuously from the side surface portion of the carrier to the first surface.

4. The metal foil with a carrier according to claim 3, wherein On the first surface of the carrier, a ratio of an area of ​​the concavo-convex region to a total area of ​​the flat region and the concavo-convex region is 0.01 or more and 0.5 or less.

5. The metal foil with a carrier according to claim 3, wherein The concavo-convex region is provided on the first surface in a pattern that divides the flat region into two or more regions.

6. The metal foil with a carrier according to claim 1 or 2, wherein: The metal foil with a carrier has a height difference portion in the uneven region that is lower than a flat surface of the metal layer in the flat region, and a height difference between the height difference portion and the flat surface is greater than 0.05 μm and less than 100 μm.

7. The metal foil with a carrier according to claim 1 or 2, wherein: The carrier has a micro Vickers hardness of 500 HV or more and 3000 HV or less.

8. The metal foil with a carrier according to claim 1 or 2, wherein The metal layer is composed of at least one metal selected from the group consisting of Cu, Au, and Pt.

9. The metal foil with a carrier according to claim 1 or 2, wherein: An intermediate layer containing at least one metal selected from the group consisting of Cu, Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, In, Sn, Zn, Ga and Mo is further provided between the carrier and the peeling layer.

10. The metal foil with a carrier according to claim 1 or 2, wherein A functional layer composed of at least one metal selected from the group consisting of Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni and Mo is further provided between the release layer and the metal layer.

11. The metal foil with a carrier according to claim 1 or 2, wherein The carrier is a glass substrate or a silicon substrate containing SiO2.

12. The metal foil with a carrier according to claim 11, wherein The carrier is the glass substrate, and the glass substrate is composed of at least one selected from the group consisting of quartz glass, borosilicate glass, alkali-free glass, soda-lime glass, and aluminosilicate glass.

13. The metal foil with a carrier according to claim 1 or 2, wherein: The peel strength of the carrier in the concavo-convex region is 20 gf / cm or more and 3000 gf / cm or less.

14. The metal foil with a carrier according to claim 1 or 2, wherein: The metal foil with carrier has a redistribution layer on the metal layer, When the metal foil with a carrier is viewed from above, at least a portion of the redistribution layer reaches an end portion of the carrier.

15. The metal foil with a carrier according to claim 14, wherein At least a portion of an end portion of the redistribution layer is located on the concave-convex region.

16. The metal foil with a carrier according to claim 5, wherein: The line width of the pattern of the concavo-convex region R provided on the first surface is greater than or equal to 0.1 mm and less than or equal to 50 mm.

17. The metal foil with a carrier according to claim 1 or 2, wherein: The metal foil with carrier further comprises: a second peeling layer disposed on the second surface of the carrier; and a second metal layer provided on the second release layer and having a thickness of 0.01 μm or more and 4.0 μm or less, The second metal layer extends from the second surface of the carrier to the side surface such that at least a portion of the side surface is covered by the second metal layer. The carrier further has the uneven region on the second surface, and the uneven region includes a region of the side surface portion covered by the second metal layer.

Citation Information

Patent Citations

  • Copper foil with glass carrier and production method therefor

    CN111511543A

  • Copper foil for printed circuit board production, copper foil with carrier, and copper-clad laminate plate, and printed circuit board production method using copper foil for printed circuit board production, copper foil with carrier, and copper-clad laminate plate

    WO2017141985A1