Method for producing fluorine-containing copolymer

By using polymerization solvent A and water that is not soluble in water in the polymerization medium for suspension polymerization, the ratio and solubility of water and monomer are controlled, the problem of slow polymerization speed is solved, and a faster preparation of fluorine-containing copolymers is achieved.

CN118946609APending Publication Date: 2024-11-12AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030929.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing fluorine-containing copolymer manufacturing methods have slow polymerization speed and lack efficient preparation methods.

Method used

In a polymerization medium containing polymerization solvent A and water, monomers of ethylene and tetrafluoroethylene are used for suspension polymerization. The polymerization solvent A is a compound that is not soluble in water, and the proportion of water to volume is 10% to 80%, and the content of the water is 10% to 80%. During the polymerization process, the mass of polymerization solvent A and the solubility of monomers are controlled to achieve rapid polymerization.

Benefits of technology

The polymerization rate of fluorine-containing copolymers is significantly improved, and high-quality copolymers are produced faster than traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946609A_ABST
    Figure CN118946609A_ABST
Patent Text Reader

Abstract

A method for producing a fluorine-containing copolymer in which a monomer containing ethylene and tetrafluoroethylene is subjected to suspension polymerization in a polymerization medium containing water and at least one type of polymerization solvent (A) that is water-insoluble and is selected from compounds represented by formulae 1 to 3, the proportion of water in the polymerization medium being 10-80 vol%, and the proportion of water in the polymerization medium being 10-80 vol%. The solubility of the polymerization solvent A with respect to the water at 25 DEG C is 500 g / L or less, and the solubility of the water with respect to the polymerization solvent A at 25 DEG C is 500 g / L or less. The explanations in formulae 1 to 3 are omitted. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a fluorine-containing copolymer. Background Art

[0002] In recent years, fluorine-based polymers have been used in various applications by utilizing their excellent properties, such as heat resistance, solvent resistance, and chemical resistance.

[0003] As a method for producing a fluorine-based polymer, polymerization methods such as a solution polymerization method, a suspension polymerization method, and an emulsion polymerization method are known.

[0004] For example, Patent Document 1 describes a production method characterized in that a fluorinated surfactant is added as a dispersion stabilizer when producing a fluorinated copolymer by suspension polymerization using a polymerization medium containing a solvent and water, wherein the solvent is selected from perfluorocarbons, hydrofluorocarbons, and heteroatom-containing perfluorocarbons. Prior art literature Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 8-333408 Summary of the invention Technical problem to be solved by the invention

[0006] However, the production method described in Patent Document 1 has a slow polymerization rate, and a method for producing a fluorinated copolymer more efficiently has been desired.

[0007] According to an embodiment of the present invention, there is provided a method for producing a fluorine-containing copolymer having a polymerization rate faster than conventional methods. Solutions to technical problems

[0008] The present invention includes the following aspects. <1> A method for producing a fluorine-containing copolymer comprises carrying out suspension polymerization with monomers containing ethylene and tetrafluoroethylene in a polymerization medium containing a polymerization solvent A and water, wherein the polymerization solvent A is at least one selected from the compounds represented by formulas 1 to 3 and is immiscible with water, and the proportion of water in the polymerization medium is 10% to 80% by volume.

Chemistry 1

Chemistry 2

Chemistry 3

Chemistry 4

[0009] According to the present invention, there is provided a method for producing a fluorine-containing copolymer having a polymerization rate faster than conventional methods. DETAILED DESCRIPTION

[0010] In the present disclosure, a numerical range expressed by “to” includes a range in which the numerical values ​​described before and after “to” are the minimum value and the maximum value, respectively. In the numerical ranges recorded in the present disclosure, the upper limit or lower limit recorded in one numerical range may also be replaced by the upper limit or lower limit of the numerical range recorded in other classifications. In addition, in the numerical ranges recorded in the present disclosure, the upper limit or lower limit of the numerical range may also be replaced by the value shown in the embodiments. In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment. In the present disclosure, when there are plural substances corresponding to each component, the amount of each component refers to the total amount of the plural substances unless otherwise specified.

[0011] [Method for producing fluorinated copolymer] The method for producing the fluorinated copolymer disclosed herein is a method of performing suspension polymerization using monomers containing ethylene and tetrafluoroethylene in a polymerization medium containing a polymerization solvent A and water, wherein the polymerization solvent A is at least one selected from the compounds represented by Formulae 1 to 3 and is immiscible with water.

[0012]

Chemistry 5

[0013]

Chemistry 6

[0014]

Chemistry 7

[0016] In Formula 1 and Formula 2, "tBu" represents a tert-butyl group.

[0017]

Chemistry 8

[0018] In formulas T1 to T6, A 1 Each independently represents a hydrogen atom, a methyl group, a tert-butyl group, -OR or -NR2, A 2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, each R independently represents a methyl group or a tert-butyl group, and * represents a bonding site.

[0019] The method for producing a fluorinated copolymer disclosed in the present invention can produce a fluorinated copolymer by polymerization at a faster polymerization rate than conventional methods. The present inventors speculate the reasons for this effect as follows.

[0020] In the method for producing the fluorinated copolymer disclosed herein, polymerization is carried out in a polymerization medium comprising a polymerization solvent A which is immiscible with water and at least one compound selected from the group consisting of the compounds represented by Formulae 1 to 3 and water. The chain transfer property of the polymerization solvent A is low. Therefore, it is presumed that the polymerization of the monomers including ethylene and tetrafluoroethylene proceeds smoothly.

[0021] Hereinafter, the method for producing the fluorinated copolymer and the fluorinated copolymer of the present disclosure will be described in detail.

[0022] (Polymerization medium) The polymerization medium contains at least one polymerization solvent A selected from the group consisting of compounds represented by Formulae 1 to 3.

[0023] <Compound represented by Formula 1>

Chemistry 9

[0024] In formula 1, Y 1 represents a nitrogen atom or an oxygen atom. Y 1 When it is a nitrogen atom, p, m, n and k are each independently an integer satisfying p+m is greater than or equal to 1 and p+m+n+k=3. Y 1 When it is an oxygen atom, k is 0, and p, m, n and k are each independently an integer satisfying p+m is greater than or equal to 1 and p+m+n=2. When p is 1 or more, n is 1 or more. Z 1 Each independently represents a group represented by any one of formulae T1 to T6.

[0025] In formulas T1 to T6, A 1 Each independently represents a hydrogen atom, a methyl group, a tert-butyl group, -OR or -NR2, A2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, each R independently represents a methyl group or a tert-butyl group, and * represents a bonding site.

[0026]

Chemistry 10

[0027] In Formula 1, the combination of p, m, n and k can be exemplified in the following aspects. Y 1 When is a nitrogen atom, (p, m, n, k) = (0, 1, 2, 0), (1, 0, 2, 0), (0, 2, 0, 1), (0, 2, 1, 0), (1, 1, 1, 0), (0, 3, 0, 0) Y 1 When is an oxygen atom, (p, m, n, k) = (0, 1, 1, 0), (1, 0, 1, 0), (0, 2, 0, 0)

[0028] From the perspective of increasing the polymerization rate and the molecular weight, in Formula 1, Y 1 An oxygen atom is preferred. Among them, as a combination of p, m, n and k, (p, m, n, k) is preferably (0, 1, 1, 0) or (1, 0, 1, 0).

[0029] When n is 1 or more, from the viewpoint of increasing the polymerization rate, Z 1 Each independently is a group represented by any one of formulae T1 to T6, preferably a group represented by any one of formulae T1 to T3, and more preferably a group represented by formula T1.

[0030] In formulas T1 to T6, A 1 Each independently represents a hydrogen atom, a methyl group, a tert-butyl group, -OR or -NR2, A 2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, and each R independently represents a methyl group or a tert-butyl group. 1 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, A 2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, and each R independently represents a methyl group or a tert-butyl group.

[0031] In the compound represented by Formula 1, Z 1 , for example, the following compounds can be mentioned.

[0032]

Chemistry 11

[0033] Specific examples of the compound represented by Formula 1 are given below, but the compound represented by Formula 1 is not limited thereto.

[0034]

Chemistry 12

[0035]

Chemistry 13

[0036] <Compound represented by Formula 2>

Chemistry 14

[0037] In formula 2, Y 2 represents a carbon atom, a silicon atom, a phosphorus atom or a sulfur atom. Y 2 When it is a carbon atom or a silicon atom, s, t, u and v are each independently an integer satisfying s+t is greater than 1 and s+t+u+v=4. Y 2 When it is a phosphorus atom, s, t, u and v are each independently an integer satisfying s+t is greater than or equal to 1 and s+t+u+v=3. Y 2 When it is a sulfur atom, s, t, u and v are each independently an integer satisfying s+t is greater than or equal to 1 and s+t+u+v=2. When s is 1 or more, u is 1 or more. X each independently represents a chlorine atom or a bromine atom. Z 1 Each independently represents a group represented by any one of formulae T1 to T6.

[0038] In Formula 2, the combination of s, t, u and v can be exemplified in the following aspects. Y 2 When is a carbon atom or a silicon atom, (s, t, u, v) = (0, 1, 0, 3), (0, 1, 1, 2), (0, 1, 2, 1), (0, 1, 3, 0), (1, 0, 1, 2), (1, 0, 2, 1), (1, 0, 3, 0), (0, 2, 0, 2), (0, 2, 1, 1) , (0,2,2,0), (1,1,1,1), (1,1,2,0), (2,0,1,1), (2,0,2,0), (0,3,0,1), (0,3,1,0), (1,2,1,0), (2,1,1,0), (3,0,1,0) Y 2 When is a phosphorus atom, (s, t, u, v) = (0, 1, 0, 2), (0, 1, 1, 1), (0, 1, 2, 0), (1, 0, 1, 1), (1, 0, 2, 0), (0, 2, 0, 1), (0, 2, 1, 0), (1, 1, 1, 0), (2, 0, 1, 0), (0, 3, 0, 0) Y 2 When is a sulfur atom, (s, t, u, v) = (0, 1, 0, 1), (0, 1, 1, 0), (1, 0, 1, 0), (0, 2, 0, 0)

[0039] Among them, as a combination of s, t, u and v, Y 2 When it is a carbon atom, preferably (s, t, u, v) is (3, 0, 1, 0), and Y 2 In the case of a phosphorus atom, (s, t, u, v) are preferably (0, 3, 0, 0).

[0040] From the perspective of increasing the polymerization rate and the molecular weight, in Formula 2, Y 2 It is preferably a carbon atom, a silicon atom or a sulfur atom, more preferably a carbon atom or a silicon atom, and still more preferably a carbon atom.

[0041] From the viewpoint of increasing the polymerization rate, in Formula 2, X is preferably a chlorine atom.

[0042] When u is 1 or more, Z 1 Each independently is a group represented by any one of formulae T1 to T6, preferably a group represented by any one of formulae T1 to T3, and more preferably a group represented by formula T1.

[0043] In formulas T1 to T6, A 1 Each independently represents a hydrogen atom, a methyl group, a tert-butyl group, -OR or -NR2, A 2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, and each R independently represents a methyl group or a tert-butyl group. 1 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, A 2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, and each R independently represents a methyl group or a tert-butyl group.

[0044] In the compound represented by Formula 2, Z 1 , Z in the compound represented by Formula 1 can be exemplified 1 Same compound.

[0045] Specific examples of the compound represented by Formula 2 are given below, but the compound represented by Formula 2 is not limited thereto.

[0046]

Chemistry 15

[0047] <Compound represented by Formula 3>

Chemistry 16

[0048] In formula 3, Y 3 represents a carbon atom or a silicon atom. R 1 ~R 4 Each independently represents a methyl group, a tert-butyl group or a tert-butoxy group.

[0049] Specific examples of the compound represented by Formula 3 are given below, but the compound represented by Formula 3 is not limited thereto.

[0050]

Chemistry 17

[0051] From the perspective of increasing the polymerization rate and the molecular weight, in Formula 3, Y 3 Preferred is a carbon atom.

[0052] In addition, from the viewpoint of increasing the polymerization rate and the molecular weight, in Formula 3, R 1 ~R 4 Preferred is methyl.

[0053] In addition, in the polymerization solvent A, the compound corresponding to the compound represented by Formula 1 and corresponding to the compound represented by Formula 2 is the compound represented by Formula 1. That is, the compound represented by Formula 1 is not included in the compound represented by Formula 2. In addition, in the polymerization solvent A, the compound corresponding to the compound represented by Formula 1 and corresponding to the compound represented by Formula 3 is the compound represented by Formula 1. That is, the compound represented by Formula 1 is not included in the compound represented by Formula 3.

[0054] For example, methyl pivalate and tert-butyl pivalate correspond to the compound represented by Formula 1 and to the compound represented by Formula 2, and are the compounds represented by Formula 1. That is, methyl pivalate and tert-butyl pivalate are not included in the compounds represented by Formula 2. Di-tert-butyl ether corresponds to the compound represented by Formula 1 and to the compound represented by Formula 3, and is the compound represented by Formula 1. That is, di-tert-butyl ether is not included in the compounds represented by Formula 3.

[0055] From the viewpoint of suspension polymerization, the polymerization solvent A is a solvent that is immiscible with water. Whether or not the solvent is immiscible with water is determined by the following method. First, water and the solvent of the determination object are added to a closed container in a mass ratio (water: solvent of the determination object) of 10:7. After oscillation at 25°C and normal pressure for 1 minute, the mixture is allowed to stand for 10 minutes. After 10 minutes, if water and the solvent of the determination object are separated into two phases, the solvent of the determination object is determined to be a solvent that is immiscible with water. From the perspective of suspension polymerization, the polymerization medium needs to be separated into two phases.

[0056] <Water> The polymerization medium comprises water. Water is not particularly limited, but preferably contains no impurities. Examples of water include distilled water, ion-exchanged water, and pure water. The proportion of water in the polymerization solvent is 10 to 80 volume %. When the proportion of water is 80 volume % or less, it is advantageous from the viewpoint of polymerization rate.

[0057] From the viewpoints of polymerization rate, heat removal and easy stirring, the volume ratio of water to polymerization solvent A is preferably 10 volume % to 80 volume %, and more preferably 30 volume % to 60 volume %. When the above ratio is 10 volume % or more, it is advantageous from the viewpoints of heat removal and stirring. When the above ratio is 80 volume % or less, it is advantageous from the viewpoint of polymerization rate.

[0058] <Other polymerization solvents> In the method for producing a fluorinated copolymer of the present disclosure, the polymerization medium may contain polymerization solvents other than the polymerization solvent A and water. However, from the viewpoint of increasing the polymerization rate, the polymerization medium preferably contains no other polymerization solvents and preferably consists only of the polymerization solvent A and water.

[0059] As other polymerization solvents, for example, there can be mentioned: aromatic hydrocarbon solvents such as benzene, toluene, and xylene; sulfoxide solvents such as dimethyl sulfoxide (DMSO); ketone solvents such as acetone and 2-butanone (methyl ethyl ketone); ether solvents such as tetrahydrofuran (THF) and dioxane; ester solvents such as ethyl acetate; alcohol solvents such as tert-butanol; and halogen solvents such as hexafluoroisopropanol, chloroform, 1H-perfluorohexane, 1H,1H,2H,2H-perfluorooctane, 1,3-bis(trifluoromethyl)benzene, 1,4-bis(trifluoromethyl)benzene, trifluorotoluene, chlorobenzene, and 1,2-dichlorobenzene.

[0060] (Contains monomers of ethylene and tetrafluoroethylene) In the method for producing a fluorinated copolymer of the present disclosure, monomers containing ethylene and tetrafluoroethylene are polymerized. That is, the fluorinated copolymer obtained by the method for producing a fluorinated copolymer of the present disclosure contains a structural unit derived from ethylene (hereinafter also referred to as an "E unit") and a structural unit derived from tetrafluoroethylene (hereinafter also referred to as a "TFE unit").

[0061] The monomers used for polymerization may contain monomers other than ethylene and tetrafluoroethylene. That is, the fluorine-containing copolymer may contain structural units other than E units and TFE units.

[0062] Examples of other monomers other than ethylene and tetrafluoroethylene include the following monomers (1) to (7). The other monomers may be one or two or more.

[0063] Monomer (1): CH2=CX 11 (CF2) n Y 11 The compound represented. Among them, X 11 and Y 11 Each of them is independently a hydrogen atom or a fluorine atom, and n is an integer of 2-8. Monomer (2): a fluoroolefin having a hydrogen atom in the ethylenically unsaturated group such as vinylidene fluoride, vinyl fluoride, trifluoroethylene and hexafluoroisobutylene. Monomer (3): a fluoroolefin having no hydrogen atom in the ethylenically unsaturated group such as hexafluoropropylene (except TFE). Monomer (4): perfluoro(alkyl vinyl ether) such as perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether), perfluoro(propyl vinyl ether) and perfluoro(butyl vinyl ether). Monomer (5): CF2=CFOCF2CF=CF2, CF2=CFO(CF2)2CF=CF2, etc., which have two ethylenically unsaturated bonds and are cyclopolymerizable perfluoro(vinyl alkenyl ether). Monomer (6): a fluorine-containing monomer having an aliphatic ring structure such as perfluoro(2,2-dimethyl-1,3-dioxolane), 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, and perfluoro(2-methylene-4-methyl-1,3-dioxolane). Monomer (7): A monomer having a polar functional group but not having a fluorine atom (hereinafter also referred to as a polar functional group-containing monomer).

[0064] Examples of the polar functional group include a hydroxyl group, a carboxyl group, an epoxy group and an acid anhydride residue. Among them, the polar functional group is preferably an acid anhydride residue.

[0065] Examples of the polar functional group-containing monomer include vinyl ethers having a hydroxyl group and an epoxy group, unsaturated carboxylic acids such as maleic acid, itaconic acid, citraconic acid and undecylenic acid, and unsaturated polycarboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, citraconic anhydride and carbamic anhydride.

[0066] Among the above monomers (1) to (7), monomer (1) is preferred because of its good reactivity with ethylene and tetrafluoroethylene. Specific examples of the monomer (1) include CH2=CF(CF2)2F, CH2=CF(CF2)3F, CH2=CF(CF2)4F, CH2=CF(CF2)5F, CH2=CF(C F2)8F, CH2=CF(CF2)2H, CH2=CF(CF2)3H, CH2=CF(CF2)4H, CH2=CF(CF2)5H, CH2=CF(CF2)8H, C H2=CH(CF2)2F, CH2=CH(CF2)3F, CH2=CH(CF2)4F, CH2=CH(CF2)5F, CH2=CH(CF2)6F, CH2=CH(C F2)8F, CH2=CH(CF2)2H, CH2=CH(CF2)3H, CH2=CH(CF2)4H, CH2=CH(CF2)5H, and CH2=CH(CF2)8H. Among them, monomer (1) is preferably CH2=CH(CF2) n F. The integer n in the monomer (1) is 2-8, preferably 3-7, and more preferably 4-6.

[0067] The content of other monomers in the monomers used for polymerization is preferably 0.001 mol% to 20 mol%, more preferably 0.1 mol% to 15 mol%, and further preferably 0.2 mol% to 5 mol%, relative to the total amount of monomers. In addition, when the other monomer is monomer (7), it is preferably 0.01 mol% to 5 mol%, more preferably 0.05 mol% to 3 mol%, and further preferably 0.1 mol% to 1 mol%.

[0068] The molar ratio of ethylene to tetrafluoroethylene (ethylene / tetrafluoroethylene) is preferably 20 / 80 to 80 / 20, more preferably 70 / 30 to 30 / 70, and even more preferably 50 / 50 to 35 / 65.

[0069] (Polymerization initiator) In the method for producing the fluorinated copolymer of the present disclosure, it is preferred to use a polymerization initiator in order to start the polymerization reaction.

[0070] The polymerization initiator is preferably a free radical polymerization initiator. Examples of the free radical polymerization initiator include: azo compounds such as azobisisobutyronitrile and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile); peroxydicarbonates such as diisopropyl peroxydicarbonate; peroxyesters such as tert-butyl peroxypivalate, tert-butyl peroxyisobutyrate, and tert-butyl peroxyacetate; non-fluorinated diacyl peroxides such as diisobutyryl peroxide, dioctanoyl peroxide, benzoyl peroxide, and lauroyl peroxide; Z(CF2) pCOO)2 (Z is a hydrogen atom, a fluorine atom or a chlorine atom, and p is an integer from 1 to 10) and other fluorine-containing diacyl peroxides; perfluoro tert-butyl peroxide; and inorganic peroxides such as potassium persulfate, sodium persulfate, and ammonium persulfate

[0071] (Chain transfer agent) The method for producing the fluorinated copolymer disclosed herein may be carried out in the presence of a chain transfer agent to carry out the polymerization reaction. The presence of the chain transfer agent makes it easy to adjust the molecular weight of the produced fluorinated polymer.

[0072] Examples of chain transfer agents include alcohols such as methanol, ethanol, 2,2,2-trifluoroethanol, 2,2,3,3-tetrafluoropropanol, 1,1,1,3,3,3-hexafluoroisopropanol, and 2,2,3,3,3-pentafluoropropanol; hydrocarbons such as n-pentane, n-hexane, and cyclohexane; hydrofluorocarbons such as CF2H2; ketones such as acetone; thiols such as methyl mercaptan; esters such as methyl acetate and ethyl acetate; and ethers such as diethyl ether and methyl ethyl ether.

[0073] (Polymerization method) The polymerization in the method for producing the fluorinated copolymer disclosed herein is suspension polymerization. The so-called suspension polymerization method is a polymerization method in which the monomer is suspended in a polymerization medium containing water and the polymerization is carried out. Suspension polymerization is different from solution polymerization in which the monomer is dissolved in the polymerization medium and the polymerization is carried out.

[0074] In the method for producing the fluorinated copolymer disclosed herein, for example, a polymerization reaction is carried out by continuously or intermittently adding monomers containing ethylene and tetrafluoroethylene to a polymerization medium.

[0075] (Polymerization conditions) In the method for producing the fluorinated copolymer of the present invention, it is preferred that at any stage in the polymerization, the amount (mol) of the polymerization solvent A be M sol、 The total solubility (mol / mol) of ethylene and tetrafluoroethylene in the polymerization solvent A is denoted as S, and the total amount (mol) of ethylene and tetrafluoroethylene dissolved in the polymerization medium other than water is denoted as M. mon When 0.5≤M sol ×S / M mon ≤1.0.

[0076] In the present disclosure, "during polymerization" means a period during which a fluorinated copolymer containing ethylene and tetrafluoroethylene is produced.

[0077] In the case where the polymerization medium consists of only the polymerization solvent A and water and does not contain a polymerization medium other than the polymerization solvent A and water, M sol ×S / M mon When the polymerization medium contains the polymerization solvent A and a polymerization medium other than water, M sol×S / M mon Less than 1.0.

[0078] M sol ×S / M mon When M is 0.5 to 1.0, chain transfer caused by the polymerization medium is suppressed and the polymerization rate is increased. sol ×S / M mon It is more preferably 0.7 to 1.0, and even more preferably 0.85 to 1.0.

[0079] <Amount M of polymerization solvent A sol > M represents the amount of substance of the polymerization solvent A sol Calculate using the following formula. M sol (mol) = weight of polymerization solvent A (g) / molecular weight of polymerization solvent A The weight of the polymerization solvent A is a value measured under atmospheric pressure.

[0080] <Total solubility S of ethylene and tetrafluoroethylene in polymerization solvent A> The total solubility S of ethylene and tetrafluoroethylene in the polymerization solvent A is calculated by the following method. First, the vapor pressure P of the polymerization solvent A is measured. sol .P sol The pressure is shown after the polymerization medium is placed in a stainless steel autoclave equipped with a stirrer, subjected to freeze degassing twice, and the internal temperature of the reactor is maintained at a predetermined temperature T. T represents the liquid phase temperature. The temperature of the gas phase is equal to the liquid phase temperature. The weighed polymerization solvent A was added to a stainless steel autoclave equipped with a stirrer. The amount M' (mol) of the polymerization solvent A was calculated based on the weight (g) of the weighed polymerization solvent A. Next, the weighed mixed gas of ethylene and tetrafluoroethylene is added to a stainless steel autoclave equipped with a stirrer. At this time, the mixing ratio (molar ratio) of ethylene and tetrafluoroethylene is set to ethylene:tetrafluoroethylene = x:y. The feeding amount M of the mixed gas of ethylene and tetrafluoroethylene is all (mol) is calculated using the weight W (g) of the weighed mixed gas using the following formula. M a11 =W / (28x+100y) When a sufficient amount of time has passed and the pressure is constant, this pressure is referred to as the total pressure P. all . The partial pressure P of the mixed gas of ethylene and tetrafluoroethylene mon Calculated by the following formula. P mon =P all -Psol The volume V of the gas phase of the stainless steel autoclave equipped with a stirrer was calculated by the following formula. V = Volume of stainless steel autoclave with stirrer - Volume of polymerization solvent A The amount of the mixed gas of ethylene and tetrafluoroethylene present in the gas phase of the stainless steel autoclave equipped with a stirrer M g (mol) is calculated by the following formula: Wherein, R represents the gas constant. M g =P mon V / RT The amount of the mixed gas of ethylene and tetrafluoroethylene dissolved in the polymerization solvent A is M' mon (mol) is calculated by the following formula. M' mon =M all -M g The total solubility S of ethylene and tetrafluoroethylene in the polymerization solvent A is calculated by the following formula. S=M' mon / M'

[0081] <The total mass M of ethylene and tetrafluoroethylene dissolved in the polymerization medium other than water mon > The total mass M of ethylene and tetrafluoroethylene dissolved in the polymerization medium other than water mon It is calculated by the following method. First, the vapor pressure P' of the polymerization medium other than water is measured. sol . P' sol The pressure is shown after a polymerization medium other than water is placed in a stainless steel autoclave equipped with a stirrer, subjected to secondary freeze degassing, and the internal temperature of the reactor is maintained at a predetermined temperature T. T represents the liquid phase temperature. The temperature of the gas phase is equal to the liquid phase temperature. Next, the weighed mixed gas of ethylene and tetrafluoroethylene is added to a stainless steel autoclave equipped with a stirrer. At this time, the mixing ratio (molar ratio) of ethylene and tetrafluoroethylene is set to ethylene:tetrafluoroethylene = x:y. The feeding amount of the mixed gas of ethylene and tetrafluoroethylene is M' all (mol) is calculated using the weight W' (g) of the weighed mixed gas by the following formula. M' all =W' / (28x+100y) When the pressure is constant after a sufficient period of time, the pressure is set as the total pressure P' all . The partial pressure of the mixed gas of ethylene and tetrafluoroethylene is P' mon Calculated by the following formula. P'mon =P' all -P' sol The volume V' of the gas phase of the stainless steel autoclave equipped with a stirrer was calculated by the following formula. V' = volume of stainless steel autoclave with agitator - volume of polymerization medium The amount of the mixed gas of ethylene and tetrafluoroethylene present in the gas phase of the stainless steel autoclave with a stirrer M' g (mol) is calculated by the following formula: Wherein, R represents the gas constant. M' g =P' mon ×V' / RT The amount of substance M of the mixed gas of ethylene and tetrafluoroethylene dissolved in the polymerization medium other than water mon (mol) is calculated by the following formula. M mon =M' all -M' g

[0082] In the method for producing the fluorinated copolymer disclosed herein, the polymerization temperature is preferably 0 to 100° C., more preferably 20 to 90° C. The polymerization pressure is preferably 0.1 to 10 MPaG, more preferably 0.5 to 3 MPaG. The polymerization time is preferably 1 to 30 hours, more preferably 2 to 20 hours. Example

[0083] The present disclosure will be described in more detail below by way of examples, but the present disclosure is not limited to the following examples unless it exceeds the gist of the present disclosure.

[0084] [Example 1] A stainless steel autoclave with a stirrer and an internal volume of 1000 mL was placed in an ice-water bath and kept for 10 minutes, and then 300 mL (3.6 mol) of dimethyl carbonate (referred to as "DMC" in the table) and 300 mL (16.7 mol) of ion-exchanged water were added and freeze-degassed twice. While raising the internal temperature to 30°C and stirring, a mixed gas of ethylene and tetrafluoroethylene (ethylene:tetrafluoroethylene (molar ratio) = 50:50) was introduced as a monomer so that the internal pressure of the reactor was 1.5 MPaG. Furthermore, 18.3 mg (0.11 mmol) of diisobutyryl peroxide (product name "PEROYL IB", manufactured by NOF Corporation, and indicated as "IBPO" in the table) was introduced as a polymerization initiator, and stirring was performed at 500 rpm (500 revolutions per minute) for 3 hours while maintaining the internal temperature at 30°C. Thus, a polymer containing a copolymer of ethylene and tetrafluoroethylene was obtained in a slurry state. After the reactor was cooled to room temperature, unreacted ethylene and tetrafluoroethylene were discharged. The obtained slurry polymer was added to methanol, and the precipitate was separated by filtration. The precipitate was dried in a vacuum oven at 40° C. for 12 hours to obtain 8.3 g of a copolymer of ethylene and tetrafluoroethylene. Wherein, dimethyl carbonate corresponds to the compound represented by Formula 1, wherein Y 1 is an oxygen atom, p is 1, m is 0, n is 1, k is 0, Z 1 is a group represented by T1, where A 1 is -OR, and R is methyl.

[0085] [Example 2] A copolymer of ethylene, tetrafluoroethylene and perfluorobutylethylene was obtained by the same method as in Example 1, except that the feed amount of the polymerization medium was changed to 120 mL (1.4 mol) of dimethyl carbonate and 480 ml (26.7 mmol) of ion exchange water, the feed amount of the polymerization initiator was changed to 7.3 mg (0.04 mmol), and 2.2 g (8.9 mmol) of perfluorobutylethylene was added as a monomer when adding dimethyl carbonate and ion exchange water as the polymerization medium. [Example 3] A copolymer of ethylene, tetrafluoroethylene and perfluorobutylethylene was obtained by the same method as in Example 2, except that the amount of the polymerization medium was changed to 300 mL (3.6 mol) of dimethyl carbonate and 300 mL (16.7 mmol) of ion exchange water and the amount of the polymerization initiator was changed to 18.3 mg (0.11 mmol). [Example 4] A copolymer of ethylene, tetrafluoroethylene and perfluorobutylethylene was obtained by the same method as in Example 2, except that the amount of the polymerization medium was changed to 480 ml (5.7 mol) of dimethyl carbonate and 120 mL (6.7 mmol) of ion exchange water and the amount of the polymerization initiator was changed to 29.3 mg (0.17 mmol).

[0086] [Example 5] A copolymer of ethylene, tetrafluoroethylene and perfluorobutylethylene was obtained by the same method as in Example 3 except that the polymerization initiator was changed to 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (product name "V70", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., denoted as "AMVN" in the table) and the polymerization temperature was changed to 35°C.

[0087] [Example 6] A copolymer of ethylene, tetrafluoroethylene and perfluorobutylethylene was obtained by the same method as in Example 3 except that the polymerization initiator was changed to tert-butyl peroxypivalate (product name "PERBUTYL PV", manufactured by NOF Corporation, denoted as "PBPV" in the table) and the polymerization temperature was changed to 66°C.

[0088] [Example 7] A copolymer of ethylene and tetrafluoroethylene was obtained by the same method as in Example 1, except that the polymerization medium was changed to di-tert-butyl carbonate (represented as "Boc2O" in the table) and water, the polymerization initiator was changed to diisopropyl peroxydicarbonate (product name "PEROYL IPP", manufactured by NOF Corporation, represented as "IPP" in the table), and the polymerization temperature was changed to 45°C. Wherein, di-tert-butyl carbonate corresponds to the compound represented by Formula 1, wherein Y 1 is an oxygen atom, p is 0, m is 1, n is 1, k is 0, Z 1 It is a group represented by T1, T1 is -OR, and R is tert-butyl.

[0089] [Example 8] A copolymer of ethylene and tetrafluoroethylene was obtained in the same manner as in Example 1 except that the polymerization medium was changed to methyl pivalate (represented as "MePiv" in the table) and water. In addition, methyl pivalate corresponds to the compound represented by Formula 1, wherein Y 1 is an oxygen atom, p is 1, m is 0, n is 1, k is 0, Z 1 is a group represented by T1, where A 1 It is tert-butyl.

[0090] [Example 9] A copolymer of ethylene and tetrafluoroethylene was obtained in the same manner as in Example 5 except that the polymerization medium was changed to tri-tert-butylphosphine (represented as "TTBP" in the table) and water and the polymerization temperature was changed to 35°C. Wherein, tri-tert-butylphosphine corresponds to the compound represented by Formula 2, wherein Y 2 is a phosphorus atom, s is 0, t is 3, u is 0, and v is 0.

[0091] [Example 10] A copolymer of ethylene and tetrafluoroethylene was obtained in the same manner as in Example 1 except that the polymerization medium was changed to tetramethylsilane (represented as "TMS" in the table) and water and the polymerization temperature was changed to 25°C. Wherein, tetramethylsilane corresponds to the compound represented by Formula 3, wherein Y 3 is a silicon atom, R 1 ~R 4 It is methyl.

[0092] [Example 11] A copolymer of ethylene and tetrafluoroethylene was obtained by the same method as in Example 1 except that the polymerization medium was changed to a mixture of dimethyl carbonate and methyl ethyl ketone (represented as "MEK" in the table) (mass ratio 85:15) (represented as "DMC / MEK=85 / 15" in the table) and water.

[0093] [Example 12] A copolymer of ethylene and tetrafluoroethylene was obtained by the same method as in Example 1 except that the polymerization medium was changed to a mixture of dimethyl carbonate and methyl ethyl ketone (represented as "MEK" in the table) (mass ratio 70:30) (represented as "DMC / MEK=70 / 30" in the table) and water.

[0094] [Example 13] A copolymer of ethylene and tetrafluoroethylene was obtained in the same manner as in Example 1 except that the polymerization medium was changed to a mixture of methyl pivalate and dimethyl carbonate (mass ratio 50:50) (represented as "MePiv / DMC=50 / 50" in the table) and water.

[0095] [Example 14] A copolymer of ethylene and tetrafluoroethylene was obtained in the same manner as in Example 1 except that the polymerization medium was changed to neopentane and water and the polymerization temperature was changed to 20°C. Wherein, neopentane corresponds to the compound represented by Formula 3, wherein Y 3 is a carbon atom, R 1 ~R 4 It is methyl.

[0096] [Example 15] A copolymer of ethylene and tetrafluoroethylene was obtained in the same manner as in Example 1 except that the polymerization medium was changed to di-tert-butyl ketone and water purified by distillation. Wherein, di-tert-butyl ketone corresponds to the compound represented by Formula 2, wherein Y 2 is a carbon atom, s is 3, t is 0, u is 1, v is 0, Z 1 is a group represented by T1, where A 1 It is tert-butyl.

[0097] [Example 16] A copolymer of ethylene and tetrafluoroethylene was obtained by the same method as in Example 1 except that the polymerization medium was changed to 2-chloro-2,4,4-trimethyl-3-pentanone and water. Among them, 2-chloro-2,4,4-trimethyl-3-pentanone corresponds to the compound represented by Formula 2, in which Y 2 is a carbon atom, s is 2, t is 0, u is 1, v is 1, X is a chlorine atom, Z 1is a group represented by T1, where A 1 It is tert-butyl.

[0098] [Example 17] An attempt was made to obtain a copolymer of ethylene, tetrafluoroethylene and perfluorobutylethylene by the same method as in Example 2, except that the amount of the polymerization medium was changed to 60 mL (0.71 mol) of dimethyl carbonate and 540 ml (30.0 mmol) of ion exchange water, and the amount of the polymerization initiator was changed to 3.7 mg (0.02 mmol). However, no copolymer was obtained.

[0099] [Example 18] An attempt was made to obtain a copolymer of ethylene and tetrafluoroethylene by the same method as in Example 1 except that the polymerization medium was changed to diethyl ketone and water. However, no copolymer was obtained. Diethyl ketone does not belong to the polymerization solvent A.

[0100] [Example 19] An attempt was made to obtain a copolymer of ethylene and tetrafluoroethylene by the same method as in Example 1 except that the polymerization medium was changed to tert-butyl methyl ether ("TBME" in the table) and water. However, no copolymer was obtained. Tert-butyl methyl ether does not belong to the polymerization solvent A.

[0101] The polymerization rate in the production method of Examples 1 to 16 and the melt flow rate (MFR value) of the copolymers obtained in Examples 1 to 16 were measured. In addition, the amount (mol) of the polymerization solvent A during the polymerization was calculated as M sol , the total solubility (mol / mol) of ethylene and tetrafluoroethylene in the polymerization solvent A is S, and the total mass (mol) of ethylene and tetrafluoroethylene dissolved in the polymerization medium other than water is M mon M sol ×S / M mon The measurement method and calculation method are as follows. In addition, substances that cannot be measured are marked as "-" in the table.

[0102] <Polymerization speed> The polymerization rate was calculated by the following formula. Polymerization rate (g / h·L) = yield of copolymer obtained (g) / {polymerization time (h)·volume of polymerization solvent (L)} The polymerization solvent described herein does not contain a polymerization initiator.

[0103] <MFR value> The mass (g) of the copolymer flowing out from a hole with a diameter of 2.095 mm and a length of 8.000 mm for 10 minutes was measured using a thermal fluidization evaluation apparatus (product name "Flowtester CFT-100EX", manufactured by Shimadzu Corporation) under the conditions of temperature: 297°C and load: 49.0 N in accordance with ASTM D3159, and this was taken as MFR (g / 10 minutes).

[0104] <M sol ×S / M mon > First, the amount (mol) M of the polymerization solvent A is calculated as described above. sol , the total solubility of ethylene and tetrafluoroethylene in the polymerization solvent A (mol / mol) S, and the total amount of ethylene and tetrafluoroethylene dissolved in the polymerization medium other than water (mol) M mon Then, use M sol , S and M mon Calculate M sol ×S / M mon .

[0105] The types of monomers, polymerization media and polymerization initiators, polymerization rates and MFR are shown in Table 1. The case where ethylene and tetrafluoroethylene are used as monomers is described as a binary system, and the case where ethylene, tetrafluoroethylene and perfluorobutylethylene are used as a ternary system.

[0106] Table 1

[0107] As shown in Table 1, in Examples 1 to 16, suspension polymerization is carried out using monomers containing ethylene and tetrafluoroethylene in a polymerization medium containing a polymerization solvent A which is immiscible with water and at least one compound selected from Formulae 1 to 3, and water, and the proportion of water in the polymerization medium is 10 volume % to 80 volume %, so the polymerization rate is faster than before.

[0108] In addition, the disclosure of Japanese Patent Application No. 2022-061017 filed on March 31, 2022 is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical specifications described in this specification are incorporated herein by reference to the same extent as if the portions incorporated by reference in each document, patent application, and technical specification were specifically and separately described.

Claims

1. A method for producing a fluorinated copolymer, comprising carrying out suspension polymerization with monomers containing ethylene and tetrafluoroethylene in a polymerization medium containing a polymerization solvent A and water, wherein: The polymerization solvent A is at least one selected from the compounds represented by the following formulas 1 to 3 and is incompatible with water. The proportion of water in the polymerization medium is 10 volume % to 80 volume %, 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 In formula 1, Y 1 represents a nitrogen atom or an oxygen atom, Y 1 When it is a nitrogen atom, p, m, n and k are each independently an integer satisfying p+m is greater than 1 and p+m+n+k=3, Y 1 When it is an oxygen atom, k is 0, and p, m, n and k are each independently an integer satisfying p+m is greater than 1 and p+m+n=2, When p is 1 or more, n is 1 or more, In formula 2, Y 2 represents a carbon atom, a silicon atom, a phosphorus atom or a sulfur atom, Y 2 When is a carbon atom or a silicon atom, s, t, u and v are each independently an integer satisfying s+t is greater than 1 and s+t+u+v=4, Y 2 When it is a phosphorus atom, s, t, u and v are each independently an integer satisfying s+t is greater than 1 and s+t+u+v=3, Y 2 When is a sulfur atom, s, t, u and v are each independently an integer satisfying s+t is greater than 1 and s+t+u+v=2, When s is greater than 1, u is greater than 1, X each independently represents a chlorine atom or a bromine atom, In formula 1 and formula 2, Z 1 are each independently a group represented by any one of the following formulae T1 to T6, In formula 3, Y 3 represents a carbon atom or a silicon atom, R 1 ~R 4 each independently represents a methyl group, a tert-butyl group or a tert-butoxy group, 【Chemistry 4】 In formulas T1 to T6, A 1 Each independently represents a hydrogen atom, a methyl group, a tert-butyl group, -OR or -NR2, A 2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, each R independently represents a methyl group or a tert-butyl group, and * represents a bonding site.

2. The method for producing a fluorinated copolymer according to claim 1, wherein In Formula 2, Y 2 represents a carbon atom, a silicon atom or a sulfur atom.

3. The method for producing a fluorinated copolymer according to claim 1, wherein In Formula 2, Y 2 represents a carbon atom or a silicon atom.

4. The method for producing a fluorinated copolymer according to any one of claims 1 to 3, wherein In the above formula 2, X represents a chlorine atom.

5. The method for producing a fluorinated copolymer according to any one of claims 1 to 4, wherein In the formulas T1 to T6, A 1 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, A 2 Each independently represents a methyl group, a tert-butyl group, -OR or -NR2, and each R independently represents a methyl group or a tert-butyl group.

6. The method for producing a fluorinated copolymer according to any one of claims 1 to 5, wherein In Formula 1 and Formula 2, Z 1 Each independently represents a group represented by any one of the formulae T1 to T3.

7. The method for producing a fluorinated copolymer according to any one of claims 1 to 6, wherein In Formula 1 and Formula 2, Z 1 are each independently a group represented by the formula T1.

8. The method for producing a fluorinated copolymer according to any one of claims 1 to 7, wherein In Formula 3, Y 3 Represents a carbon atom.

9. The method for producing a fluorinated copolymer according to any one of claims 1 to 8, wherein At any stage of the polymerization process, the mass (mol) of the polymerization solvent A is set to M sol , the total solubility (mol / mol) of the ethylene and tetrafluoroethylene in the polymerization solvent A is S, the total mass (mol) of the ethylene and tetrafluoroethylene dissolved in the polymerization solvent other than water is M mon When 0.5≤M sol ×S / M mon ≤1.0.